460MPa-grade low-segregation easy-to-weld wind power steel plate and preparation method thereof
By rationally designing the alloy composition and process processes, the segregation problem of 460MPa-grade wind power steel plates is solved, and high-performance and low-cost low-segregation and easy-to-weld wind power steel plates are achieved, ensuring the high yield strength and low-temperature impact work of the wind power steel plates, and reducing manufacturing costs .
Patent Information
- Application Number
- CN202410915886.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
When developing 460MPa grade wind power steel plates, the research on tissue regulation and key preparation technologies is limited, especially the impact of heterogeneous structure induced by segregation of thick-specification wind power steel plates on welding fracture toughness, and the manufacturing cost is relatively high.
By reasonably designing the alloy composition of the 460MPa grade low segregation easy-to-weld wind power steel plate, using continuous casting process and thermal mechanical rolling and cold control (TMCP) process, the carbon equivalent of the steel plate and the welding crack sensitivity index are controlled, the degree of segregation is reduced, and the surface of the steel plate is ensured. The performance before and after welding of the core part is consistent, avoiding the addition of precious metal elements Mo.
The high yield strength, tensile strength and low-temperature impact work of the steel plate are achieved, the alloy cost and manufacturing cost are reduced, the production efficiency is improved, and the high performance and welding fracture toughness of the steel for wind power are ensured.
Smart Images

Figure CN118880192A_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of iron and steel metallurgy, and in particular to a 460MPa-grade low-segregation easily welded wind power steel plate and a preparation method thereof. [Background technology]
[0002] The construction of wind turbines is complex and costly. In order to ensure the safety of the entire unit within its service life, the strength and service life of each structural component must be strictly controlled. As the supporting skeleton of the entire wind turbine, the tower must meet high standards for strength and safety indicators. Therefore, by developing and using wind power steel with higher strength levels, the service life and safety indicators of the entire wind turbine can be improved, and the lightweight control goal can be achieved by reducing the thickness. At present, the steel used for onshore wind power towers has begun to increase from 355MPa to 420MPa. Europe has taken the lead in developing and applying 420MPa high-strength wind power steel, and Japan has begun to use 460MPa wind power steel plates in small batches. my country is still in the development and demonstration stage for 460-500MPa wind power steel, and its research on organizational regulation and key preparation technology is very limited. Research on key fracture toughness such as fatigue and low-temperature impact in the welding zone of new materials during service is also lacking, especially the influence of heterogeneous structure induced by segregation of thick-gauge wind power steel plates on welding fracture toughness. Therefore, based on the development of the wind power industry, reserving high-performance and high-quality preparation technology for wind power steel and key technologies for welding fracture toughness evaluation is an important strategy for the development of green energy.
[0003] At present, the research and reports on wind power steel mostly use Nb and Mo microalloying technology to control the steel plate structure and deliver it in normalized state or TMCP, with a strength level of 345-420MPa. For example, patent application CN 117344217 A discloses a 40 kg wind power steel plate and preparation method suitable for normalizing in high-cold areas, with a yield strength range of 332-455MPa; patent application CN 108265226 A discloses offshore wind power steel with a yield strength ≥ 460MPa and a manufacturing method, with a yield strength range of 460-585MPa, and the higher strength is related to its high carbon content of 0.14-0.19%; patent application CN 116536580 A discloses an easy-to-weld, high-strength and tough 500MPa-grade wind power steel plate and its preparation method, with a yield strength of ≥580MPa, an impact energy of ≥130J at -60℃, and a thermal simulation impact energy of ≥95J after welding at -60℃. It adopts needle-shaped ferrite + bainite control technology, and its excellent performance is related to the high microalloy addition, including Mo: 0.15-0.5%, Cr: 0.15-0.5%, Nb: 0.04-0.1%, Ni: 0.2-0.5%, Ti: 0.01-0.05%, which also makes the manufacturing cost of 500MPa-grade wind power steel plate higher than that of ferrite + pearlite wind power steel with lower strength and more stable performance. In addition, the patents related to wind power steel that have been disclosed so far do not involve the performance test position of steel plate samples, especially for the core of the steel plate with segregation defects, the performance before and after welding is still unclear.
[0004] Therefore, it is necessary to study a 460MPa grade low segregation easy-to-weld wind power steel plate and a preparation method to address the shortcomings of the prior art and to solve or alleviate one or more of the above problems. [Summary of the invention]
[0005] In view of this, the present invention provides a 460MPa-grade low-segregation easily welded wind power steel plate and a preparation method. Without adding the precious metal element Mo, the alloy composition of the steel plate is reasonably designed and the degree of segregation of the steel plate is reduced by controlling the key continuous casting process, so as to achieve basically consistent performance before and after welding on the surface and core of the steel plate, thereby ensuring stable performance and service safety of wind power steel.
[0006] On the one hand, the present invention provides a 460MPa-level low-segregation and easily welded wind power steel plate, which comprises the following components by weight percentage: C: 0.05-0.0.08%, Si: 0.15-0.35%, Mn: 1.15-1.55%, Ni: 0.12-0.35%, Cr: 0.15-0.45%, Nb: 0.02-0.05%, Ti: 0.01-0.03%, Alt: 0.01-0.05%, P≤0.008%, S≤0.005, N≤0.004%, and the carbon equivalent Ceq is controlled to be ≤0.45%, the welding crack sensitivity index Pcm≤0.2%, and the rest is Fe and unavoidable impurity elements.
[0007] According to the aspects and any possible implementation methods described above, an implementation method is further provided, wherein Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15, wherein: C, Mn, Cr, Mo, V, Ni, and Cu are the contents of the elements in the electrical steel plate.
[0008] According to the aspects and any possible implementation methods described above, an implementation method is further provided, wherein Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B, wherein C, Si, Mn, Cu, Ni, Cr, Mo, V, and B are the contents of the elements in the electrical steel plate.
[0009] According to the aspects and any possible implementation methods described above, an implementation method is further provided, wherein the 460MPa grade low segregation easy-to-weld wind power steel plate has a yield strength ≥460MPa, a tensile strength ≥600MPa, an elongation after fracture ≥20%, and an impact energy at -60 and -80°C ≥150J and 80J respectively, and under the condition of a welding heat input of 20kJ / cm, the impact energy of the welding heat affected zone at -60°C is ≥150J.
[0010] According to the above aspects and any possible implementation, a method for preparing a 460MPa-grade low-segregation and easily welded wind power steel plate is further provided, which is used to prepare the 460MPa-grade low-segregation and easily welded wind power steel plate, and the preparation method comprises the following steps:
[0011] S1: heating the raw steel billet to a preset temperature, and keeping the temperature until the center and edge of the steel billet have the same temperature, to obtain the first steel billet;
[0012] S2: performing rough rolling on the first steel billet to obtain a second steel billet;
[0013] S3: finishing rolling the second steel billet to obtain a finished steel plate;
[0014] S4: water-cooling the finished steel plate to obtain the 460MPa-grade low-segregation and easily weldable wind power steel plate.
[0015] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the raw material steel billet in S1 is a 260 mm thick steel billet.
[0016] According to the above aspects and any possible implementation, an implementation is further provided, wherein the preset temperature in S1 is between 1150-1220° C., and the insulation time is 120-180 min.
[0017] According to the aspects and any possible implementation methods described above, an implementation method is further provided, in which the rough rolling process in S2 is specifically as follows: the starting temperature of rough rolling is always controlled between 1150-1200°C, and the final rolling temperature is controlled between 1050-1100°C, to ensure complete recrystallization rolling, refine the austenite grain size, and the cumulative deformation reaches more than 70%, and the intermediate billet thickness is controlled to be more than 60 mm.
[0018] According to the aspects and any possible implementation methods described above, an implementation method is further provided, in which the finishing rolling process in S3 is specifically as follows: the finishing rolling start temperature is always controlled between 880-920°C, and the final rolling temperature is controlled between 840-860°C, ensuring completely non-recrystallization rolling, forming flattened austenite, increasing the nucleation points of the subsequent continuous cooling phase transformation structure, the cumulative deformation amount reaches more than 60%, and the thickness of the finished steel plate is controlled at 20-30mm.
[0019] According to the aspects and any possible implementation methods described above, an implementation method is further provided, in which the water cooling process in S4 is specifically: spraying water to cool the finished steel plate, and controlling the final cooling temperature between 600-680°C, and then air-cooling the steel plate temperature to 300-350°C for stacking, and cooling to room temperature to obtain the 460MPa grade low segregation and easy-to-weld wind power steel plate.
[0020] According to the above aspects and any possible implementation, there is further provided an implementation, in which the microstructure of the 460MPa-grade low-segregation and easily welded wind power steel plate is ferrite+pearlite microstructure.
[0021] Compared with the prior art, the present invention can achieve the following technical effects:
[0022] 1. The present invention reasonably designs the alloy composition of the steel plate, adopts a low C and low Mn design system, reasonably controls Ceq≤0.45% and Pcm≤0.2%, reduces the core segregation of the steel plate, ensures easy weldability, and the key is that the Mo addition component system is not adopted, which significantly reduces the alloy cost of the steel plate;
[0023] 2. The present invention directly adopts the TMCP rolling process without involving subsequent heat treatment steps, thereby improving production efficiency and reducing manufacturing costs;
[0024] 3. The 460MPa-grade low-segregation, easy-to-weld wind power steel plate prepared by the present invention has fine and uniform grains, and can achieve excellent performance that the impact energy of the heat-affected zone and the substrate at -60°C after welding is greater than 150J.
[0025] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time.
Brief Description of the Drawings
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is a metallographic diagram of the central segregation in the thickness direction of the wind power steel plate of Example 1 of the present invention;
[0028] Figure 2 This is a SEM image of the surface structure of the wind power steel plate in the thickness direction of Example 1 of the present invention;
[0029] Figure 3 This is a SEM image of the core structure in the thickness direction of the wind power steel plate of Example 1 of the present invention;
[0030] Figure 4 The present invention is a flow chart of a method for preparing a 460MPa-grade low-segregation easily welded wind power steel plate. [Specific implementation method]
[0031] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0032] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0034] like Figure 4As shown, the present invention provides a 460MPa-level low-segregation easily welded wind power steel plate and a preparation method thereof. The 460MPa-level low-segregation easily welded wind power steel plate comprises the following components by weight percentage: C: 0.05-0.0.08%, Si: 0.15-0.35%, Mn: 1.15-1.55%, Ni: 0.12-0.35%, Cr: 0.15-0.45%, Nb: 0.02-0.05%, Ti: 0.01-0.03%, Alt: 0.01-0.05%, P≤0.008%, S≤0.005, N≤0.004%, and the carbon equivalent Ceq is controlled to be ≤0.45%, the welding crack sensitivity index Pcm≤0.2%, and the rest is Fe and unavoidable impurity elements.
[0035] The Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15, wherein: C, Mn, Cr, Mo, V, Ni, Cu are the contents of the elements in the electrical steel plate.
[0036] The Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B, wherein C, Si, Mn, Cu, Ni, Cr, Mo, V, and B are the contents of these elements in the electrical steel plate.
[0037] The 460MPa grade low segregation easily welded wind power steel plate has a yield strength of ≥460MPa, a tensile strength of ≥600MPa, an elongation after fracture of ≥20%, an impact energy of ≥150J and 80J at -60 and -80°C respectively, and under the condition of a welding heat input of 20kJ / cm, an impact energy of the welding heat affected zone at -60°C is ≥150J.
[0038] The specific functions of each alloy element in the present invention are as follows:
[0039] C: Low carbon design is adopted to ensure the strength of the steel plate and control the carbon equivalent (Ceq) and welding crack sensitivity index (Pcm) below 0.45% and 0.2% respectively, ensuring that the steel plate is easy to weld. Therefore, C of the present invention is selected to be 0.05-0.0.08%.
[0040] Si: It can be used as a good deoxidizing element to increase the anti-oxidation property of steel. At the same time, it can improve the strength of steel in the form of solid solution strengthening. However, too high Si content will reduce the toughness of the steel plate. Therefore, the Si content of the present invention is selected to be 0.15-0.35%.
[0041] Mn: Austenitizing stabilizing element, which can significantly improve the strength of steel and can be used as a good deoxidizer and desulfurizer to reduce the content of impurity elements such as O and S in steel. However, when the Mn content exceeds 1.55%, the center segregation during the continuous casting of the steel billet is serious, which affects the low-temperature impact toughness of the center of the steel plate before and after welding. In order to reduce the center segregation of the steel plate, the Mn content of the present invention is selected to be 1.15-1.55%.
[0042] Ni: Increases the hardenability of steel, can simultaneously improve the strength and toughness of steel, strengthen and refine ferrite, but too high a Ni content will significantly increase the alloy cost and easily cause micro cracks in the welding process. Therefore, the Ni content of the present invention is selected to be 0.12-0.35%.
[0043] Cr: increases the hardenability of steel, can improve the strength and toughness of steel, and can form a passivation film on the surface of steel, improving the corrosion resistance and oxidation resistance of steel. Considering the high cost of Cr, it will be controlled when used. Therefore, the Cr content of the present invention is selected to be 0.15-0.45%.
[0044] Nb: exists in steel in the form of solid solution and precipitation, which can improve the hardenability of steel, promote grain refinement, and strengthen the matrix. At the same time, the precipitation of Nb has a positive effect on inhibiting the coarsening of austenite grains in the heat-affected zone during welding. However, considering the alloy cost, the Nb content of the present invention is selected to be 0.02-0.05%.
[0045] Ti: A good deoxidizing element, and combined with C in steel, it can form stable TiC, which has an inhibitory effect on grain coarsening. However, if the Ti content exceeds 0.03%, it is easy to induce coarse TiN and other inclusions, which have an adverse effect on the toughness of the steel. Therefore, the Ti content of the present invention is selected to be 0.01-0.03%.
[0046] Al: It is mainly used for deoxidation and nitrogenation, improving the purity of steel, and is beneficial to improving the low-temperature toughness and fatigue performance of steel. However, if the Al content exceeds 0.05%, it will significantly increase the content of inclusions such as Al2O3 in the steel, and reduce the toughness, fatigue performance and welding performance of the steel. Therefore, the Al content of the present invention is selected to be 0.01-0.05%.
[0047] P, S: harmful impurity elements in steel are inevitable. P increases the cold brittleness of steel, deteriorates welding performance, reduces plasticity, and deteriorates cold bending performance. S is also a harmful element under normal circumstances, which reduces the purity of steel, makes steel hot brittle, reduces the ductility and toughness of steel, and causes surface cracking during forging and rolling. Therefore, the P content of the present invention is controlled below 0.008%, and the S content is controlled below 0.005%.
[0048] N: It can play a role in solid solution strengthening and can combine with Al in steel to form AlN, refine grains, and improve the strength and hardness of steel. If the N content exceeds 0.005%, the increase of irregular large-sized inclusions such as TiN will reduce the toughness of the steel. Therefore, the N content of the present invention is controlled to be below 0.004%.
[0049] The present invention also provides a method for preparing a 460MPa-grade low-segregation easily welded wind power steel plate, which is used to prepare the 460MPa-grade low-segregation easily welded wind power steel plate. The production steps mainly include billet heating, controlled rolling and cooling process steps. Among them, the controlled rolling process adopts a thermomechanical controlled rolling and controlled cooling (TMCP) process, which is divided into a rough rolling process and a finishing rolling process.
[0050] In a specific embodiment, the preparation method comprises the following steps:
[0051] S1: heating the raw steel billet to a preset temperature, and keeping the temperature until the center and edge of the steel billet have the same temperature, to obtain the first steel billet;
[0052] S2: performing rough rolling on the first steel billet to obtain a second steel billet;
[0053] S3: finishing rolling the second steel billet to obtain a finished steel plate;
[0054] S4: water-cooling the finished steel plate to obtain the 460MPa-grade low-segregation and easily weldable wind power steel plate.
[0055] The raw material steel billet in S1 is a 260 mm thick steel billet.
[0056] The preset temperature in S1 is between 1150-1220° C., and the insulation time is 120-180 minutes.
[0057] The rough rolling process in S2 is specifically as follows: the rough rolling start temperature is always controlled between 1150-1200°C, and the final rolling temperature is controlled between 1050-1100°C to ensure complete recrystallization rolling, refine the austenite grain size, and the cumulative deformation reaches more than 70%, and the intermediate billet thickness is controlled to be more than 60mm.
[0058] The finishing rolling process in S3 is specifically as follows: the finishing rolling start temperature is always controlled between 880-920°C, and the final rolling temperature is controlled between 840-860°C, to ensure complete non-recrystallization rolling, to form flattened austenite, to increase the nucleation points of the subsequent continuous cooling phase transformation structure, to achieve a cumulative deformation of more than 60%, and to control the thickness of the finished steel plate to 20-30mm.
[0059] The water cooling process in S4 is specifically as follows: spraying water to cool the finished steel plate, controlling the final cooling temperature between 600-680°C, and then air-cooling the steel plate to 300-350°C for stacking, and cooling to room temperature to obtain the 460MPa grade low segregation and easy-to-weld wind power steel plate.
[0060] The microstructure of the 460MPa-grade low-segregation and easily weldable wind power steel plate is ferrite+pearlite microstructure.
[0061] Example 1
[0062] A 460MPa-grade low-segregation easily weldable wind power steel plate, whose smelting chemical composition is C: 0.06%, Si: 0.24%, Mn: 1.3%, Ni: 0.2%, Cr: 0.3%, Nb: 0.03%, Ti: 0.015%, Alt: 0.01%, P: 0.007, S: 0.004, N: 0.003, and Ceq=0.35%, Pcm=0.15%, and the rest is Fe and unavoidable impurity elements.
[0063] The 260mm continuous casting billet was heated to 1200℃ and kept warm for 150min to make the billet completely austenitized. Then the billet was rough rolled and finished rolled using the TMCP rolling process, with the rough rolling start temperature of 1182℃, the rough rolling final rolling temperature of 1060℃, the finishing rolling start temperature of 890℃, the finishing rolling final rolling temperature of 845℃, and the cumulative total reduction of 92%. Then it was sprayed with water to cool at a final cooling temperature of 620℃, and finally slowly cooled to 340℃ through the slide and stacked to room temperature.
[0064] like Figure 1 As shown in the figure, after hot acid etching, the core segregation of the 20mm thick wind power steel plate is very slight and presents a discontinuous distribution. Figure 2 and Figure 3 The results show that the microstructures near the surface and core of the steel plate are typical ferrite + pearlite microstructures with fine grain size. The average grain sizes of the surface and core are 5.8 and 7.3 μm, respectively. The yield strengths of the surface and core of the steel plate are 496 and 472 MPa, respectively. The impact energy at -60°C is 231 and 197 J, respectively. The elongations after fracture are 23.5% and 21.4%, respectively. The impact energy at -60°C of the simulated welding heat affected zone under the condition of 20 kJ / cm heat input is 205 and 178 J, respectively.
[0065] Example 2
[0066] A 460MPa-grade low-segregation easily weldable wind power steel plate, whose smelting chemical composition is C: 0.08%, Si: 0.3%, Mn: 1.5%, Ni: 0.25%, Cr: 0.35%, Nb: 0.04%, Ti: 0.015%, Alt: 0.02%, P: 0.008, S: 0.004, N: 0.003 by weight percentage, and Ceq=0.42%, Pcm=0.19%, and the rest are Fe and unavoidable impurity elements.
[0067] The 260mm continuous casting billet is heated to 1180℃ and kept warm for 150min to make the billet completely austenitized. Then the billet is rough rolled and finished rolled using the TMCP rolling process, where the rough rolling start temperature is 1170℃, the rough rolling final rolling is 1050℃, the finishing rolling start temperature is 880℃, the finishing rolling final rolling temperature is 850℃, and the cumulative total reduction is 90%. Then it is sprayed with water to cool at a final cooling temperature of 600℃, and finally slowly cooled to 350℃ through the slide and stacked to room temperature.
[0068] The near-surface and core microstructures of the 25mm thick wind power steel plate prepared by this process are typical ferrite + pearlite microstructures with fine grain size. The average grain sizes of the surface and core are 6.2 and 7.8μm respectively. The yield strength of the surface and core of the steel plate are 512 and 473MPa respectively, the impact energy at -60℃ is 201 and 177J respectively, the elongation after fracture is 21.5% and 20.4% respectively, and the impact energy at -60℃ of the simulated welding heat affected zone under the condition of 20kJ / cm heat input is 186 and 153J respectively.
[0069] Example 3
[0070] A 460MPa-grade low-segregation easily weldable wind power steel plate, whose smelting chemical composition is C: 0.08%, Si: 0.3%, Mn: 1.2%, Ni: 0.25%, Cr: 0.3%, Nb: 0.05%, Ti: 0.02%, Alt: 0.02%, P: 0.007, S: 0.005, N: 0.003 by weight percentage, and Ceq=0.36%, Pcm=0.17%, and the rest are Fe and unavoidable impurity elements.
[0071] The 260mm continuous casting billet is heated to 1190℃ and kept warm for 120min to make the billet completely austenitized. Then the billet is rough rolled and finished rolled using the TMCP rolling process, where the rough rolling start temperature is 1160℃, the rough rolling final rolling is 1060℃, the finishing rolling start temperature is 900℃, the finishing rolling final rolling temperature is 860℃, and the cumulative total reduction is 90%. Then it is sprayed with water to cool at a final cooling temperature of 600℃, and finally slowly cooled to 320℃ through the slideway and stacked to cool to room temperature.
[0072] The near-surface and core microstructures of the 25mm thick wind power steel plate prepared by this process are typical ferrite + pearlite microstructures with fine grain size. The average grain sizes of the surface and core are 6.7 and 8.5μm respectively. The yield strength of the surface and core of the steel plate are 498 and 465MPa respectively, the impact energy at -60℃ is 213 and 187J respectively, the elongation after fracture is 24.1% and 22.3% respectively, and the impact energy at -60℃ of the simulated welding heat affected zone under the condition of 20kJ / cm heat input is 218 and 193J respectively.
[0073] The above is a detailed introduction to a 460MPa grade low segregation easy-to-weld wind power steel plate and a preparation method provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of the present application; at the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
[0074] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.
[0075] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0076] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0077] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A 460MPa grade low segregation easily weldable wind power steel plate, characterized in that: The 460MPa low segregation easy-to-weld wind power steel plate comprises the following components by weight percentage: C: 0.05-0.0.08%, Si: 0.15-0.35%, Mn: 1.15-1.55%, Ni: 0.12-0.35%, Cr: 0.15-0.45%, Nb: 0.02-0.05%, Ti: 0.01-0.03%, Alt: 0.01-0.05%, P≤0.008%, S≤0.005, N≤0.004%, and control the carbon equivalent Ceq≤0.45%, welding crack sensitivity index Pcm≤0.2%, the rest are Fe and unavoidable impurity elements.
2. The 460MPa low-segregation easily weldable wind power steel plate according to claim 1, characterized in that: The Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15, wherein: C, Mn, Cr, Mo, V, Ni, Cu are the contents of the elements in the electrical steel plate.
3. The 460MPa low segregation easily weldable wind power steel plate according to claim 1, characterized in that: The Pcm=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B, wherein C, Si, Mn, Cu, Ni, Cr, Mo, V, and B are the contents of these elements in the electrical steel plate.
4. The 460MPa low-segregation easily weldable wind power steel plate according to claim 1, characterized in that: The 460MPa grade low segregation easily welded wind power steel plate has a yield strength of ≥460MPa, a tensile strength of ≥600MPa, an elongation after fracture of ≥20%, an impact energy of ≥150J and 80J at -60 and -80°C respectively, and under the condition of a welding heat input of 20kJ / cm, an impact energy of the welding heat affected zone at -60°C is ≥150J.
5. A method for preparing a 460MPa low-segregation easily welded wind power steel plate, used for preparing the 460MPa low-segregation easily welded wind power steel plate according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1: heating the raw steel billet to a preset temperature, and keeping the temperature until the center and edge of the steel billet have the same temperature, to obtain the first steel billet; S2: performing rough rolling on the first steel billet to obtain a second steel billet; S3: finishing rolling the second steel billet to obtain a finished steel plate; S4: water-cooling the finished steel plate to obtain the 460MPa-grade low-segregation and easily weldable wind power steel plate.
6. The preparation method according to claim 5, characterized in that: The preset temperature in S1 is between 1150-1220° C., the holding time is 120-180 min, and the raw material steel billet in S1 is a 260 mm thick steel billet.
7. The preparation method according to claim 5, characterized in that: The rough rolling process in S2 is specifically as follows: the rough rolling start temperature is always controlled between 1150-1200°C, and the final rolling temperature is controlled between 1050-1100°C to ensure complete recrystallization rolling, refine the austenite grain size, and the cumulative deformation reaches more than 70%, and the intermediate billet thickness is controlled to be more than 60mm.
8. The preparation method according to claim 5, characterized in that: The finishing rolling process in S3 is specifically as follows: the finishing rolling start temperature is always controlled between 880-920°C, and the final rolling temperature is controlled between 840-860°C, to ensure complete non-recrystallization rolling, to form flattened austenite, to increase the nucleation points of the subsequent continuous cooling phase transformation structure, to achieve a cumulative deformation of more than 60%, and to control the thickness of the finished steel plate to 20-30mm.
9. The preparation method according to claim 5, characterized in that: The water cooling process in S4 is specifically as follows: spraying water to cool the finished steel plate, controlling the final cooling temperature between 600-680°C, and then air-cooling the steel plate to 300-350°C for stacking, and cooling to room temperature to obtain the 460MPa grade low segregation and easy-to-weld wind power steel plate.
10. The preparation method according to claim 9, characterized in that: The microstructure of the 460MPa-grade low-segregation and easily weldable wind power steel plate is ferrite+pearlite microstructure.