Super-hydrophobic composite material and preparation method thereof

Through the composite of hydrophobic modified resin and fiber fabric and the hot pressing forming of superhydrophobic coating and hard template, the problems of unsolid bonding and low mechanical strength of superhydrophobic composite materials are solved, the structural function integration is achieved, and the material is improved. Hydrophobicity and mechanical properties.

CN118880628APending Publication Date: 2024-11-01CHENGDU AERONAUTIC POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192133.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The coating of the existing superhydrophobic composite materials has poor bonding to the substrate interface, low mechanical strength, and cumbersome surface modification process, limited application fields, lack strong structural support, and insufficient life cycle.

Method used

The hydrophobic epoxy composite material substrate is prepared by composited with hydrophobic modified resin and fiber fabric, and the superhydrophobic epoxy coating is heat-pressed with hard templates, combined with hydrophobic particles to form a superhydrophobic composite material with integrated structural functions.

Benefits of technology

The combination of high mechanical strength and superhydrophobic properties is achieved, with the surface contact angle reaching 151.1°, the rolling angle is as low as 1°, and the bond strength between the coating and the substrate is improved through co-curing molding, extending the life cycle of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a super-hydrophobic composite material and a preparation method thereof, and relates to the technical field of composite materials. The super-hydrophobic epoxy composite material comprises a hydrophobic epoxy composite material substrate and a super-hydrophobic epoxy coating, the hydrophobic epoxy composite material substrate is formed by compounding hydrophobic modified resin and a fiber fabric; the super-hydrophobic epoxy coating is formed by mixing hydrophobic modified resin and hydrophobic particles; a modifying agent of the hydrophobic modified resin is amino functional polysiloxane; the hydrophobic epoxy composite material substrate and the super-hydrophobic epoxy coating are co-cured and molded at one time; the problems that an existing common super-hydrophobic coating and the surface of a composite material component are not firmly bonded, and the mechanical strength is low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a super-hydrophobic composite material and a preparation method thereof. Background Art

[0002] In recent years, inspired by the "lotus effect" in nature, people have discovered that super-hydrophobic surfaces have excellent self-cleaning, anti-icing, anti-corrosion, underwater drag reduction and other properties. Studies have found that this is mainly achieved through the special low-surface energy materials on the functional surface and the coordinated micro / nano hierarchical structure. At present, super-hydrophobic surfaces are mostly achieved through functional coatings and surface modification, but the coating and substrate interface adhesion is insufficient, there is a debonding problem, the surface modification process is cumbersome, the application field is limited, and the super-hydrophobic surface microstructure prepared by coating and modification lacks strong structural support, the theoretical mechanical strength is insufficient, and the life cycle is limited.

[0003] Fiber-reinforced resin-based composites have high specific strength and strong designability. In recent years, with the continuous expansion of application fields, the requirements for them have become diversified. Structural and functional integration is gradually becoming a research hotspot for resin-based composites. The development of highly hydrophobic resin-based composites has considerable application prospects in surface engineering fields such as self-cleaning and anti-icing.

[0004] At present, most of the reports on hydrophobic composite materials at home and abroad have been conducted on the preparation of hydrophobic functional surfaces on composite substrates through coating and surface modification. Although these surface hydrophobicization studies based on composite materials have shown excellent hydrophobicity, corrosion resistance, and even anti-icing properties, their functional surface layers still lack structural support and have problems such as insufficient life under harsh application conditions. Summary of the invention

[0005] The object of the present invention is to provide a super-hydrophobic composite material and a preparation method thereof, so as to solve the problems of weak adhesion and low mechanical strength commonly existing between the existing common super-hydrophobic coating and the surface of the composite material component.

[0006] In order to solve the above problems, the present invention adopts the following technical means: A super hydrophobic composite material, comprising a hydrophobic epoxy composite material substrate and a super hydrophobic epoxy coating; The hydrophobic epoxy composite material substrate is composited by hydrophobic modified resin and fiber fabric; The super hydrophobic epoxy coating is formed by mixing a hydrophobic modified resin and hydrophobic particles; The modifier of the hydrophobically modified resin is amino-functional polysiloxane.

[0007] Preferably, the resin matrix of the hydrophobically modified resin is a double-part A-type epoxy resin, and the curing agent is an amine curing agent.

[0008] Furthermore, the hydrophobic particles are one of polytetrafluoroethylene and silicon dioxide, and the particle size of the hydrophobic particles does not exceed 10 microns.

[0009] At the same time, a method for preparing a super-hydrophobic composite material comprises the following steps: S1. Modifying the resin matrix using amino-functional polysiloxane to obtain a hydrophobically modified resin; S2. The hydrophobic modified resin and the fiber fabric are wet-laid to obtain a hydrophobic epoxy composite substrate preform; S3. The hydrophobic modified resin is mixed with the hydrophobic particles to prepare a super hydrophobic epoxy coating; S4. Spraying the super hydrophobic epoxy coating on the surface of the hydrophobic epoxy composite substrate preform; S5. Compression-molding and curing the coated hydrophobic epoxy composite substrate preform using a hard template having a surface microstructure.

[0010] Furthermore, the step S1 includes: The amino functional polysiloxane is dissolved in 3-glycidyloxypropyltrimethoxysilane solvent, and after being stirred evenly, a curing agent is added, and after mixing, epoxy resin is added, and after mixing evenly, bubbles are discharged to obtain a hydrophobic modified resin.

[0011] Furthermore, the amino-functional polysiloxane is added in an amount of 1 to 15 wt % of the resin matrix / curing agent system, and the 3-glycidyloxypropyltrimethoxysilane solvent is added in an amount of 5 to 15 wt % of the resin matrix / curing agent system.

[0012] Furthermore, in the step S2, the fiber fabric and the hydrophobically modified resin are compounded in a mass ratio of 1:1.

[0013] Furthermore, the step S3 includes: The hydrophobic modified resin is dissolved in ethyl acetate, the hydrophobic powder is dispersed in anhydrous ethanol, and then the hydrophobic modified resin solution and the hydrophobic powder suspension are mixed.

[0014] Furthermore, the hydrophobic powder is mixed with anhydrous ethanol at a ratio of 1:2-3.5, the hydrophobic modified resin is mixed with ethyl acetate at a ratio of 1:0.75, and the mass ratio of the hydrophobic modified resin to the hydrophobic powder is 1:1-3.5.

[0015] Furthermore, in step S4, multiple thin sprays are used for spraying, the spraying speed is 0.6~1.8m / s, the spraying distance is 10~25cm, the air pressure is 0.1~0.5MPa, each sample is sprayed 2~6 times, and the interval time between each spraying is greater than 1min.

[0016] During use, the present invention has the following beneficial effects: Structural and functional integration: The hydrophobic properties of the super-hydrophobic epoxy coating are organically combined with the structural advantages of the fiber composite material, so that the surface fiber can form a structural reinforcement for the functional material, and the design and preparation of a super-hydrophobic composite material with structural and functional integration is realized, with a contact angle (CA) of 151.1° and a rolling angle (SA) as low as 1°; Epoxy resin hydrophobic modification: By hydrophobic modification of epoxy resin, the surface energy of the composite material matrix is ​​reduced, thereby reducing the dependence of the realization of superhydrophobic performance on the content of modifier, achieving the ideal superhydrophobic state while maintaining its original mechanical strength; Hard template hot pressing: The micro / nanostructured super-hydrophobic composite material imitating the surface of lotus leaves is prepared by hard template hot pressing. The rough structure is formed during the hot pressing curing process, which makes the surface mechanical strength high and realizes the precise control of the surface morphology structure. Through one-time co-curing, the surface functional layer and the reinforcing material are integrated to obtain a structural and functional integrated hydrophobic composite product with both load-bearing and hydrophobic properties, and the surface hydrophobicity can reach the super-hydrophobic level. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0018] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0020] Example 1 (1) Hydrophobic modification of resin matrix The epoxy resin (E51) was hydrophobically modified using amino-functional polysiloxane. First, the amino-functional polysiloxane modifier was dissolved in 3-glycidyloxypropyltrimethoxysilane solvent (the solvent was 5-15wt% of the resin matrix / curing agent system) at 1-15wt% of the mass of the epoxy system (including the curing agent), and magnetically stirred for 2 minutes (the magnetic stirring speed was constant at 600rpm); the curing agent was added, and after mixing, magnetic stirring was performed for 15 minutes; the epoxy resin was added, and after mixing, magnetic stirring was performed for 5 minutes; vacuum was drawn at 50°C for 0.5h to remove bubbles, and a hydrophobically modified resin was obtained. Among them, in this step, the curing agent selected was an amine curing agent, specifically D230.

[0021] (2) Preparation of hydrophobic composite material preform Cut a number of fiber fabrics (with a mass ratio of 1:1 to the hydrophobic modified resin), wherein the fiber fabric here can be carbon fiber. Prepare a hydrophobic epoxy composite material substrate preform on a steel plate mold by a wet laying process; (3) Preparation and spraying of hydrophobic coating Take polytetrafluoroethylene (PTFE) powder with a particle size of about 500nm, mix it with anhydrous ethanol solvent in a ratio of 1:2~3.5, and stir it magnetically at 600rpm for 10 minutes; take a hydrophobic modified resin (containing 1 / 4 curing agent) and dissolve it in an ethyl acetate solvent in a ratio of 1:0.75, and stir it manually for 2 minutes; mix the PTFE suspension obtained above and the hydrophobic modified resin solution in a ratio of 1:1, and stir it magnetically at 600rpm for 10 minutes to obtain a super hydrophobic epoxy coating; spray the hydrophobic epoxy coating on the hydrophobic epoxy composite material substrate preform after paving, and use a "multiple thin spray" method for spraying, the spraying speed is 0.6~1.8m / s, the spraying distance is 10~25cm, the air pressure is 0.1~0.5MPa, each sample is sprayed 2~6 times, each interval is greater than 1min, and the coating thickness is about 30μm; (4) Hard template molding and curing The preform after spraying is placed in a steel plate with a rough surface (the steel plate is sandblasted with 120-mesh corundum in advance), and put into a molding machine for curing at 80°C / 2h+120°C / 1h and a pressure of 0.2MPa to obtain a hydrophobic composite material (SH-CM) with a micro / nano structure.

[0022] Example 2 (1) Hydrophobic modification of resin matrix The epoxy resin (E51) was hydrophobically modified using amino-functional polysiloxane. First, the amino-functional polysiloxane modifier was dissolved in 3-glycidyloxypropyltrimethoxysilane solvent (the solvent was 5-15wt% of the resin matrix / curing agent system) at 1-15wt% of the mass of the epoxy system (including the curing agent), and magnetically stirred for 2 minutes (the magnetic stirring speed was constant at 600rpm); the curing agent was added, and after mixing, magnetic stirring was performed for 15 minutes; the epoxy resin was added, and after mixing, magnetic stirring was performed for 5 minutes; vacuum was drawn at 50°C for 0.5h to remove bubbles, and a hydrophobically modified resin was obtained. Among them, in this step, the curing agent selected was an amine curing agent, specifically D230.

[0023] (2) Preparation of hydrophobic composite material preform Cut a number of fiber fabrics (with a mass ratio of 1:1 to the hydrophobic modified resin), wherein the fiber fabric here can be carbon fiber. Prepare a hydrophobic epoxy composite material substrate preform on a steel plate mold by a wet laying process; (3) Preparation and spraying of hydrophobic coating Take polytetrafluoroethylene (PTFE) powder with a particle size of about 500nm, mix it with anhydrous ethanol solvent in a ratio of 1:2~3.5, and stir it magnetically at 600rpm for 10 minutes; take a hydrophobic modified resin (containing 1 / 4 curing agent) and dissolve it in an ethyl acetate solvent in a ratio of 1:0.75, and stir it manually for 2 minutes; mix the PTFE suspension obtained above and the hydrophobic modified resin solution in a ratio of 1:2.5, and stir it magnetically at 600rpm for 10 minutes to obtain a super hydrophobic epoxy coating; spray the hydrophobic epoxy coating on the hydrophobic epoxy composite material substrate preform after paving, and use a "multiple thin spray" method for spraying, the spraying speed is 0.6~1.8m / s, the spraying distance is 10~25cm, the air pressure is 0.1~0.5MPa, each sample is sprayed 2~6 times, each interval is greater than 1min, and the coating thickness is about 30μm; (4) Hard template molding and curing The preform after spraying is placed in a steel plate with a rough surface (the steel plate is sandblasted with 120-mesh corundum in advance), and put into a molding machine for curing at 80°C / 2h+120°C / 1h and a pressure of 0.2MPa to obtain a hydrophobic composite material (SH-CM) with a micro / nano structure.

[0024] Example 3 (1) Hydrophobic modification of resin matrix The epoxy resin (E51) was hydrophobically modified using amino-functional polysiloxane. First, the amino-functional polysiloxane modifier was dissolved in 3-glycidyloxypropyltrimethoxysilane solvent (the solvent was 5-15wt% of the resin matrix / curing agent system) at 1-15wt% of the mass of the epoxy system (including the curing agent), and magnetically stirred for 2 minutes (the magnetic stirring speed was constant at 600rpm); the curing agent was added, and after mixing, magnetic stirring was performed for 15 minutes; the epoxy resin was added, and after mixing, magnetic stirring was performed for 5 minutes; vacuum was drawn at 50°C for 0.5h to remove bubbles, and a hydrophobically modified resin was obtained. Among them, in this step, the curing agent selected was an amine curing agent, specifically D230.

[0025] (2) Preparation of hydrophobic composite material preform Cut a number of fiber fabrics (with a mass ratio of 1:1 to the hydrophobic modified resin), wherein the fiber fabric here can be carbon fiber. Prepare a hydrophobic epoxy composite material substrate preform on a steel plate mold by a wet laying process; (3) Preparation and spraying of hydrophobic coating Take polytetrafluoroethylene (PTFE) powder with a particle size of about 500nm, mix it with anhydrous ethanol solvent in a ratio of 1:2~3.5, and stir it magnetically at 600rpm for 10 minutes; take a hydrophobic modified resin (containing 1 / 4 curing agent) and dissolve it in an ethyl acetate solvent in a ratio of 1:0.75, and stir it manually for 2 minutes; mix the PTFE suspension obtained above and the hydrophobic modified resin solution in a ratio of 1:3.5, and stir it magnetically at 600rpm for 10 minutes to obtain a super hydrophobic epoxy coating; spray the hydrophobic epoxy coating on the hydrophobic epoxy composite material substrate preform after paving, and use a "multiple thin spray" method for spraying, the spraying speed is 0.6~1.8m / s, the spraying distance is 10~25cm, the air pressure is 0.1~0.5MPa, each sample is sprayed 2~6 times, each interval is greater than 1min, and the coating thickness is about 30μm; (4) Hard template molding and curing The preform after spraying is placed in a steel plate with a rough surface (the steel plate is sandblasted with 120-mesh corundum in advance), and put into a molding machine for curing at 80°C / 2h+120°C / 1h and a pressure of 0.2MPa to obtain a hydrophobic composite material (SH-CM) with a micro / nano structure.

[0026] In the aforementioned embodiments, embodiment 2 is used as the optimal embodiment.Wherein, by allowing super-hydrophobic epoxy coating and hydrophobic epoxy composite substrate to be co-cured and formed, it is not only possible to improve the bonding strength between super-hydrophobic epoxy coating and hydrophobic epoxy composite substrate, the reinforcing fiber of substrate can also protect and reinforce coating, and meanwhile, it is also possible to effectively avoid adding hydrophobic particles, causing hydrophobic epoxy composite substrate to affect the problem of its interlayer bonding because of adding low surface energy particles.Moreover, the application is by adding a certain amount of hydrophobic particles, while hydrophobic particles themselves have the ability to improve hydrophobicity, combined with the agglomeration occurring in its preparation process, it is possible to increase the roughness of coating surface to a certain extent, while forming a multi-level scale structure, to further improve the super-hydrophobic performance of coating.

[0027] In general, the hydrophobic particles used as fillers will cause the performance of the coating to decline after agglomeration. Since the hydrophobic particles are low surface energy particles, their large-scale agglomeration will greatly reduce the adhesion performance of the coating. If the filler agglomerates, the peel strength of the coating will generally be reduced. However, the present application utilizes the agglomeration of the hydrophobic particles through a specific molding method. Even if the hydrophobic particles agglomerate to a certain extent, it can effectively prevent the coating from falling off from the substrate under harsh environments.

[0028] However, for this application, the hydrophobic particles cannot be added too much. If they are added excessively, the agglomeration of the hydrophobic particles will be too serious, and after the coating and the substrate are integrally formed, their bonding strength will be greatly reduced in harsh environments.

[0029] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A super hydrophobic composite material, It is characterized in that including a hydrophobic epoxy composite substrate and a super hydrophobic epoxy coating; The hydrophobic epoxy composite material substrate is composited by hydrophobic modified resin and fiber fabric; The super hydrophobic epoxy coating is formed by mixing a hydrophobic modified resin and hydrophobic particles; The modifier of the hydrophobically modified resin is amino-functional polysiloxane.

2. A super-hydrophobic composite material according to claim 1, It is characterized in that The resin matrix of the hydrophobic epoxy composite material substrate is double-part A-type epoxy resin, and the curing agent is an amine curing agent.

3. A super hydrophobic composite material according to claim 1 or 2, It is characterized in that The hydrophobic particles are one of polytetrafluoroethylene and silicon dioxide, and the particle size of the hydrophobic particles can be one or both of micron particles and nanoparticles, and is not more than 10 microns.

4. A method for preparing a super-hydrophobic composite material, It is characterized in that The following steps are involved: S1. Modifying the resin matrix using amino-functional polysiloxane to obtain a hydrophobically modified resin; S2. The hydrophobic modified resin and the fiber fabric are wet-laid to obtain a hydrophobic epoxy composite substrate preform; S3. The hydrophobic modified resin is mixed with the hydrophobic particles to prepare a super hydrophobic epoxy coating; S4. Spraying the super hydrophobic epoxy coating on the surface of the hydrophobic epoxy composite substrate preform; S5. Compression-molding and curing the coated hydrophobic epoxy composite substrate preform using a hard template having a surface microstructure.

5. A method for preparing a super-hydrophobic composite material according to claim 4, It is characterized in that The step S1 comprises: The amino functional polysiloxane is dissolved in 3-glycidyloxypropyltrimethoxysilane solvent, and after being stirred evenly, a curing agent is added, and after mixing, epoxy resin is added, and after mixing evenly, bubbles are discharged to obtain a hydrophobic modified resin.

6. A method for preparing a super-hydrophobic composite material according to claim 5, It is characterized in that The amino-functional polysiloxane is added in an amount of 1 to 15 wt % of the resin matrix / curing agent system, and the 3-glycidyloxypropyltrimethoxysilane solvent is added in an amount of 5 to 15 wt % of the resin matrix / curing agent system.

7. A method for preparing a super-hydrophobic composite material according to claim 4, It is characterized in that In the step S2, the fiber fabric and the hydrophobically modified resin are compounded in a mass ratio of 1:

1.

8. A method for preparing a super-hydrophobic composite material according to claim 4, It is characterized in that The step S3 comprises: The hydrophobic modified resin is dissolved in ethyl acetate, the hydrophobic powder is dispersed in anhydrous ethanol, and then the hydrophobic modified resin solution and the hydrophobic powder suspension are mixed.

9. A method for preparing a super-hydrophobic composite material according to claim 8, It is characterized in that The hydrophobic powder and anhydrous ethanol are mixed in a ratio of 1:2-3.5, the hydrophobic modified resin and ethyl acetate are mixed in a ratio of 1:0.75, and the mass ratio of the hydrophobic modified resin to the hydrophobic powder is 1:1-3.

5.

10. A method for preparing a super-hydrophobic composite material according to claim 4, It is characterized in that In step S4, multiple thin sprays are used for spraying, the spraying speed is 0.6-1.8 m / s, the spraying distance is 10-25 cm, the air pressure is 0.1-0.5 MPa, and each sample is sprayed 2-6 times, with an interval of more than 1 min each time.