Preparation method of accident fault-tolerant zirconium cladding surface Mo / FeCrAlMo composite coating
By depositing Mo/FeCrAlMo composite coating on the zirconium alloy matrix, the Fe and Cr elements are prevented from diffusion and forming a dense oxide isolation layer, the problem of Cr coating volatilization and eutectic reaction in high-temperature water vapor is solved, and high temperature is achieved Improved water vapor oxidation performance and improved coating stability.
Patent Information
- Application Number
- CN202411048739.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-01
AI Technical Summary
The existing Cr coating is prone to volatilization in high-temperature water vapor, resulting in coating defects, and reacts with zirconium alloy eutectics when the temperature exceeds 1300°C, destroying the stability of the coating and affecting its oxidation resistance.
The preparation method of Mo/FeCrAlMo composite coating is adopted, and the FeCrAlMo high-entropy alloy layer and Mo layer are deposited on the surface of the zirconium alloy matrix through zirconium alloy cleaning and magnetron sputtering technology. The Mo layer prevents the diffusion of Fe and Cr elements and enhances the stability of the coating. and oxygen solubility is reduced by FeCrAlMo high entropy alloy to form a dense oxide isolation layer.
It significantly improves the protective performance of the coating, improves the resistance to high-temperature water vapor oxidation and radiation resistance, extends the service life of the coating, and maintains good adhesion and protection effect in high-temperature environments.
Smart Images

Figure CN118880262A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal coatings, and in particular relates to a method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding. Background Art
[0002] Zirconium alloys are widely used as reactor nuclear fuel cladding materials due to their unique comprehensive properties such as small thermal neutron absorption cross-section, excellent resistance to high-temperature water corrosion, and good mechanical properties.
[0003] As the application conditions of zirconium alloys in the field of nuclear energy become more and more stringent, the use of surface engineering to deposit coatings on the surface of zirconium alloys can effectively improve the oxidation resistance of the cladding and extend the rescue time of accidents. It is an important means to improve the accident resistance of the cladding. At present, the general Cr coating has excellent corrosion resistance under the normal operating environment of the reactor (high temperature and high pressure water), and can greatly extend the service life of the cladding under non-accident conditions. Under accident conditions, although the Cr coating can significantly improve the oxidation resistance of the Zr alloy, the Cr coating generates volatile hydroxides in water vapor at temperatures exceeding 1200°C. Although the reaction rate is slow, the gaseous products will also cause defects in the coating. When the temperature exceeds 1300°C, the Cr coating will also undergo a eutectic reaction with the matrix zirconium alloy, destroying the stability of the coating bonding and affecting the performance of the coating. The upper limit of the coating's oxidation resistance is not high.
[0004] Therefore, there is an urgent need to develop a coating that is resistant to high temperature steam oxidation, water corrosion and has excellent mechanical properties to solve the problems existing in the prior art. Summary of the invention
[0005] In view of the above technical problems, the present invention aims to provide a method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding, wherein the composite coating is sputtered on the surface of a zirconium alloy substrate by sequentially cleaning the zirconium alloy and sputtering the composite coating. The coating is composed of a FeCrAlMo high-entropy alloy layer and a Mo layer from the outside to the inside. The composite coating has good mechanical properties and is firm. The Mo layer of the coating can effectively slow down or prevent the diffusion of Fe and Cr elements in the high-entropy alloy coating to the zirconium substrate at high temperatures, thereby avoiding or reducing the formation of intermetallic compounds, improving the stability of the coating bonding, and greatly improving the protective performance of the coating. In addition, the multi-component FeCrAlMo high-entropy alloy can reduce the solubility of oxygen in the alloy, which is more conducive to the formation of an oxide isolation layer. The FeCrAlMo high-entropy alloy layer and the Mo layer synergistically improve the performance of the protective layer.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding comprises the following steps:
[0008] S1. Degreasing and cleaning the zirconium alloy substrate in sequence;
[0009] S2, using FeCrAlMo high entropy alloy target and metal Mo target as sputtering sources and argon as working gas, the cleaned zirconium alloy sample is sent to the sample stage in the vacuum chamber of the magnetron sputtering equipment, a Mo layer is first sputtered on the surface of the zirconium alloy sample by using RF power supply 1 or DC power supply, and then a FeCrAlMo high entropy alloy coating is sputtered on the Mo layer by using RF power supply 2, and finally a Mo / FeCrAlMo composite coating is deposited on the zirconium alloy substrate;
[0010] During the deposition process, the temperature of the zirconium alloy substrate is room temperature, the bias voltage of the zirconium alloy substrate is 0 V, the workpiece holder rotation speed is 2 r / min, the target-substrate distance is 70 mm, the argon gas flow rate is 10 sccm, the metal Mo target is connected to the RF power supply 1 or the DC power supply, the Mo target power is 150 W, the deposition time is 60 to 120 min, the FeCrAlMo high entropy alloy target is connected to the RF power supply 2, the FeCrAlMo high entropy alloy target power is 175 W, and the deposition time is 240 min.
[0011] As a limitation of the present invention, the Mo / FeCrAlMo composite coating structure is a BCC phase.
[0012] As a second limitation of the present invention, the composition of the zirconium alloy coating is Mo / FeCrAlMo; wherein the Fe content is 24.3-27.8 at.%, the Cr content is 24.9-27.5 at.%, the Al content is 20.9-21.4 at.%, and the Mo content is 23.7-29.2 at.%.
[0013] As a third limitation of the present invention, the cleaning is carried out according to the following steps:
[0014] S11, using anhydrous ethanol to perform normal temperature ultrasonic cleaning on the deoiled zirconium alloy substrate for 3 times, each time for 10 minutes;
[0015] S12, drying the zirconium alloy substrate after washing with anhydrous ethanol;
[0016] S13, performing glow cleaning on the dried zirconium alloy substrate.
[0017] As a further limitation of the present invention, the glow cleaning condition is: the vacuum degree is less than 3.0×10 -5 Pa, the working pressure is 6.3×10 -3Pa, the argon flow rate is 20 sccm, the zirconium alloy substrate bias is -400 V, and the cleaning time is 20 min.
[0018] The present invention has another limitation that the Mo / FeCrAlMo composite coating has a thickness of 4.22 to 5.1 μm and a hardness of 6.044 to 7.138 GPa.
[0019] As is known to all, the thickness of the composite coating affects its protective performance. When the coating is thicker, although its protective performance is improved, the adhesion between the coating and the substrate is weakened, and the thermal stress and internal stress accumulation of the coating is greater; when the coating is thinner, although it is conducive to improving its adhesion, its protective effect will be worse. Therefore, the appropriate thickness of the present invention not only has good adhesion and service life, but also has good protective performance.
[0020] The present invention creatively deposits a Mo layer between the high entropy alloy layer and the zirconium substrate. At a high temperature of 1200°C, the Fe and Cr elements in the FeCrAlMo coating are prone to serious interdiffusion with the substrate zirconium alloy, generating brittle intermetallic compounds at the interface between the substrate and the coating, which deteriorates the toughness of the coating and makes it very easy to break and fall off, thus losing its protective effect. The sputtering deposition of the Mo layer can effectively slow down or prevent the Fe and Cr elements in the FeCrAlMo high entropy alloy coating from diffusing into the zirconium substrate, thereby avoiding or reducing the formation of intermetallic compounds, improving the stability of the coating bonding, and greatly improving the protective performance of the coating. In addition, since the diffusion between Zr and Mo is slow and the thermal expansion coefficients of the two are close, Mo becomes an ideal buffer layer for preventing or slowing down the interdiffusion of elements in the high entropy alloy coating and the zirconium alloy and having sufficient film-based bonding.
[0021] The selection of the coating component elements of the present invention needs to take into account the use environment requirements of the coating. In the field of nuclear energy, the requirements for the protective coating are very harsh, and the extreme environment and temperature become the primary factors that need to be considered for the protective coating. The present invention selects Fe, Cr, Al, and Mo elements to design a high entropy alloy coating as the outer layer of the composite coating. The synergistic effect between the various elements jointly improves its protective performance:
[0022] (1) From the perspective of nuclear applications, these elements are passivation elements or high melting point elements, all of which have low thermal neutron absorption cross sections;
[0023] (2) α-Al2O3 can maintain structural stability below 1500°C and has higher stability than Cr2O3 in high-temperature steam; Fe, Cr, and Mo exist in a BCC structure throughout the solid state range. Al can promote the formation of a BCC phase structure and promote the stability of this phase. Compared with multiphase alloys, single BCC structural materials have better resistance to void expansion and low radiation-induced chemical separation, and can be used as structural materials for advanced nuclear reactors;
[0024] (3) Mo is also added to the high entropy alloy coating, which can improve the adhesion between the coating and the intermediate Mo coating and enhance its firmness; in addition, due to the "third element effect", the addition of Cr and Mo elements to the high entropy alloy coating can promote the formation of dense Al2O3 oxide scale, enhance its corrosion and oxidation resistance, reduce the solubility of oxygen in the alloy, and be more conducive to the formation of an oxide isolation layer;
[0025] (4) In addition, considering that the Mo element in the coating will generate volatile oxide MoO3 at high temperature, it may have an adverse effect on the high-temperature water vapor oxidation of the coating. However, due to the selective oxidation mechanism between the elements and Al>Cr>Fe>Mo, that is, the generation of Al2O3 and Cr2O3 takes precedence over the generation of MoO3, the dense Al2O3 and Cr2O3 layer can block or reduce the adverse effect of MoO3 volatilization on the coating's resistance to high-temperature water vapor oxidation.
[0026] The above technical solution of the present invention is taken as a whole, and each step is closely related and influences each other, which jointly determine the morphological characteristics and performance of the product.
[0027] The above technical solution has the following advantages or beneficial effects:
[0028] 1. The present invention uses zirconium alloy as a substrate and sputters on the substrate in sequence to form a Mo / FeCrAlMo composite coating. On the one hand, the Mo layer, as a diffusion barrier layer, can prevent the eutectic reaction between the Fe element in the high entropy alloy coating and the Zr element in the substrate, effectively block the mutual diffusion of the Fe element and the Zr element and the invasion of the oxygen atoms into the substrate, and improve the high-temperature water vapor oxidation resistance of the zirconium alloy. On the other hand, the FeCrAlMo high entropy alloy layer has a reasonable atomic ratio composition, and the formed Al2O3 and Cr2O3 layers can block or reduce the adverse effects of MoO3 volatilization on the high-temperature water vapor oxidation resistance of the coating, and has excellent mechanical properties and good protective properties.
[0029] 2. The preparation process of the present invention is controllable, has a short cycle, and is suitable for industrial production. The prepared coating has the characteristics of good resistance to high-temperature steam oxidation, good radiation resistance, and resistance to high-temperature and high-pressure water corrosion.
[0030] The present invention is suitable for preparing a Mo / FeCrAlMo composite coating on the surface of a zirconium substrate, and is used for cladding protection in the nuclear energy field. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a surface morphology image of the coating prepared in Example 1 of the present invention;
[0032] Figure 2 This is a cross-sectional morphology diagram of the coating prepared in Example 1 of the present invention;
[0033] Figure 3 This is a cross-sectional morphology diagram of the coating prepared in Example 1 of the present invention after high-temperature steam oxidation;
[0034] Figure 4 This is a cross-sectional morphology diagram of the coating prepared in Example 2 of the present invention after high-temperature steam oxidation;
[0035] Figure 5 This is a cross-sectional morphology diagram of the substrate sample of Comparative Example 1 of the present invention after high-temperature steam oxidation;
[0036] Figure 6 This is a cross-sectional morphology diagram of the coating prepared in Comparative Example 2 of the present invention after high-temperature steam oxidation. DETAILED DESCRIPTION
[0037] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0038] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0039] Example 1
[0040] Select silicon wafer and ZIRLO alloy (zirconium alloy composition: Zr 1.1 Nb 1.1 Sn 0.11 Fe 0.13O) as a substrate, a Mo / FeCrAlMo composite coating is deposited on a silicon wafer (when a Mo / FeCrAlMo composite coating is prepared on a zirconium alloy substrate, the Mo / FeCrAlMo composite coating is simultaneously prepared on the silicon wafer, and the preparation method is the same. The Mo / FeCrAlMo composite coating on the silicon wafer is used for basic characterization of the coating) and a ZIRLO alloy substrate. The specific preparation steps of the Mo / FeCrAlMo composite coating deposited on the ZIRLO alloy substrate are as follows:
[0041] S1. Place the zirconium alloy substrate in a 5% degreasing solution and perform ultrasonic degreasing treatment at 50°C for 20 minutes; rinse the degreasing zirconium alloy substrate with running deionized water, and then place the cleaned zirconium alloy substrate in anhydrous ethanol for 3 times of ultrasonic cleaning at room temperature, each time for 15 minutes, and blow dry with an air compressor air gun after cleaning;
[0042] The cleaned zirconium alloy substrate was sent into a vacuum chamber containing a FeCrAlMo high entropy alloy target (the FeCrAlMo target was made by the existing hot pressing sintering method) and a Mo target (the Mo target was made by the existing arc melting method), and placed on a workpiece rack. The furnace door was closed and the vacuum was evacuated to less than 3×10 -5 Pa. 20 sccm of argon was introduced to maintain the working pressure at 6.3×10 - 3 Pa, substrate bias voltage -400V, the substrate was glow cleaned for 20min;
[0043] S2, using FeCrAlMo high entropy alloy target and metal Mo target as sputtering sources, connecting FeCrAlMo high entropy alloy target to RF power supply 2, connecting Mo target to RF power supply 1, using argon as working gas, argon flow rate of 10 sccm, maintaining working pressure of 8.6×10 -3 Pa, the workpiece holder speed is 2r / min, the target-substrate distance is 70mm, the FeCrAlMo high entropy alloy target power is 175W, the Mo target power is 150W, the substrate bias is 0V, the substrate temperature is room temperature, and the RF power supply 1 is used to first sputter a layer of Mo on the surface of the zirconium alloy sample, and the deposition time is 90min, and then the RF power supply 2 is used to sputter the FeCrAlMo high entropy alloy coating on the Mo layer, and the deposition time is 240min. The sputtering method is continuous sputtering, and the magnetron sputtering adopts VTC-600-2HD dual-target magnetron sputtering instrument to form a composite coating after completion.
[0044] The coating surface and cross-sectional morphology were observed using a tungsten filament scanning electron microscope, its phase composition was analyzed using an X-ray diffractometer, and its composition was characterized using an X-ray photoelectron spectroscopy. Figure 1 and Figure 2As shown, they are the surface morphology and cross-sectional morphology of the prepared coating. According to the test, the Fe content of the Mo / FeCrAlMo composite coating is 24.6at.%, the Cr content is 24.9at.%, the Al content is 21.3at.%, and the Mo content is 29.2at.%; the total coating thickness is 4.22μm, of which the Mo coating thickness is 1.08μm and the FeCrAlMo coating thickness is 3.14μm; the hardness is 6.597GPa.
[0045] In addition, the coating prepared in Example 1 was subjected to a high-temperature steam oxidation test at 1200°C for 30 min. Figure 3 As shown, it is the cross-sectional morphology of the prepared coating after oxidation, and the thickness of the oxygen diffusion layer is 57.98 μm.
[0046] Example 2
[0047] In this embodiment, a Mo / FeCrAlMo composite coating is deposited on a ZIRLO alloy substrate. The preparation process is similar to that of the composite coating in Example 1, except that the magnetron sputtering parameters are different. Specifically, the FeCrAlMo high entropy alloy target is connected to a radio frequency power supply 2, the Mo target is connected to a radio frequency power supply 1, the argon flow rate is 10 sccm, and the working pressure is maintained at 8.6×10 -3 Pa, the workpiece holder speed is 2r / min, the target substrate distance is 70mm, the Mo target power is 150W, the deposition time is 120min, the FeCrAlMo high entropy alloy target power is 175W, the deposition time is 240min, the sputtering mode is continuous sputtering, the substrate bias is 0V, the substrate temperature is room temperature, and a composite coating is obtained after sputtering is completed.
[0048] The coating prepared in this embodiment was measured using the same test method as in Example 1. After testing, the Fe content in the Mo / FeCrAlMo composite coating was 24.3 at.%, the Cr content was 25.5 at.%, the Al content was 21.4 at.%, and the Mo content was 28.8 at.%; the total coating thickness was 4.67 μm, of which the Mo coating thickness was 1.54 μm and the FeCrAlMo coating thickness was 3.13 μm; and the hardness was 7.138 GPa.
[0049] In addition, the coating prepared in Example 2 was subjected to a high-temperature steam oxidation test at 1200°C for 30 min. Figure 4 As shown, it is the cross-sectional morphology of the prepared coating after oxidation, and the thickness of the oxygen diffusion layer is 59.60 μm.
[0050] Example 3
[0051] In this embodiment, a Mo / FeCrAlMo composite coating is deposited on a ZIRLO alloy substrate. The preparation process is similar to that of Example 1, except that the magnetron sputtering parameters are different, specifically: the FeCrAlMo high entropy alloy target is connected to a radio frequency power supply 2, the Mo target is connected to a DC power supply, the argon flow rate is 10 sccm, and the working pressure is maintained at 8.6×10 -3 Pa, the workpiece holder speed is 2r / min, the target substrate distance is 70mm, the Mo target power is 150W, the deposition time is 60min, the sputtering mode is continuous sputtering, the FeCrAlMo high entropy alloy target power is 175W, the deposition time is 240min, the sputtering mode is continuous sputtering, the substrate bias is 0V, the substrate temperature is room temperature, and a composite coating is obtained after sputtering is completed.
[0052] The coating prepared in this embodiment was measured using the same test method as in Example 1. After testing, the Fe content in the Mo / FeCrAlMo composite coating was 27.8 at.%, the Cr content was 27.5 at.%, the Al content was 20.9 at.%, and the Mo content was 23.7 at.%; the total coating thickness was 5.1 μm, of which the Mo coating thickness was 1.78 μm and the FeCrAlMo coating thickness was 3.32 μm; and the hardness was 6.044 GPa.
[0053] Comparative Example 1
[0054] In this comparative example, a FeCrAlMo coating is deposited on a ZIRLO alloy substrate. The preparation process is similar to that of Example 1, except that only the FeCrAlMo coating is sputtered during the magnetron sputtering process. Specifically, the FeCrAlMo high entropy alloy target is connected to a radio frequency power supply 2, the argon flow rate is 10 sccm, and the working gas pressure is maintained at 8.6×10 -3 Pa, the workpiece holder speed is 2r / min, the target substrate distance is 70mm, the FeCrAlMo high entropy alloy target power is 175W, the deposition time is 240min, the sputtering mode is continuous sputtering, the substrate bias is 0V, and the substrate temperature is room temperature.
[0055] During the experiment, the FeCrAlMo high entropy alloy coating was severely peeled off due to the mismatch of thermal expansion coefficient and excessive internal stress, and it was difficult to prepare the FeCrAlMo high entropy alloy coating on the zirconium substrate.
[0056] Comparative Example 2
[0057] This comparative example is a Mo coating deposited on a ZIRLO alloy substrate. The difference between the preparation process and Example 1 is that only the Mo coating is sputtered during the magnetron sputtering process. Specifically, the Mo target is connected to a radio frequency power supply 1, the argon gas flow rate is 10 sccm, and the working gas pressure is maintained at 8.6×10 -3Pa, the workpiece holder rotation speed is 2r / min, the target substrate distance is 70mm, the Mo target power is 150W, the deposition time is 120min, the sputtering mode is continuous sputtering, the substrate bias is 0V, and the substrate temperature is room temperature.
[0058] Although the Mo coating can be successfully deposited on the zirconium substrate in this comparative example, since the Mo coating will generate MoO3 at 600°C and MoO3 will sublime at 795°C, it is impossible to form a protective oxide film at 1200°C and cannot be used to protect the surface of the nuclear cladding tube.
[0059] Comparative Example 3
[0060] The ZIRLO alloy (the alloy used in Example 1) was selected as a comparison, and the zirconium alloy was cleaned before testing, as follows:
[0061] The zirconium alloy substrate was placed in a 5% degreasing solution and subjected to ultrasonic degreasing treatment at 50°C for 20 minutes. The degreasing zirconium alloy substrate was rinsed with running deionized water, and then the cleaned zirconium alloy substrate was placed in anhydrous ethanol and ultrasonically cleaned at room temperature for 3 times, each time for 15 minutes. After cleaning, it was blown dry with an air gun from an air compressor.
[0062] The hardness of the zirconium alloy was tested by the same testing method as in Example 1. The hardness was found to be 3.972 GPa.
[0063] In addition, the base alloy in this comparative example was subjected to a high temperature steam oxidation test at 1200°C for 30 minutes. Figure 5 As shown in the figure, the cross-sectional morphology of the matrix alloy after oxidation can be seen, and the thickness of the oxygen diffusion layer is 114.61μm.
[0064] Comparative Example 4
[0065] A silicon wafer and a ZIRLO alloy (using the matrix composition of Example 1) were selected as the matrix, and a Cr coating was deposited on the silicon wafer (depositing the coating on the silicon wafer is used for the basic characterization of the coating) and the ZIRLO alloy matrix, respectively. The specific preparation steps are as follows:
[0066] The zirconium alloy substrate is placed in a degreasing solution with a concentration of 5%, and ultrasonically degreased at 50°C for 20 minutes; the degreasing zirconium alloy substrate is rinsed with flowing deionized water, and then the cleaned zirconium alloy substrate is placed in anhydrous ethanol and ultrasonically cleaned at room temperature for 3 times, each time for 15 minutes, and blown dry with an air gun of an air compressor after cleaning;
[0067] The cleaned zirconium alloy substrate was placed into a vacuum chamber equipped with a Cr target and placed on a workpiece rack. The furnace door was closed and the vacuum was evacuated to less than 3×10 -5Pa. 20 sccm of argon was introduced to maintain the working pressure at 6.3×10 -3 Pa, substrate bias voltage -400V, the substrate was glow cleaned for 20min;
[0068] The Cr target was used as the sputtering source. The Cr target was connected to a DC power supply. Argon was used as the working gas. The argon flow rate was 10 sccm. The working pressure was maintained at 8.6×10 -3 Pa, the workpiece holder speed is 2r / min, the target-substrate distance is 70mm, the Cr target power is 150W, the substrate bias is 0V, the substrate temperature is room temperature, and a DC power supply is used to sputter a layer of Cr on the surface of the zirconium alloy sample. The deposition time is 240min, the sputtering mode is discontinuous sputtering (i.e., stop for 10min every sputtering for 1h), and the magnetron sputtering uses a VTC-600-2HD dual-target magnetron sputtering instrument.
[0069] The coating prepared in this embodiment was tested by the same testing method as in Embodiment 1. The test showed that the Cr content in the Cr coating was 100 at. %; the coating thickness was 5.67 μm, and the hardness was 7.689 GPa.
[0070] In addition, the coating prepared in this comparative example was subjected to a high temperature steam oxidation test at 1200°C for 30 minutes. Figure 6 As shown in the figure, it is a cross-sectional morphology of the prepared coating after oxidation, and the thickness of the oxygen diffusion layer is 96.82 μm. Obviously, its water vapor oxidation resistance is far inferior to the water vapor oxidation resistance of the present invention.
[0071] In summary, by comparing the hardness and water vapor oxidation resistance of the samples in Example 1, Example 2, Comparative Example 3 and Comparative Example 4, the hardness of the composite coating of Example 1, the composite coating of Example 2, the ZIRLO substrate, and the Cr coating are 6.597 GPa, 7.138 GPa, 3.972 GPa, and 7.689 GPa, respectively, and the oxygen diffusion thickness of the coating of Example 1, the coating of Example 2, the ZIRLO substrate, and the Cr coating after water vapor oxidation are 57.98 μm, 59.60 μm, 114.61 μm, and 96.82 μm, respectively. From the hardness results, the Mo / FeCrAlMo composite coating and the Cr coating are both greater than the ZIRLO substrate, and the hardness values of the Mo / FeCrAlMo composite coating and the Cr coating are slightly different, indicating that the mechanical properties of the two coatings are equivalent. From the perspective of the thickness of the oxygen diffusion layer after steam oxidation, the oxygen diffusion layer thickness of the Mo / FeCrAlMo composite coating and the Cr coating is smaller than that of the substrate, and the oxygen diffusion layer thickness of the Mo / FeCrAlMo composite coating is smaller than that of the Cr coating, indicating that the Mo / FeCrAlMo composite coating has better resistance to steam oxidation.
[0072] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding, characterized in that: The following steps are involved: S1. Degreasing and cleaning the zirconium alloy substrate in sequence; S2, using FeCrAlMo high entropy alloy target and metal Mo target as sputtering sources and argon as working gas, the cleaned zirconium alloy sample is sent to the sample stage in the vacuum chamber of the magnetron sputtering equipment, a Mo layer is first sputtered on the surface of the zirconium alloy sample by using RF power supply 1 or DC power supply, and then a FeCrAlMo high entropy alloy coating is sputtered on the Mo layer by using RF power supply 2, and finally a Mo / FeCrAlMo composite coating is deposited on the zirconium alloy substrate; During the deposition process, the temperature of the zirconium alloy substrate is room temperature, the bias voltage of the zirconium alloy substrate is 0 V, the workpiece holder rotation speed is 2 r / min, the target-substrate distance is 70 mm, the argon gas flow rate is 10 sccm, the metal Mo target is connected to the RF power supply 1 or the DC power supply, the Mo target power is 150 W, the deposition time is 60 to 120 min, the FeCrAlMo high entropy alloy target is connected to the RF power supply 2, the FeCrAlMo high entropy alloy target power is 175 W, and the deposition time is 240 min.
2. The method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding according to claim 1, characterized in that: The Mo / FeCrAlMo composite coating has a BCC phase structure.
3. The method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding according to claim 1, characterized in that: The composition of the zirconium alloy coating is Mo / FeCrAlMo, wherein the Fe content is 24.3-27.8 at.%, the Cr content is 24.9-27.5 at.%, the Al content is 20.9-21.4 at.%, and the Mo content is 23.7-29.2 at.%.
4. The method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding according to claim 1, characterized in that: The cleaning is carried out according to the following steps: S11, using anhydrous ethanol to perform ultrasonic cleaning on the deoiled zirconium alloy substrate at room temperature for 3 times, each time for 15 minutes; S12, drying the zirconium alloy substrate after washing with anhydrous ethanol; S13, performing glow cleaning on the dried zirconium alloy substrate.
5. The method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding according to claim 4, characterized in that: The glow cleaning condition is: the vacuum degree is less than 3.0×10 -5 Pa, the working pressure is 6.3×10 -3 Pa, the argon flow rate is 20 sccm, the zirconium alloy substrate bias is -400 V, and the cleaning time is 20 min.
6. The method for preparing a Mo / FeCrAlMo composite coating on the surface of an accident-tolerant zirconium cladding according to any one of claims 1 to 5, characterized in that: The Mo / FeCrAlMo composite coating has a thickness of 4.22-5.1 μm and a hardness of 6.044-7.138 GPa.