Photovoltaic electrotinning solution

By using electroplating tin solution containing metal tin salts and other additives on photovoltaic cells, the problems of low efficiency and high cost in the existing silver-clad copper and screen printing processes are solved, and the formation of a uniform tin film is achieved and the photovoltaic is improved. The conductivity and stability of the battery.

CN118880404APending Publication Date: 2024-11-01JIANGSU AISEN SEMICON MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411317253.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing photovoltaic cell metallization process, silver-clad copper and screen printing processes have problems such as low efficiency, high cost and poor reliability, and it is difficult to achieve large-scale industrialization, especially at high temperatures, desilverization and oxidation are prone to occur. Influences resistivity and silver uniformity.

Method used

Provide a electroplating tin solution for photovoltaics, containing metal tin salt, buffering agent, complexing agent, wetting agent, antioxidant and grain refining agent, and form a uniform and good adhesion tin film on the photovoltaic cell through electroplating process. , improve conductivity and stability.

Benefits of technology

It realizes the formation of a uniform tin film on the photovoltaic cell, reduces resistance, improves power generation efficiency, enhances the stability and life of the battery module, and reduces process costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a photovoltaic electrotinning solution which comprises the following raw materials: 15-65 g / L of metal tin salt; 0.3-5 g / L of a buffering agent; 100 to 350 g / L of a complexing agent; 1-3 g / L of a wetting agent; 0.1 to 1.5 g / L of an antioxidant; and solvent water. A layer of uniform tin film with good adhesiveness can be formed on the photovoltaic battery piece, the photovoltaic battery piece can be protected against environmental erosion, the stability of the photovoltaic battery piece is improved, and the service life of the photovoltaic battery piece is prolonged. And meanwhile, the conductivity of the photovoltaic cell can be improved, the resistance is reduced, and the power generation efficiency of the photovoltaic module is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating, and in particular relates to a photovoltaic electroplating tin solution. Background Art

[0002] Metallization is one of the key processes of photovoltaic cells. It is mainly used to make photovoltaic cell electrodes, form ohmic contacts at both ends of the PN junction, and realize current output. At present, there are silver paste screen printing, silver-coated copper, tin-coated copper, copper electroplating, inkjet printing, laser transfer, etc. in the metallization process of photovoltaic cells. Among them, the screen printing process is basically adopted in the mass production line, and the processes such as silver-coated copper, tin-coated copper, copper electroplating, and laser transfer have not yet achieved large-scale industrialization. Screen printing: The slurry is permeable to the mesh of the graphic part of the screen, and the slurry is not permeable to the mesh of the non-graphic part. When printing, the slurry is poured into one end of the screen, and the pressure is applied by the scraper and moved toward the other end of the screen. During the movement, the ink is squeezed from the mesh of the graphic part to the substrate by the scraper. The viscosity of the slurry fixes the imprint within a certain range. During the printing process, the scraper contacts the screen printing plate and the substrate, and the contact line moves with the scraper. When the scraper scrapes the entire printing area and lifts up, the screen is separated from the substrate, and the workbench returns to the loading position. Screen printing also has several shortcomings: first, it is easy to cause pollution and waste of raw materials; second, it is difficult to improve the printing accuracy and the aspect ratio of the printed fine grid at present, but the metal grid with a larger aspect ratio is the key link to improve the photoelectric conversion efficiency of the battery. Silver-coated copper is a process extended to reduce the use of silver paste. It uses copper to replace part of the silver, adopts chemical plating technology, and forms silver plating layers of different thicknesses on the surface of ultrafine copper powder after specific molding and surface treatment processes, combining the advantages of silver and copper. When the particle size of the copper powder increases, the copper powder has better dispersion performance, the dispersant reduces the contact barrier between the silver ammonia complex ions and the copper powder, and the replacement reaction is more likely to occur. The silver content coated on the copper powder particles is higher, and the resistivity of the silver-coated copper will decrease. When the coating temperature of the silver-coated copper is lower than 50°C, the silver content of the silver-coated copper powder increases slowly and the resistivity is large; when it is higher than 50°C, the silver content increases sharply; when the coating temperature reaches about 70°C, the silver content reaches the maximum value. However, as the temperature increases, the surface of the copper powder will oxidize to hinder the precipitation of silver on the copper surface. Silver-clad copper technology can reduce silver consumption, but the disadvantage is that efficiency cannot be improved and new problems may arise. 1) Silver and copper have different melting points and hardness. Under high temperature conditions, desilvering and copper oxidation will increase resistance, and the uniformity of the coated silver will decrease; 2) The ball powder particles in the screen printing process need to have sufficient mesh passing ability, which requires the diameter of the copper powder to be less than 15 microns, which greatly increases the processing cost; 3) The quality reliability of the components and the performance testing of the process have yet to be verified. Tin-clad copper uses tin and copper to replace the use of silver paste, which greatly reduces the process cost, and at the same time has good performance in terms of conversion rate and reliability.

[0003] Therefore, in view of the above technical problems, it is necessary to provide a photovoltaic electroplating tin solution.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The purpose of the present invention is to provide a tin electroplating solution for photovoltaics.

[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0007] The electroplating tin solution for photovoltaics comprises raw materials of 15-65 g / L of metal tin salt, 0.3-5 g / L of buffer, 100-350 g / L of complexing agent, 1-3 g / L of wetting agent, 0.1-1.5 g / L of antioxidant and solvent water.

[0008] In one or more embodiments of the present invention, the metal tin salt is selected from stannous pyrophosphate, stannous methanesulfonate, stannous chloride, stannous sulfate, and stannous citrate.

[0009] In one or more embodiments of the present invention, the complexing agent is selected from alkali metal pyrophosphate, citric acid, ascorbic acid, glucose.

[0010] In one or more embodiments of the present invention, the buffer is selected from hydrogen phosphates such as disodium hydrogen phosphate, dipotassium hydrogen phosphate, and the like.

[0011] In one or more embodiments of the present invention, the wetting agent is selected from isooctyl phosphate, isooctyl polyoxyethylene ether phosphate, and sodium lauryl sulfate.

[0012] In one or more embodiments of the present invention, the antioxidant is selected from amine antioxidants and phenolic antioxidants such as catechol.

[0013] In one or more embodiments of the present invention, a grain refiner of 0.05-0.12 g / L is further included.

[0014] In one or more embodiments of the present invention, the grain refiner is selected from water-soluble cationic quaternary ammonium salt DDS (Hebei Jinri Chemical), and the product obtained by the reaction of glycerol diglycidyl ether and alkyl indole carboxylic acid compounds.

[0015] In one or more embodiments of the present invention, the alkyl indole carboxylic acid compound is selected from 2-methylindole-3-acetic acid, (2,5-dimethyl-1H-indol-3-yl)-acetic acid, 2-(2,4,6-trimethyl-1H-indol-3-yl)-acetic acid, (2,5,7-trimethyl-1H-indol-3-yl)-acetic acid, 5-methoxy-2-methyl-3-indoleacetic acid, (7-methoxy-2-methyl-1H-indol-3-yl)-acetic acid, (2,6,7-trimethyl-1H-indol-3-yl)-acetic acid, and (7-ethyl-2-methyl-1H-indol-3-yl)-acetic acid.

[0016] In one or more embodiments of the present invention, the reaction ratio of glycerol diglycidyl ether and alkyl indole carboxylic acid compound is: mass ratio (1.1-1.5):1.

[0017] In one or more embodiments of the present invention, the reaction process of glycerol diglycidyl ether and alkyl indole carboxylic acid compounds comprises the following steps: S1: uniformly dispersing the alkyl indole carboxylic acid compound in a mixed solution of water and dioxane (wherein the mass proportion of water is 30-80%), adjusting the pH of the solution to be alkaline, then adding di-tert-butyl dicarbonate, stirring for 2-3 hours, adding N, N-dimethylethylenediamine to the system, and adding phosphorous acid or citric acid to wash and purify the product, thereby obtaining an alkyl indole carboxylic acid compound in which the amino group is protected by a tert-butyloxycarbonyl group;

[0018] S2: The product obtained in S1 is mixed with glycerol diglycidyl ether in a mass ratio of (1.1-1.5):1, a Lewis acid catalyst is added thereto, and then the temperature is raised to 105-110°C, and the pressure is increased to 0.1-0.2MPa for reaction. After 5-7 hours, the mixture is cooled to room temperature and filtered to remove the catalyst, and then a mixture of 1-2M hydrochloric acid and dioxane is added. After stirring for 30-60 minutes, impurities are removed by distillation to obtain a grain control agent.

[0019] Compared with the prior art, the photovoltaic electroplating tin solution of the present invention forms a uniform tin film with good adhesion on the photovoltaic cell, which can protect the photovoltaic cell from environmental corrosion and improve its stability and life. At the same time, it can also improve the conductivity of the photovoltaic cell, reduce resistance, and thus improve the power generation efficiency of the photovoltaic module. DETAILED DESCRIPTION

[0020] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0021] Including but not limited to the following embodiments, the working conditions of the plating solution are as follows: temperature 20-25°C, cathode current density 1.0A / dm 2 , continuous filtration, stirring mode is that the cathode moving speed is 1-2m / min.

[0022] Example 1

[0023] The composition of the photovoltaic electroplating tin solution of this embodiment includes 15 g / L of stannous pyrophosphate; 0.3 g / L of disodium hydrogen phosphate as a buffer; 100 g / L of potassium pyrophosphate as a chelating agent; 1 g / L of isooctyl phosphate as a wetting agent; 0.1 g / L of catechol as an antioxidant; and solvent water.

[0024] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 4μm.

[0025] Example 2

[0026] The composition of the photovoltaic electroplating tin solution of this embodiment includes 40 g / L of stannous pyrophosphate; 3 g / L of disodium hydrogen phosphate as a buffer; 250 g / L of potassium pyrophosphate as a chelating agent; 2 g / L of isooctyl phosphate as a wetting agent; 1 g / L of catechol as an antioxidant; and solvent water.

[0027] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope, and the crystal phase is clear, the crystals are fine and smooth, and the grain size is 5μm.

[0028] Example 3

[0029] The composition of the photovoltaic electroplating tin solution of this embodiment includes 65 g / L of stannous pyrophosphate; 5 g / L of disodium hydrogen phosphate as a buffer; 350 g / L of potassium pyrophosphate as a chelating agent; 3 g / L of isooctyl phosphate as a wetting agent; 1.5 g / L of catechol as an antioxidant; and solvent water.

[0030] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 4μm.

[0031] Example 4

[0032] The composition of the photovoltaic electroplating tin solution of this embodiment includes 35 g / L of stannous methanesulfonate; 1 g / L of dipotassium hydrogen phosphate as a buffer; 150 g / L of citric acid as a complexing agent; 1.5 g / L of sodium dodecyl sulfate as a wetting agent; 0.8 g / L of catechol as an antioxidant; and solvent water.

[0033] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope, and the crystal phase is clear, the crystals are fine and smooth, and the grain size is 5μm.

[0034] Example 5

[0035] The composition of the photovoltaic electroplating tin solution of this embodiment includes 35 g / L stannous citrate; 1 g / L dipotassium hydrogen phosphate as a buffer; 150 g / L glucose as a chelating agent; 1.5 g / L sodium dodecyl sulfate as a wetting agent; 0.8 g / L catechol as an antioxidant; and water as a solvent.

[0036] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 4μm.

[0037] Example 6

[0038] The only difference between this embodiment and embodiment 1 is that it further includes a grain refiner DDS 0.12 g / L.

[0039] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope, and the crystal phase is clear, the crystals are fine and smooth, and the grain size is 3μm.

[0040] Example 7

[0041] The only difference between this embodiment and embodiment 1 is that it further includes a grain refiner DDS 0.05 g / L.

[0042] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope, and the crystal phase is clear, the crystals are fine and smooth, and the grain size is 3μm.

[0043] Example 8

[0044] The only difference between this embodiment and embodiment 1 is that it further includes a grain refiner DDS 0.09 g / L.

[0045] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope, and the crystal phase is clear, the crystals are fine and smooth, and the grain size is 3μm.

[0046] Example 9

[0047] The only difference between this embodiment and embodiment 1 is that it further comprises 0.07 g / L of a product obtained by the reaction of glycerol diglycidyl ether and an alkyl indole carboxylic acid compound as a grain refiner.

[0048] The reaction process of glycerol diglycidyl ether and alkyl indole carboxylic acid compound 2-methyl indole-3-acetic acid comprises the following steps: S1: uniformly dispersing the alkyl indole carboxylic acid compound in a mixed solution of water and dioxane (wherein the mass proportion of water is 30%), adjusting the pH of the solution to be alkaline, then adding di-tert-butyl dicarbonate, stirring for 2-3 hours, adding N, N-dimethylethylenediamine to the system, and adding phosphorous acid or citric acid to wash and purify the product, so as to obtain an alkyl indole carboxylic acid compound whose amino group is protected by a tert-butyloxycarbonyl group;

[0049] S2: The product obtained in S1 was mixed with glycerol diglycidyl ether in a mass ratio of 1.1:1, a Lewis acid catalyst was added thereto, and then the temperature was raised to 105°C and the pressure was increased to 0.1 MPa for reaction. After 5 hours, the mixture was cooled to room temperature and filtered to remove the catalyst. Then, a mixture of 1M hydrochloric acid and dioxane was added, and the mixture was stirred for 30 minutes, and then impurities were removed by distillation to obtain a grain control agent.

[0050] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 2μm.

[0051] Example 10

[0052] The only difference between this embodiment and embodiment 1 is that it further comprises 0.07 g / L of a product obtained by the reaction of glycerol diglycidyl ether and an alkyl indole carboxylic acid compound as a grain refiner.

[0053] The reaction process of glycerol diglycidyl ether and alkyl indole carboxylic acid compound (2,6,7-trimethyl-1H-indol-3-yl)-acetic acid comprises the following steps: S1: uniformly dispersing the alkyl indole carboxylic acid compound in a mixed solution of water and dioxane (wherein the mass proportion of water is 80%), adjusting the pH of the solution to be alkaline, then adding di-tert-butyl dicarbonate, stirring for 2-3 hours, adding N,N-dimethylethylenediamine to the system, and adding phosphorous acid or citric acid to wash and purify the product, so as to obtain an alkyl indole carboxylic acid compound whose amino group is protected by tert-butyloxycarbonyl;

[0054] S2: The product obtained in S1 is mixed with glycerol diglycidyl ether in a mass ratio of 1.5:1, a Lewis acid catalyst is added thereto, and then the temperature is raised to 110°C and the pressure is increased to 0.2MPa for reaction. After 7 hours, the mixture is cooled to room temperature and filtered to remove the catalyst. A mixture of 2M hydrochloric acid and dioxane is added, and the mixture is stirred for 60 minutes, and then impurities are removed by distillation to obtain a grain control agent.

[0055] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 2μm.

[0056] Embodiment 11

[0057] The only difference between this embodiment and embodiment 1 is that it further comprises 0.07 g / L of a product obtained by the reaction of glycerol diglycidyl ether and an alkyl indole carboxylic acid compound as a grain refiner.

[0058] The reaction process of glycerol diglycidyl ether and alkyl indole carboxylic acid compound 5-methoxy-2-methyl-3-indoleacetic acid comprises the following steps: S1: uniformly dispersing the alkyl indole carboxylic acid compound in a mixed solution of water and dioxane (wherein the mass proportion of water is 60%), adjusting the pH of the solution to be alkaline, then adding di-tert-butyl dicarbonate, stirring for 2.3 hours, adding N,N-dimethylethylenediamine to the system, and adding phosphorous acid or citric acid to wash and purify the product, so as to obtain an alkyl indole carboxylic acid compound whose amino group is protected by tert-butyloxycarbonyl;

[0059] S2: The product obtained in S1 was mixed with glycerol diglycidyl ether in a mass ratio of 1.3:1, a Lewis acid catalyst was added thereto, and then the temperature was raised to 107°C and the pressure was increased to 0.15 MPa for reaction. After 6 hours, the mixture was cooled to room temperature and filtered to remove the catalyst. Then, a mixture of 1.5 M hydrochloric acid and dioxane was added, and the mixture was stirred for 50 minutes, and then impurities were removed by distillation to obtain a grain control agent.

[0060] The surface of the sample obtained by electroplating the copper sheet is smooth. The grain size is measured using a scanning electron microscope. The crystal phase is clear, the crystals are fine and smooth, and the grain size is 2μm.

[0061] Test items:

[0062] 1. Uniformity

[0063] Use electroplating solution to electroplate a copper sheet with a thickness of about 10 microns. Measure the thickness at 10 points from left to right. Calculate its uniformity according to the formula: Uniformity = (maximum value - minimum value) / 10.

[0064] 2. Salt spray resistance

[0065] A 10-micron tin layer was electroplated on a copper sheet and placed in a neutral (5% sodium chloride salt water) salt spray test chamber.

[0066] Observe the changes in the coating.

[0067] 3. Antioxidant properties

[0068] Heat the plating solution to 40°C, use an air pump to pump air into the plating solution (10L / Min, 40°C hot air), and record the time when the plating solution becomes turbid.

[0069] Plating solution Uniformity / μm Salt spray resistance Antioxidant performance / h Example 1 0.1 72h no corrosion 90 Example 2 0.1 72h no corrosion 90 Example 3 0.1 72h no corrosion 90 Example 4 0.1 72h no corrosion 90 Example 5 0.1 72h no corrosion 90 Example 6 0.05 148h no corrosion 105 Example 7 0.05 148h no corrosion 105 Example 8 0.05 148h no corrosion 105 Example 9 0.05 160h no corrosion 120 Example 10 0.05 160h no corrosion 120 Embodiment 11 0.05 160h no corrosion 120

[0070] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that fall within the meaning and scope of the equivalent elements of the claims be included in the invention. No statement in the claims should be considered as limiting the claims involved.

[0071] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A photovoltaic electroplating tin solution, the raw materials of which include: 15-65 g / L of metal tin salt; 0.3-5 g / L of buffer; 100-350 g / L of complexing agent; 1-3 g / L of wetting agent; 0.1-1.5 g / L of antioxidant; and solvent water.

2. The photovoltaic electroplating tin solution according to claim 1, characterized in that: The metal tin salt is selected from stannous pyrophosphate, stannous methanesulfonate, stannous chloride, stannous sulfate, and stannous citrate.

3. The photovoltaic electroplating tin solution according to claim 1, characterized in that: The complexing agent is selected from alkali metal pyrophosphate, citric acid, ascorbic acid, and glucose.

4. The photovoltaic electroplating tin solution according to claim 1, characterized in that: The buffer is selected from hydrogen phosphate.

5. The photovoltaic electroplating tin solution according to claim 1, characterized in that: The wetting agent is selected from isooctyl phosphate, isooctyl polyoxyethylene ether phosphate, and sodium lauryl sulfate.

6. The photovoltaic electroplating tin solution according to claim 1, characterized in that: The antioxidant is selected from amine antioxidants and phenolic antioxidants.

7. The photovoltaic electroplating tin solution according to any one of claims 1 to 6, characterized in that: It also includes grain refiner 0.05-0.12 g / L.

8. The photovoltaic electroplating tin solution according to claim 7, characterized in that: The grain refiner is selected from the product obtained by the reaction of water-soluble cationic quaternary ammonium salt DDS, glycerol diglycidyl ether and alkyl indole carboxylic acid compounds.

9. The photovoltaic electroplating tin solution according to claim 8, characterized in that: The alkyl indole carboxylic acid compound is selected from 2-methylindole-3-acetic acid, (2,5-dimethyl-1H-indol-3-yl)-acetic acid, 2-(2,4,6-trimethyl-1H-indol-3-yl)-acetic acid, (2,5,7-trimethyl-1H-indol-3-yl)-acetic acid, 5-methoxy-2-methyl-3-indoleacetic acid, (7-methoxy-2-methyl-1H-indol-3-yl)-acetic acid, (2,6,7-trimethyl-1H-indol-3-yl)-acetic acid, and (7-ethyl-2-methyl-1H-indol-3-yl)-acetic acid.

10. The photovoltaic electroplating tin solution according to claim 8, characterized in that: The reaction ratio of the glycerol diglycidyl ether and the alkyl indole carboxylic acid compound is: mass ratio (1.1-1.5):1.

Citation Information

Cited By

  • Electroplating solution containing matte tin plating additive and preparation method thereof

    CN122215003A