High-strength optical fiber and manufacturing method thereof
Through the multi-layer eye mask mold extrusion and multi-layer coating design, the problem of insufficient fiber strength is solved, high-strength, lightweight and excellent bending performance is achieved, and high-performance fibers are suitable for special applications.
Patent Information
- Application Number
- CN202411029403.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
AI Technical Summary
The insufficient strength of existing optical fibers leads to large volume and weight in special applications, and poor bending performance and data transmission performance, making it difficult to meet the requirements of high strength and lightweight.
Multiple extrusions are carried out using multi-layer eye mask molds to penetrate each other, forming a stable hybrid layer, and improving the strength and protection performance of the optical fiber through the multi-layer coating layer design, including inner and outer protection. The layer is designed to optimize the diameter, eccentricity and attenuation performance of the optical fiber.
It realizes optical fibers with high strength, light weight, good bending performance and excellent optical performance, avoiding the problems of eccentricity and poor attenuation, and ensuring the appearance and use stability of the optical fiber.
Smart Images

Figure CN118884636A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical fibers, and in particular relates to a high-strength optical fiber and a manufacturing method thereof. Background Art
[0002] The strength of conventional optical fiber is generally only about 50N. Therefore, in order to ensure that the optical fiber has good fiber strength during use, a protective layer will be set on the outer layer of the optical fiber to form an optical cable. However, the volume and weight of the optical cable are 10-100 times that of the optical fiber. In some special occasions, special optical fibers with certain volume and weight requirements are required, such as emergency optical cables, sensor optical cables, and test optical cables. Because of their different construction methods and application environments, these special optical fibers have higher requirements for strength, bending performance, and data transmission performance.
[0003] How to realize an optical fiber with small volume, light weight and high strength and a method for manufacturing the same are problems that need to be solved urgently by those skilled in the art. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a high-strength optical fiber and a manufacturing method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] A method for manufacturing a high-strength optical fiber, comprising:
[0007] 1) The core covered with the cladding is coated with resin twice to form an optical fiber;
[0008] 2) The optical fiber is coated with a mixed material composed of a reinforcing material and epoxy resin to form a mixed layer on the optical fiber;
[0009] 3) The optical fiber coated with the mixed layer passes through a first mold provided with a multi-layer eye mask, so that the mixed materials penetrate each other through multiple extrusions of the multi-layer eye mask;
[0010] 4) The optical fiber passing through the first mold is cured for the first time and then passes through the second mold, so that the optical fiber diameter and eccentricity meet the preset requirements, and then is cured for the second time and coated with an outer sheath.
[0011] Furthermore, the apertures of the multi-layer eye mask of the first mold are designed in a stepped manner from large to small.
[0012] Furthermore, the reinforcing material is high molecular weight polyethylene material powder, aramid powder or basalt powder.
[0013] Furthermore, the diameter of the optical fiber is between 0.34 mm and 0.5 mm, the linear density is between 0.12 g / km and 0.15 g / km, the bending performance radius of 1 minute is less than 5 mm, and the eccentricity is less than 25 um; at a tensile rate of 50 m / min, the tensile strength of the optical fiber is at least 150 N; the attenuation performance of the optical fiber satisfies 1310 nm ≤ 0.4 dB / km and satisfies 1550 nm ≤ 0.3 dB / km.
[0014] Furthermore, the two resin coatings form a first coating layer and a second coating layer respectively; the Young's modulus of the resin coated on the first coating layer is between 0.3mpa and 0.8mpa, and the thickness of the first coating layer is between 40um and 75um; the second coating layer is resin coating, the Young's modulus of the resin coated on the second coating layer is between 300mpa and 500mpa, and the thickness of the first coating layer is between 35um and 50um; the thickness of the mixed layer is between 80um and 120um.
[0015] Furthermore, a carbon coating is provided between the cladding and the first coating layer.
[0016] Furthermore, a softener is added to the epoxy resin, and the ratio of the softener added is 2:1 to 7:1.
[0017] Furthermore, the epoxy resin is selected from thermosetting epoxy resin and UV curing epoxy resin.
[0018] Furthermore, the outer protective layer is made of acrylic resin, epoxy resin, nylon or polyimide material, and the thickness of the outer protective layer is between 20um and 50um.
[0019] A high-strength optical fiber is manufactured by the above manufacturing method. The optical fiber comprises, from the inside to the outside, a core, a cladding, a first coating layer, a second coating layer, a mixed layer formed by mixing and curing a reinforcing material and epoxy resin, and an outer sheath.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention provides a method for manufacturing a high-strength optical fiber. The method uses a multi-layer first mold to perform multiple extrusions so that the reinforcing material can achieve mutual penetration of the resin material and the reinforcing material in a relatively short time, strengthens the elasticity after curing, and stabilizes the mixed layer at a certain thickness, thereby avoiding the phenomenon that the mixed layer is thick, the optical fiber is prone to eccentricity, poor attenuation, and excessive diameter. It also avoids the phenomenon that the mixed layer is thin, resulting in insufficient adhesion between the reinforcing material and the optical fiber, and the reinforcing material is easy to fall off from the material, thereby resulting in insufficient tensile strength of the produced high-strength optical fiber, poor appearance, and the like.
[0022] The high-strength optical fiber of the present invention uses resin coating for the first coating layer, the Young's modulus of the coated resin is between 0.3mpa and 0.8mpa, and the thickness of the first coating layer is between 40um and 75um, thereby ensuring that the optical fiber can release the buffer stress well; the high-strength optical fiber of the present invention uses resin coating for the second coating layer, the Young's modulus of the coated resin is between 300um and 500mpa, and the thickness of the first coating layer is between 35um and 50um, and this design can ensure the strength of the optical fiber and also play a good protective role. The light-intensity optical fiber of the present invention designs the size and thickness of the included layers so that the optical fiber of the present invention has a small volume, light weight and high strength at the same time.
[0023] The high-strength optical fiber of the present invention is designed with an outer sheath. Since the mixed layer is obtained by mixing and curing a reinforcing material and an epoxy resin, the surface of the mixed layer is not completely smooth, and thus the attenuation is relatively large. Therefore, the design of the outer sheath can better improve the appearance and attenuation of the optical fiber, and can also make the surface of the optical fiber smooth, thereby avoiding the phenomenon of "fiber jamming" during use.
[0024] The present invention provides a high-strength optical fiber, which includes a core, a cladding, a first coating layer, a second coating layer, a mixed layer and an outer sheath. The high-strength optical fiber has the advantages of high strength, small size, light weight, good bending performance, good optical performance and good concentricity. The design of the mixed layer formed by mixing a reinforcing material with an epoxy resin enhances the strength and bending performance of the optical fiber of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is one of the structural schematic diagrams of the high-strength optical fiber in the embodiment;
[0026] Figure 2 This is one of the structural schematic diagrams of the high-strength optical fiber in the embodiment;
[0027] Figure 3 A schematic diagram of the composition of a processing system for high-strength optical fiber in an embodiment;
[0028] In the figure, 1-core and cladding; 2-first coating layer; 3-second coating layer; 4-mixed layer; 5-outer sheath; 6-carbon coating; 7-pay-off device; 8-tension wheel; 9-reinforcement material injection device; 10-first layer first mold; 11-second layer first mold; 12-third layer first mold; 13-resin; 14-first curing device; 15-guide wheel device; 16-second mold; 17-second curing device; 18-take-up device. DETAILED DESCRIPTION
[0029] Embodiment 1:
[0030] A method for manufacturing a high-strength optical fiber of the present invention comprises:
[0031] 1) The core covered with the cladding is coated with resin twice to form an optical fiber;
[0032] 2) Mixing the reinforcing material with the epoxy resin to form a mixed material and applying the mixed material on the optical fiber to form a mixed layer on the optical fiber;
[0033] 3) passing the optical fiber coated with the mixed layer through a first mold provided with a multi-layer eye mask, so that the reinforcing material of the mixed layer and the epoxy resin penetrate each other through multiple extrusions of the first mold, and then performing the first curing;
[0034] 4) Passing the optical fiber through the second mold so that the optical fiber diameter and eccentricity meet the preset requirements, and then performing a second curing;
[0035] 5) Cover the optical fiber with an outer sheath.
[0036] A high-strength optical fiber made by the above-mentioned manufacturing method, such as Figure 1 As shown, the optical fiber comprises, from the inside to the outside, a core and cladding 1, a first coating layer 2, a second coating layer 3 and an outer sheath 5, and a mixed layer 4 formed by mixing and curing a reinforcing material and an epoxy resin is provided between the second coating layer and the outer sheath.
[0037] Embodiment 2:
[0038] This example is further designed on the basis of the first embodiment in that: in this example, the apertures of the eye mask of the multi-layer first mold are designed in a stepped manner from large to small, and the apertures of the eye mask are arranged from large to small according to the traveling direction of the optical fiber.
[0039] Embodiment three:
[0040] This example is further designed on the basis of the first embodiment in that the reinforcing material in this example is high molecular polyethylene material powder, aramid powder or basalt powder.
[0041] Embodiment 4:
[0042] This example is further designed on the basis of Example 1 in that: the diameter of the optical fiber in this example is between 0.34 mm and 0.5 mm, the linear density is between 0.12 g / km and 0.15 g / km, the bending performance radius of 1 minute is less than 5 mm, and the eccentricity is less than 25 um; at a tensile rate of 50 m / min, the tensile strength of the optical fiber is at least 150 N; the attenuation performance of the optical fiber satisfies 1310 nm ≤ 0.4 dB / km and satisfies 1550 nm ≤ 0.3 dB / km, that is, for an optical signal with a wavelength of 1310 nm, its attenuation performance is less than or equal to 0.4 dB / km; for an optical signal with a wavelength of 1550 nm, its attenuation performance is less than or equal to 0.3 dB / km.
[0043] Embodiment five:
[0044] This example is further designed on the basis of Example 1 in that: the two coating layers of the optical fiber in this example include a first coating layer and a second coating layer; wherein the first coating layer is resin coated, the Young's modulus of the resin coated on the first coating layer is between 0.3 MPa and 0.8 MPa, and the thickness of the first coating layer is between 40-75 um; the second coating layer is resin coated, the Young's modulus of the resin coated on the second coating layer is between 300-500 MPa, and the thickness of the first coating layer is between 35-50 um; the thickness of the mixed layer is between 80 um and 120 um.
[0045] Embodiment six:
[0046] This example is further designed on the basis of the first embodiment: Figure 2 As shown, a carbon coating 6 is provided between the cladding and the first coating layer of the optical fiber in this example.
[0047] Embodiment seven:
[0048] This example is further designed on the basis of the first embodiment in that a softener is added to the epoxy resin in the present example, and the ratio of the softener added is 2:1 to 7:1.
[0049] Embodiment eight:
[0050] This example is further designed on the basis of the fifth embodiment in that the epoxy resin in this example can be selected from thermosetting epoxy resin and UV-curing epoxy resin, and the resin model can be selected according to the requirements of the optical fiber products and the manufacturing process of each manufacturer, such as 7228 or 1486.
[0051] Embodiment nine:
[0052] This embodiment is further designed on the basis of the first embodiment in that: the outer protective layer is made of acrylic resin, epoxy resin, nylon or polyimide material, and the thickness of the outer protective layer is between 20um and 50um.
[0053] Embodiment ten:
[0054] A high-strength optical fiber processing system of the present invention is used for processing the high-strength optical fiber described in any of the above embodiments, and the processing system includes a cladding processing unit, a first coating layer processing unit, a second coating layer processing unit, a mixed layer processing unit and an outer sheath processing unit;
[0055] like Figure 3 As shown, the mixed layer processing unit is provided with a pay-off device 7 including a tension wheel 8, a stepped penetration device and a take-up device 18;
[0056] The stepped penetration device includes a reinforcing material injection device 9, a penetration device formed by a first mold with a multi-layer eye mask and a first curing device 14 for penetrating resin material and reinforcing material, and an extrusion device formed by a guide wheel, a second mold 16 and a second curing device 17 for ensuring the diameter and eccentricity of the optical fiber.
[0057] In this example, a guide wheel device 15 is further provided between the first curing device and the second mold. The first mold has three layers (each layer is provided with an eye mold), including a first-layer first mold 10, a second-layer first mold 11 and a third-layer first mold 12. The three-layer first mold and the second mold are provided with resin 13.
[0058] The reinforcing material of the present invention enters the infiltration device together with the optical fiber through tension-free pay-off, and then is extruded by the eye mold of the first mold for multiple times, so that the reinforcing material and the resin material infiltrate each other.
[0059] Application Example 1:
[0060] This example uses the processing system and manufacturing method of the present invention to process and manufacture high-strength optical fibers. In this example, the reinforcing material is a high molecular polyethylene material; the Young's modulus of the resin coated on the first coating layer is 0.3 MPa, and the thickness is 40 um; the Young's modulus of the resin coated on the second coating layer is 300 MPa, and the thickness of the first coating layer is 35 um; the thickness of the mixed layer is 80 um; in this example, a carbon coating is also provided between the cladding and the first coating layer. In this example, a thermosetting epoxy resin is selected and a softener is added, and the ratio of the softener added is 2:1; in this example, an acrylic resin material is selected for the outer sheath, and the thickness of the outer sheath is 20 um; in this example, the first mold in the processing system is provided with 4 layers, and the eye mold aperture of the 4-layer first mold is designed in a stepped manner from large to small, and the specific value can be determined by the technician according to the requirements of the optical fiber finished product.
[0061] Application Example 2:
[0062] In this example, the processing system and manufacturing method of the present invention are used to process and manufacture high-strength optical fibers. In this example, aramid is selected as the reinforcing material; the Young's modulus of the resin coated on the first coating layer is 0.8 MPa, and the thickness is 75 um; the Young's modulus of the resin coated on the second coating layer is 500 MPa, and the thickness of the first coating layer is 50 um; the thickness of the mixed layer is 120 um; in this example, ultraviolet-curing epoxy resin is selected and a softener is added, and the ratio of the softener added is 7:1; in this example, epoxy resin is selected as the outer sheath, and the thickness of the outer sheath is 50 um; in this example, the first mold in the processing system is provided with 5 layers, and the eye mold apertures of the 5-layer first mold are designed in a stepped manner from large to small, and the specific values can be determined by technical personnel according to the requirements of the optical fiber finished product.
[0063] Application Example 3:
[0064] In this example, the processing system and manufacturing method of the present invention are used to process and manufacture high-strength optical fibers. In this example, basalt is selected as the reinforcing material; the Young's modulus of the resin coated on the first coating layer is 0.5 MPa and the thickness is 58 um; the Young's modulus of the resin coated on the second coating layer is between 400 MPa, and the thickness of the first coating layer is 43 um; the thickness of the mixed layer is 100 um; in this example, ultraviolet curing epoxy resin is added with a softener, and the ratio of the softener added is 4:1; in this example, nylon or polyimide material is selected as the outer sheath, and the thickness of the outer sheath is 35 um; in this example, the first mold in the processing system is provided with 3 layers, and the eye mold aperture of the 3-layer first mold adopts a stepped design from large to small, and the specific value can be determined by the technician according to the requirements of the optical fiber finished product.
[0065] Application Example 4:
[0066] This example uses the processing system and manufacturing method of the present invention to process and manufacture high-strength optical fibers. In this example, the fiber core uses 200um 200kpsi optical fibers, and the reinforcement material uses bulky high-density polyethylene with a linear density of 200dttm. In the processing system, the first mold is provided with 3 layers, and the eye mold aperture of the first mold is designed in a stepped manner from large to small. In this example, the eye mold aperture of the first layer of the first mold is 0.7, the eye mold aperture of the first layer of the first mold is 0.45, and the eye mold aperture of the first layer of the first mold is 0.32. In this example, thermosetting epoxy resin is selected and softener is added, and the ratio of softener added is 5:1. The second mold eye mold aperture is 0.35. A mixture of thermosetting epoxy resin and softener is introduced, and then cured again to produce a semi-finished product of high-strength optical fiber, the diameter of which is between 0.34-0.36mm. The semi-finished product uses a 0.4mm eye mold and polypropylene UV curing resin, and the resin modulus is 600mpa-800mpa. The finished product has a diameter of about 0.37-0.39mm. In this example, the line density of the finished product is 0.129g / km and the diameter is 0.38mm; at a tensile rate of 50m / min, the minimum tensile strength is 154N; the attenuation performance of the finished product meets: 1310nm≤0.329dB / km and meets 1550nm≤0.194dB / km; the bending performance radius of 1 minute is less than 5mm (thereby ensuring that the high-strength optical fiber of the present invention can be unbroken); the bending loss of 15mm radius is less than 0.1dB; the eccentricity of the finished product is 22um.
[0067] The high-strength optical fiber of the present invention has the advantages of high strength, small size, light weight, good bending performance, good optical performance and good concentricity. The design of the mixed layer formed by mixing the reinforcing material and the epoxy resin strengthens the strength and bending performance of the optical fiber of the present invention.
Claims
1. A method for manufacturing a high-strength optical fiber, characterized in that: include: 1) The core covered with the cladding is coated with resin twice to form an optical fiber; 2) The optical fiber is coated with a mixed material composed of a reinforcing material and epoxy resin to form a mixed layer on the optical fiber; 3) The optical fiber coated with the mixed layer passes through a first mold provided with a multi-layer eye mask, so that the mixed materials penetrate each other through multiple extrusions of the multi-layer eye mask; 4) The optical fiber passing through the first mold is cured for the first time and then passes through the second mold, so that the optical fiber diameter and eccentricity meet the preset requirements, and then is cured for the second time and coated with an outer sheath.
2. The method for manufacturing a high-strength optical fiber according to claim 1, characterized in that: The apertures of the multi-layer eye mask of the first mold are designed in a stepped manner from large to small.
3. The method for manufacturing a high-strength optical fiber according to claim 1, characterized in that: The reinforcing material is high molecular polyethylene powder, aramid powder or basalt powder.
4. The method for manufacturing a high-strength optical fiber according to claim 1, characterized in that: The diameter of the optical fiber is between 0.34 mm and 0.5 mm, the linear density is between 0.12 g / km and 0.15 g / km, the bending performance radius of 1 minute is less than 5 mm, and the eccentricity is less than 25 um; at a tensile rate of 50 m / min, the tensile strength of the optical fiber is at least 150 N; the attenuation performance of the optical fiber satisfies 1310 nm ≤ 0.4 dB / km and 1550 nm ≤ 0.3 dB / km.
5. The method for manufacturing a high-strength optical fiber according to claim 1, characterized in that: The two resin coatings form a first coating layer and a second coating layer respectively; the Young's modulus of the resin coated on the first coating layer is between 0.3mpa and 0.8mpa, and the thickness of the first coating layer is between 40um and 75um; the second coating layer is resin coating, the Young's modulus of the resin coated on the second coating layer is between 300mpa and 500mpa, and the thickness of the first coating layer is between 35um and 50um; the thickness of the mixed layer is between 80um and 120um.
6. The high-strength optical fiber according to claim 1, characterized in that: A carbon coating is further provided between the cladding layer and the first coating layer.
7. The high-strength optical fiber according to claim 1, characterized in that: The epoxy resin is added with a softener, and the ratio of the softener added is 2:1 to 7:
1.
8. The high-strength optical fiber according to claim 1, characterized in that: The epoxy resin is selected from thermosetting epoxy resin and ultraviolet curing epoxy resin.
9. The high-strength optical fiber according to claim 1, characterized in that: The outer protective layer is made of acrylic resin, epoxy resin, nylon or polyimide material, and the thickness of the outer protective layer is between 20um and 50um.
10. A high-strength optical fiber manufactured by the method for manufacturing a high-strength optical fiber according to any one of claims 1 to 9, characterized in that: The optical fiber comprises, from the inside to the outside, a core, a cladding, a first coating layer, a second coating layer, a mixed layer formed by mixing and curing a reinforcing material and epoxy resin, and an outer sheath.