Patterning composition, patterning film, semiconductor device and preparation method thereof
By introducing anti-aging agents with specific structures into the patterned composition, using epoxy structure to capture acid groups, the aging problem of composition is solved, the stability and storage cycle are improved, the cost is reduced, and the preparation effect of semiconductor devices is improved .
Patent Information
- Application Number
- CN202411269104.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-01
AI Technical Summary
The existing patterned compositions fail to age due to acidic instability during storage, which affects the preparation effect of semiconductor devices and is costly.
The patterned composition is introduced with an epoxy structure-containing anti-aging agent with a specific structure, which captures residual acid through the epoxy structure, inhibits the deprotection reaction, prolongs the storage period of the composition and improves stability.
The stability and storage cycle of the patterned composition are significantly improved, the cost of semiconductor devices is reduced, and the quality and preparation efficiency of micro patterns are improved.
Smart Images

Figure CN118884779A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of semiconductor preparation technology, and specifically to a patterned composition, a patterned film, a semiconductor device and a preparation method thereof. Background Art
[0002] With the development of integrated circuits and semiconductor technology, the industry's requirements for the preparation of micro-patterns in integrated circuits and semiconductor devices are becoming increasingly higher. Patterned compositions are key materials for realizing micro-patterned preparation, but due to reasons such as raw materials, trace amounts of acid are usually unavoidable in the system of patterned compositions. These residual acids will trigger a deprotection reaction of the film-forming resin in the system, causing the acidic unstable groups hanging on the film-forming resin to fall off, and continuously generating new acids in the patterned composition system, thereby causing the patterned composition to age and fail, thereby affecting its patterning effect in the preparation of semiconductor devices. Therefore, it is urgent to provide a patterned composition that can be stably present for a long time. Summary of the invention
[0003] In view of this, the embodiments of the present application provide a patterned composition, a patterned film, a semiconductor device and a method for preparing the same. The patterned composition includes an anti-aging agent, which includes a compound containing an epoxy structure with a specific structure, which can effectively inhibit the aging of the patterned composition, thereby improving the stability of the patterned composition and effectively inhibiting its aging failure during long-term storage and use.
[0004] In a first aspect, the present application provides a patterned composition, the patterned composition comprising a film-forming resin, a photoacid generator, a solvent and an additive, the additive comprising an anti-aging agent, and the anti-aging agent comprising a compound as shown in formula (I):
[0005] (Ⅰ) Among them, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 are independently selected from hydrogen, substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 ; The R 11 is selected from a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group; said R 12 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, or substituted or unsubstituted aryl; x is an integer from 1 to 12.
[0006] The anti-aging agent in the patterned composition provided in the present application includes a compound as shown in formula (I), which effectively captures the acid in the patterned composition system through the epoxy structure formed by the alicyclic body, thereby inhibiting the acid in the system from inducing the deprotection reaction of the film-forming resin, and further inhibiting the aging of the patterned composition, so that it can exist stably before being applied to patterning in semiconductor preparation, avoiding its aging failure, greatly reducing the production cost of semiconductor devices, and can also effectively improve the stability of the patterned composition in the patterning process of semiconductor device preparation and the quality of the obtained micro-pattern.
[0007] In some embodiments of the present application, when R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 When it is a substituted alkyl, substituted alkenyl, substituted alkynyl or substituted alkoxy, the substituent group is selected from one or more of a halogen atom, a hydroxyl group, a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, a substituted or unsubstituted alkynyl, a substituted or unsubstituted alkoxy, a substituted or unsubstituted aryl, and a substituted or unsubstituted aryloxy group.
[0008] In some embodiments of the present application, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 At least one of them is not a hydrogen atom.
[0009] In some embodiments of the present application, at least one of R4 and R5 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 ; and / or, at least one of said R6 and said R7 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 .
[0010] In some embodiments of the present application, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 The number of carbon atoms is less than or equal to 15.
[0011] In some embodiments of the present application, the anti-aging agent includes one or more compounds shown in formula (1) to formula (12): (1) ; (2) ; (3) ; (4); (5); (6); (7); (8); (9); (10); (11); (12); Wherein, m is an integer of 1-18, and n is an integer of 1-18.
[0012] In some embodiments of the present application, the weight percentage of the anti-aging agent in the patterned composition is 0.001%-2%.
[0013] In some embodiments of the present application, the additive further comprises a fluorine-containing resin, and the mass percentage of the fluorine-containing resin in the patterned composition is 0.05%-0.2%.
[0014] In some embodiments of the present application, in the patterned composition, the mass percentage of the film-forming resin is 2%-20%; and / or, the mass percentage of the photoacid generator is 0.1%-10%; and / or, the mass percentage of the solvent is 50%-98%.
[0015] In some embodiments of the present application, the film-forming resin includes an acrylic polymer.
[0016] In some embodiments of the present application, the patterned composition further includes a photodegradable base; the mass percentage of the photodegradable base in the patterned composition is 0.1%-10%.
[0017] In some embodiments of the present application, the acid residual concentration of the patterned composition after aging at 40°C for 42 days is less than or equal to 5×10 -3 mol / kg.
[0018] The second aspect of the present application provides a patterned film, which is formed by the patterned composition provided in the first aspect. The patterned composition provided in the present application has a good anti-aging effect, and adding it to the patterned composition can significantly improve its stability and anti-aging performance, thereby improving the quality and success rate of forming a patterned film on the surface of the relevant device.
[0019] The third aspect of the present application also provides a semiconductor device, which is prepared by coating the patterned composition provided in the first aspect on a substrate, and then exposing and developing, or by exposing and developing the patterned film provided in the second aspect. The patterned composition provided in the present application has good stability and can form a patterned film on the surface of a semiconductor device to produce a high-quality micro pattern.
[0020] A fourth aspect of the present application also provides a method for preparing a semiconductor device, comprising: Applying the patterning composition provided in the first aspect on a substrate to form a film layer on the substrate; The film layer is exposed and developed through a photomask to form a patterned film on the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The graphs are the variation curves of the residual acid concentration in the system over time when the patterned compositions of Example 1, Example 2 and Comparative Example 4 are stored at 40° C.; Figure 2 The curves of the residual acid concentration in the system of the patterned compositions of Comparative Examples 1 to 3 changing with time when stored at 40° C.; Figure 3 The curves of the residual acid concentration in the system of the patterned compositions of Example 3 and Comparative Example 5 changing with time when stored at 40° C.; Figure 4A The exposure performance test results of the patterned composition of Example 2 after being stored at 0° C. and 40° C. respectively; Figure 4B The exposure performance test results of the patterned composition of Comparative Example 1 after being stored at 0° C. and 40° C. respectively; Figure 4C The exposure performance test results of the patterned composition of Comparative Example 2 after being stored at 0° C. and 40° C. respectively; Figure 4D The exposure performance test results of the patterned composition of Comparative Example 3 after being stored at 0° C. and 40° C. respectively; Figure 5 The exposure performance test results of the patterned composition of Example 3 after being stored at 0° C. and 40° C. are summarized; Figure 6 The exposure performance test results of the patterned composition of Comparative Example 5 after storage at 0° C. and 40° C. are summarized. DETAILED DESCRIPTION
[0022] The present application is further described in detail below in conjunction with preferred embodiments, but the protection scope of the present application is not limited to the following specific embodiments.
[0023] In the present application, all professional terms have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present application.
[0024] Micro Electro Mechanical Systems (MEMS) is short for micro-electromechanical systems. MEMS devices are small in size, light in weight, high in precision, high in reliability, and high in sensitivity, making them very suitable for manufacturing miniaturized systems. With the development of technologies such as integrated circuits and semiconductors, the line width of integrated circuits continues to shrink and the degree of integration continues to increase. The requirements for the preparation of micro-patterns on the surface of MEMS devices are also getting higher and higher, that is, the requirements for micro-patterning are getting higher and higher. Micro-patterning in this application refers to the technology of transferring the micro-pattern on the mask to the substrate with the help of a patterned composition under the action of light or other energy activation. Taking the micro-patterning of the substrate in the preparation process of semiconductor devices as an example, the preparation process is mainly to first apply the patterned composition on the substrate to form a film layer on the substrate, and then transfer the pattern on the mask to the substrate through processes such as exposure, development, and etching to form a micro-geometric figure corresponding to the mask.
[0025] Usually, there are trace amounts of acid in the system of the patterned composition. These unavoidable residual acids caused by raw materials and other reasons will trigger the deprotection reaction of the film-forming resin in the system, causing the acidic unstable groups hanging on the film-forming resin to fall off, and constantly generating new acids in the patterned composition system, thereby causing the patterned composition to age and fail, thereby affecting its patterning effect in the preparation of semiconductor devices. Therefore, it is urgent to provide a patterned composition that can exist stably for a long time.
[0026] In order to solve the above problems, the present application provides a patterned composition, which includes a film-forming resin, a photoacid generator, a solvent and an additive, wherein the additive includes an anti-aging agent, and the anti-aging agent includes a compound containing an epoxy structure with a specific structure, which can effectively inhibit the aging of the patterned composition, thereby improving the stability of the patterned composition and effectively inhibiting its aging failure during long-term storage.
[0027] The present application provides a patterned composition, which includes a film-forming resin, a photoacid generator, a solvent and an additive, wherein the additive includes an anti-aging agent, and the anti-aging agent includes a compound shown in formula (I):
[0028] (Ⅰ) Among them, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10are independently selected from hydrogen, substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 ; The R 11 is selected from a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group; said R 12 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, or substituted or unsubstituted aryl; X is an integer of 1-12.
[0029] The patterned composition provided by the present application includes an anti-aging agent containing a compound as shown in formula (I). During the storage of the patterned composition, the epoxy structure formed by the alicyclic main body in the compound can effectively capture the trace residual acid in the patterned composition system through a special ring-opening reaction or interaction with hydrogen bonds, etc., to prevent the acid unstable groups hanging on the film-forming resin from falling off, and inhibit the generation of new acid, thereby effectively inhibiting it at the starting stage of aging, thereby inhibiting the film-forming resin from decomposing and failing due to deprotection reaction before exposure, and stably existing during storage, extending the storage period of the patterned composition, thereby improving its success rate of micro-patterning in the process of preparing semiconductor devices and the quality of the prepared micro-patterns, thereby improving the comprehensive performance of semiconductor devices. In addition, the patterned composition prepared by the compound can stably exist during storage, greatly reducing the loss cost of the patterned composition, thereby reducing the preparation cost of micro-patterning in the semiconductor preparation process, and improving the preparation efficiency, shortening the preparation process, and facilitating its industrial application.
[0030] In an embodiment of the present application, the anti-aging agent includes one or more compounds as shown in formula (I). In some embodiments of the present application, the anti-aging agent includes a compound as shown in formula (I). In other embodiments of the present application, the anti-aging agent includes a plurality of different compounds as shown in formula (I). The amount and type of the anti-aging agent in the patterned composition of the present application can be selected according to actual use requirements.
[0031] In the embodiments of the present application, the alkyl group may be a chain alkyl group or a cycloalkyl group. Chain alkyl groups are saturated hydrocarbon groups formed by removing a hydrogen atom from a chain alkane molecule, and may include straight-chain alkyl groups and branched-chain alkyl groups. Specifically, the alkyl group may include, but is not limited to, at least one of methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, cyclopentyl, 2-methylbutyl, 3-methylbutyl, 4-methylbutyl, 2,2-dimethylpropyl, n-hexyl, cyclohexyl, 2-methylhexyl, 3-methylhexyl, 4-methylpentyl, 5-methylpentyl, 2-ethylbutyl, 3-ethylbutyl, heptyl, octyl, nonyl and decyl. In some embodiments of the present application, the number of carbon atoms of the substituted or unsubstituted alkyl group is 1-18. In some specific embodiments, the number of carbon atoms in the substituted or unsubstituted alkyl group can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18.
[0032] In the embodiments of the present application, the alkenyl group may be an alkenyl group. An alkenyl group is a chain unsaturated hydrocarbon group containing at least one carbon-carbon double bond, and may include a straight-chain alkenyl group and a branched alkenyl group. Specifically, the alkenyl group may include, but is not limited to, at least one of vinyl, propenyl, allyl, isopropenyl, butenyl, butadienyl, and hexenyl. In some embodiments of the present application, the carbon number of the substituted or unsubstituted alkenyl group is 1-18. In some specific embodiments, the carbon number of the substituted or unsubstituted alkenyl group may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18.
[0033] In the embodiments of the present application, the alkynyl group is an unsaturated hydrocarbon group containing at least one carbon-carbon triple bond, and may include, but is not limited to, a straight chain alkynyl group and a branched chain alkynyl group. Specifically, the alkynyl group may include, but is not limited to, at least one of ethynyl, 1-propynyl, and 2-propynyl. In some embodiments of the present application, the number of carbon atoms of the substituted or unsubstituted alkynyl group is 1-18. In some specific embodiments, the number of carbon atoms of the substituted or unsubstituted alkynyl group may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18.
[0034] In the embodiments of the present application, an alkoxy group is a group consisting of an alkyl group bonded to an oxygen atom. Specifically, the alkoxy group may include, but is not limited to, at least one of a methoxy group, an ethoxy group, a propoxy group, a butoxy group, an isobutoxy group, and a tert-butoxy group. In some embodiments of the present application, the number of carbon atoms of the substituted or unsubstituted alkoxy group is 1-18. In some specific embodiments, the number of carbon atoms of the substituted or unsubstituted alkoxy group may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18.
[0035] In the embodiment of the present application, -(C=O)-R 11 In, R 11 is selected from a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group. 12 , R 12 Selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, or substituted or unsubstituted aryl. Among them, the halogen atom may include but is not limited to at least one of a fluorine atom, a bromine atom, and a chlorine atom. The aryl group is a monovalent group remaining after removing a hydrogen atom from the aromatic carbon of the aromatic hydrocarbon molecule. In the present application, the aryl group may include a monocyclic aryl group or a polycyclic aryl group. Specifically, the aryl group may include but is not limited to at least one of a phenyl group, a naphthyl group, an anthracene group, a tetraphenyl group, a pentacene group, and a tetrahydronaphthyl group. In some embodiments of the present application, the number of carbon atoms of the substituted or unsubstituted aryl group may be 6-18. Specifically, the number of carbon atoms of the substituted or unsubstituted aryl group may be 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18.
[0036] In some specific embodiments of the present application, -(C=O)-R 11 It can be a C2-C20 alkylcarbonyl group, that is, R 11 The number of carbon atoms of -(C=O)OR may be 1-19, and the C2-C20 alkylcarbonyl group may be, for example, an alkylcarbonyl group having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 carbon atoms. 12 It can be a C2-C20 alkyl ester group, and the number of carbon atoms in the C2-C20 alkyl ester group can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20.
[0037] In the embodiment of the present application, x in the compound shown in formula (I) is an integer of 1-12. Specifically, x can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12. That is to say, the number of carbon atoms in the alicyclic main structure of the compound shown in formula (I) is an integer of 6-17. Specifically, the number of carbon atoms in the alicyclic main structure of the compound shown in formula (I) can be, for example, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17. The present application limits the number of carbon atoms in the alicyclic main structure of the compound shown in formula (I) within a suitable range by limiting the size of x within a suitable range, thereby limiting the number of carbon atoms in the alicyclic main structure of the compound shown in formula (I) within a suitable range, so that the compound has good solubility in the patterned composition, and the epoxy structure can significantly exert its anti-aging effect, thereby improving the stability of the patterned composition during storage and extending the storage period of the patterned composition.
[0038] In the embodiment of the present application, when x is an integer of 2-12, the R2 connected to different carbon atoms may be all the same, partially the same, or all different; the R3 connected to different carbon atoms may be all the same, partially the same, or all different.
[0039] In the implementation manner of the present application, when R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 When it is a substituted alkyl, substituted alkenyl, substituted alkynyl or substituted alkoxy, the substituent group is selected from one or more of a halogen atom, a hydroxyl group (-OH), a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, a substituted or unsubstituted alkynyl, a substituted or unsubstituted alkoxy, a substituted or unsubstituted aryl, and a substituted or unsubstituted aryloxy group.
[0040] In the embodiments of the present application, the aryloxy group is a group composed of an aryl group bonded to an oxygen atom. In some embodiments of the present application, the carbon number of the substituted or unsubstituted aryloxy group is 6-18. Specifically, the carbon number of the substituted or unsubstituted aryloxy group can be 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18. Specifically, the aryloxy group can include, but is not limited to, at least one of phenoxy and naphthoxy.
[0041] In the embodiments of the present application, substitution means that at least one hydrogen atom in an alkyl, alkenyl, alkynyl, alkoxyl, or aryl group is replaced by a substituent group. In the embodiments of the present application, when multiple hydrogen atoms in an alkyl, alkenyl, alkynyl, alkoxyl, or aryl group are replaced by substituent groups, the substituent groups may be the same or different.
[0042] In some embodiments of the present application, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10In some embodiments, at least one of R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 are selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 ; Among them, R 11 , R 12 are selected from one or more of a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, and a substituted or unsubstituted aryl group. 10 The part in is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 , and the rest are hydrogen atoms. Compared with R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 All are hydrogen atoms. When R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 When at least one of the atoms is not a hydrogen atom, the compound as shown in formula (I) is less likely to polymerize, which can further improve the stability of the anti-aging agent.
[0043] In some embodiments of the present application, at least one of R4 and R5 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 ; and / or, at least one of R6 and R7 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 In some specific embodiments of the present application, any one of R4 and R5 is a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, a substituted or unsubstituted alkynyl, a substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 , the other is a hydrogen atom; and / or, any one of R6 and R7 is a substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 , the other is a hydrogen atom; where R11 is one or more selected from a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, and a substituted or unsubstituted aryl group; R 12 One or more selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted aryl. The present application can further enhance the anti-aging effect of the epoxy structure by selecting a special group at a special site of the compound shown in formula (I).
[0044] In some embodiments of the present application, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 The number of carbon atoms in R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 The number of carbon atoms in R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 The number of carbon atoms in R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 By controlling the number of carbon atoms within a suitable range, the length of the side chain grafted on the alicyclic main body of the compound as shown in formula (I) can be effectively controlled, thereby ensuring that the compound as shown in formula (I) has both good solubility and anti-aging effects, so that it can effectively play its anti-aging role in the patterned composite system, and avoid the compound as shown in formula (I) having too low solubility due to the excessive chain length of the grafted group, thereby preventing it from being unable to play its anti-aging effect in the patterned composite system.
[0045] In some embodiments of the present application, the anti-aging agent includes one or more compounds shown in formula (1) to formula (12): (1) ; (2) ; (3) ; (4); (5); (6); (7); (8); (9); (10); (11); (12); Wherein, m is an integer of 1-18, and n is an integer of 1-18.
[0046] In some specific embodiments of the present application, m can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, and n can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18. The m and n in formula (4) to (11) of the present application are only indicative of the number of methylene groups, and the values of m and n in formula (4) to (11) can be the same or different. The present application can effectively avoid the low solubility of the compound shown in formula (I) due to the excessive chain length of the group grafted on the alicyclic main structure, thereby preventing it from fully exerting the anti-aging effect in the patterned composition system, thereby further improving the anti-aging effect of the patterned composition.
[0047] The epoxy structure of the above-mentioned compounds has a better anti-aging effect. Adding them to the patterned composition can further improve the stability of the patterned composition. In addition, these compounds are easy to prepare or easily purchased on the market, and the acquisition cost is low. The patterned composition prepared by using the above-mentioned compounds can effectively reduce the production cost of semiconductor preparation.
[0048] In some embodiments of the present application, the mass percentage of the anti-aging agent in the patterned composition is 0.001%-2%. In some embodiments, the mass percentage of the anti-aging agent in the patterned composition can be, for example, 0.001%, 0.002%, 0.005%, 0.008%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%. The present application can further enhance its anti-aging effect while ensuring that the effect of the micro-patterning preparation of the patterned composition is not affected by controlling the content of the anti-aging agent in the patterned composition within a suitable range. In some specific embodiments, the mass of the anti-aging agent accounts for 0.01%-1% of the total mass of the patterned composition.
[0049] In some embodiments of the present application, the additive also includes a fluorine-containing resin. The fluorine-containing resin in the additive can play a hydrophobic role, improve the curing ability and hydrophobic properties of the patterned composition, and when a water film is formed on the surface of the coating, the water will not penetrate into the coating to affect the patterning process and the performance of the obtained patterned film, thereby further broadening the application scenarios of the patterned composition. In some specific embodiments of the present application, the fluorine-containing resin can be, for example, a methacrylate resin containing fluorine elements. In an embodiment of the present application, the mass percentage of the fluorine-containing resin in the patterned composition is 0.05%-2%. In some specific embodiments, the mass percentage of the fluorine-containing resin in the patterned composition can be, for example, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%. The present application can further improve the curing ability and hydrophobic properties of the patterned composition by controlling the content of the fluorine-containing resin in the patterned composition within a suitable range, thereby improving the quality of the patterned film obtained therefrom.
[0050] In the embodiment of the present application, the film-forming resin includes an acrylate polymer. The film-forming resin is one of the important components of the patterned composition, and can provide adhesion, chemical resistance and structural reliability for the patterned composition. The above-mentioned resin has high acid sensitivity. Under the action of acid or acid and high temperature, its hanging acidic groups are easy to fall off from the main chain of the resin, and the solubility reversal is obvious and the response speed is fast. The above-mentioned acrylate polymer refers to a structure in which the repeating units of its main chain include an addition reaction of acrylate, for example, the repeating units of its main chain include a structure in which methacrylate undergoes an addition reaction. In the present application, the acrylate polymer is a homopolymer or copolymer of acrylate and its derivatives, methacrylate and its derivatives. In some specific embodiments of the present application, the film-forming resin includes but is not limited to polyacrylate and polymethacrylate resin.
[0051] In some embodiments of the present application, the mass percentage of the film-forming resin in the patterned composition is 2%-20%. In some specific embodiments, the mass percentage of the film-forming resin in the patterned composition can be, for example, 2%, 3%, 4%, 5%, 8%, 10%, 12%, 15%, 16%, 18%, and 20%. The present application controls the content of the film-forming resin in the patterned composition within a suitable range, on the one hand, to ensure the film-forming performance and suitable coating viscosity of the patterned composition, and on the other hand, to effectively control the production cost of the patterned composition. In some embodiments of the present application, the patterned composition can be freeze-dried first, and then the obtained solid is tested by nuclear magnetic resonance to calculate the mass proportion of the film-forming resin in the patterned composition.
[0052] In some embodiments of the present application, a photoacid generator (PAG) refers to a compound that can react or dissociate to produce one or more acids (e.g., proton strong acid) under light conditions, and the above acid can act on the film-forming resin during the heat treatment process after irradiation, so that the solubility of the film-forming resin is reversed. In this way, the patterned composition is formed into a coating, and the coating is irradiated through a photomask, and then treated by development, etc., to obtain a preset pattern.
[0053] In some specific embodiments of the present application, the photoacid generator includes an ionic photoacid generator, the cation of the ionic photoacid generator is selected from phenylsulfonium salts, for example, triphenylsulfonium salts; its anion includes an anion fragment containing fluorine element; in some specific embodiments, the cation in the above-mentioned photoacid generator is , Anionic fragments include but are not limited to , , , , , , , , , The above-mentioned photoacid generator has certain transparency and absorptivity to light with a wavelength of 100 nm-380 nm, especially absorptivity to light with a wavelength of 193 nm, and has a high acid generation efficiency.
[0054] In some embodiments of the present application, the mass percentage of the photoacid generator in the patterned composition is 0.1%-10%. In some specific embodiments, the mass percentage of the photoacid generator in the patterned composition can be, for example, 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%. The present application can improve the exposure performance of the patterned composition, improve the clarity and contrast of the patterned film, and then improve the quality and precision of the obtained micro-pattern, and can also reduce its aging rate by adding a suitable amount of photoacid generator to the patterned composition. On the other hand, the acid content in the system can also be effectively controlled to avoid excessive aging of the film-forming resin. In some embodiments, the patterned composition can be subjected to freeze drying and other treatments to remove the solvent, and the solid matter obtained after freeze drying is dissolved in a quantitative deuterated reagent and subjected to nuclear magnetic resonance testing, and the nuclear magnetic resonance test results are normalized, and then the content of the photoacid generator in the patterned composition is calculated and determined.
[0055] In some embodiments of the present application, the patterning composition further includes a photo-decomposable base (PDB). PDB is a thermodynamically stable compound that is alkaline when not irradiated and can be decomposed into a neutral compound or a weakly acidic compound after irradiation. It can improve the exposure performance and post-exposure baking delay time of the patterning material composition, and can also improve the contrast of the pattern obtained after exposure and reduce the edge roughness of the obtained pattern. In some embodiments of the present application, the photo-decomposable base includes but is not limited to , , , , , , , The above-mentioned photoacid generator has certain transparency and absorptivity to light with a wavelength of 100 nm-380 nm and has a high acid generation efficiency.
[0056] In some embodiments of the present application, the mass percentage of the photodecomposition alkali in the patterned composition is 0.1%-10%. In some specific embodiments, the mass percentage of the photodecomposition alkali in the patterned composition can be, for example, 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%. The present application controls the content of the photodecomposition alkali in the patterned composition within a suitable range, while ensuring that the patterned composition contains sufficient effective component film-forming resin, and further improves the imaging quality of the micro-pattern obtained therefrom. In some embodiments, the patterned composition can be subjected to freeze-drying and other treatments to remove the solvent, and the solid substance obtained after freeze-drying is dissolved in a quantitative deuterated reagent and subjected to nuclear magnetic resonance testing, and the nuclear magnetic resonance test results are normalized, and then the content of the photodecomposition alkali in the patterned composition is calculated and determined.
[0057] In some embodiments of the present application, the patterning composition includes both a photoacid generator and a photodecomposition base. In this case, the specific selection of the photoacid generator and the photodecomposition base is different.
[0058] In the embodiment of the present application, the solvent in the patterned composition can be any solvent known in the art that can dissolve and disperse the aforementioned film-forming resin, the aforementioned photoacid generator, the aforementioned additives and other related components. In some specific embodiments, the above-mentioned solvent includes but is not limited to one or more of propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), γ-butyrolactone (GBL), cyclohexanone (CYC), diheptanone, etc. The above-mentioned type of solvent can better dissolve the components such as the film-forming resin, photoacid generator and additives mentioned above, which is conducive to obtaining a patterned composition with uniform components and high stability, and is conducive to improving the film-forming performance of the patterned composition; and when the patterned composition is used to prepare a patterned film, the above-mentioned solvent can be completely volatilized during the pretreatment process before the coating is irradiated, so as not to affect the formation of the patterned film and the quality of the patterned film.
[0059] In some embodiments of the present application, the mass percentage of the solvent in the patterned composition is 50%-98%. In some specific embodiments, the mass percentage of the solvent in the patterned composition can be, for example, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98%. The present application can improve the coating ability and component uniformity of the patterned composition while ensuring that the solvent can completely dissolve the film-forming resin, additives, photoacid generator and other components, and reduce the preparation cost of the patterned composition as much as possible by controlling the solvent within the above range.
[0060] In the embodiment of the present application, the acid residual concentration of the patterned composition after aging at 40°C for 42 days is less than or equal to 5×10 -3 In some specific embodiments, the acid residual concentration of the patterned composition after aging at 40° C. for 42 days may be less than or equal to 5×10 -3 mol / kg, less than or equal to 4×10 -3 mol / kg, less than or equal to 3×10 -3 mol / kg, less than or equal to 2×10 -3 mol / kg, less than or equal to 1×10 -3mol / kg. In the embodiments of the present application, the potentiometric titration method can be used to characterize the acid residual concentration in the patterned composition. In the present application, the stability of the patterned composition can be characterized by the acid residual concentration of the patterned composition after aging for a period of time at a certain temperature. The lower the acid residual concentration in the patterned composition after aging for a period of time at a certain temperature, the better its anti-aging effect, which proves that its stability is better and has a longer storage period. In some specific embodiments, the acid residual concentration of the patterned composition aged for 42 days at 40°C is used to characterize the high temperature stability of the patterned composition. After the patterned composition of the present application is aged at 40°C for a period of time, the acid residual concentration can still be maintained at a low level. This is because the epoxy-containing compound with a specific structure in the anti-aging agent can react with the residual acid in the patterned composition, thereby inhibiting the continuous generation of acid in the system, inhibiting the aging of the patterned composition, and then improving the stability of the patterned composition, extending the storage period of the patterned composition, and effectively avoiding its aging failure during long-term storage.
[0061] In some embodiments of the present application, in order to improve the comprehensive performance of the patterned composition, the additives may also include one or more of a leveling agent and a surfactant. The addition of a leveling agent and a surfactant can improve the uniformity of the coating film layer. The leveling agent and the surfactant can be added according to actual use requirements.
[0062] In one embodiment of the present application, a method for preparing a patterned composition includes: mixing a film-forming resin, a photoacid generator, an additive and a solvent to obtain a patterned composition. The method for preparing a patterned composition provided in the present application is simple, has a low preparation cost, and uses simple and readily available raw materials. The obtained patterned composition has excellent anti-aging effect, good stability, and a long storage period, which is conducive to commercial application.
[0063] The present application also provides a patterned film, which is formed by the patterned composition provided in the embodiment of the present application. The patterned film can be used as a high-precision mask in the patterning process of manufacturing integrated circuits, and the pattern of the patterned film can be transferred to a substrate such as a silicon wafer by etching to form a preset pattern on the substrate. Due to the good stability of the patterned composition provided in the embodiment of the present application, the patterned film obtained by the patterned composition has high patterning quality.
[0064] In one embodiment of the present application, a method for preparing a patterned film includes: coating a patterned composition on a substrate to form a film layer; exposing and developing the film layer through a photomask to form a patterned film on the surface of the substrate.
[0065] The present application provides a semiconductor device, which is made by using the patterned thin film described in any of the above embodiments. The semiconductor device provided by the present application has high precision, which is conducive to improving the comprehensive performance of the semiconductor device. In some embodiments of the present application, the semiconductor device includes a structure obtained by etching a film layer (i.e., a patterned thin film) formed by coating a structure to be patterned (such as a substrate to be patterned) with the above-mentioned patterned composition, and then exposing and developing the film layer to form a film.
[0066] In the present application, there is no limitation on the specific type of semiconductor device. In one embodiment of the present application, the semiconductor device may be an integrated circuit device including a chip. During the preparation of the chip, other functional layers may be prepared after the aforementioned patterning process is completed.
[0067] The present application also provides a method for preparing a semiconductor device, comprising: S101, coating the patterned composition described in any one of the above embodiments on a substrate to form a film layer on the substrate; S102, exposing the patterned composition coating, or the above-mentioned film layer, to an exposure light source through a photomask; S103, developing the exposed patterned composition coating or film layer with a developer to form a patterned thin film on the substrate.
[0068] The preparation method provided in the present application is simple, and the prepared semiconductor device has excellent comprehensive performance, which is conducive to its commercial application.
[0069] In step S101, the substrate can be selected according to actual needs. Specifically, the substrate can be, but is not limited to, a silicon wafer or a silicon wafer covered with a coating, and the coating can be, for example, an anti-reflective coating, an anti-etching coating, an epitaxial layer, a metal layer, a dielectric layer, a modified layer or a matching layer. Usually other coatings can be obtained by pre-treating the substrate. The pre-treatment method can be: subjecting the silicon wafer substrate to O2 plasma surface hydrophilic activation; or cleaning in Piranha solution (H2O: 30% ammonia: 30% H2O2 = 5:1:1) for 15 mins-20 mins, and then washing with deionized water and isopropanol to complete the hydrophilic treatment; or using evaporation or spin coating to cover hexamethyldisilazane (Hexamethyldisilazane, HMDS) on the substrate to perform surface hydrophobic treatment on the substrate; the hydrophobic treatment can be after the hydrophilic treatment; or adding a bottom antireflection layer (BARC), a bottom carbon-containing coating (Spin on carbon, SOC), or a bottom silicon-containing coating (Spin on glass, SOG).
[0070] In the embodiment of the present application, according to the size of the substrate, a suitable volume of the patterned composition is applied to the substrate by spin coating to form a patterned composition coating having a thickness of 5 nm-200 nm, and the surface roughness of the patterned composition coating may be less than 2 nm. For example, a 4-inch substrate may be spin coated with 1 mL-5 mL of the patterned composition.
[0071] In some embodiments of the present application, the substrate may be cleaned before coating to remove impurities and dust on the substrate surface. Specifically, the cleaning method may be, but is not limited to, using a solvent, acid, ultrasonic or spray cleaning, etc. In some embodiments of the present application, the cleaning method may be ultrasonic cleaning.
[0072] In step S102, the light source for exposure may be, but is not limited to, light with a wavelength of 100 nm-380 nm, X-rays, electron beams, ion beams, etc. In some specific embodiments of the present application, the light source for exposure may be light with a wavelength of 160 nm-200 nm.
[0073] In some embodiments of the present application, after coating, baking treatment can be performed before exposure to remove excess solvent in the film layer and improve the structural reliability of the patterned composition; baking treatment can also be performed after exposure and before development to promote chemical reactions in the coating. The baking temperature is 60°C-200°C, and the baking time is 20s-120s. Specifically, the baking temperature can be but not limited to 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, and the baking time can be but not limited to 20s, 40s, 60s, 80s, 100s or 120s, etc. In one embodiment of the present application, the baking temperature can be 60°C-150°C, and the baking time can be 20 s-80 s. In some specific embodiments of the present application, the baking temperature can be 100°C-200°C, and the baking time can be 70s-120s.
[0074] In step S103, a developing solution is used for developing treatment. Since the chemical properties of the exposed area in the film layer change and the solubility changes, the exposed film layer needs to be cleaned with a developing solution to obtain a patterned film. In the embodiment of the present application, the cleaning time is 10 s-300 s, and the cleaning can be divided into single-step cleaning and multi-step cleaning. In the cleaned film layer, if the exposed area is washed away, it is positive development to form a positive pattern, and the patterned composition is a positive patterned composition; if the exposed area is not washed away, it is negative development to form a negative pattern, and the patterned composition is a negative patterned composition.
[0075] In some embodiments of the present application, the developing solution includes a developer, and the developer can be selected according to the properties of the patterned composition and used in combination to improve the etching effect. The developing time is 10 s-120 s. Specifically, the developer can be selected from an organic solution, an inorganic solution, a pure solvent, a mixed solvent, a solvent containing other additives, etc. Specifically, in some embodiments of the present application, the developer can be a tetramethylammonium hydroxide (TMAH) aqueous solution with a concentration of 0.5-5%, or it can be an organic solvent such as ketones, alcohols, ethers, esters, lactones, and high-boiling alcohols, among which ketones can be, for example, cyclohexanone and methyl-2-n-pentyl ketone; alcohols can be, for example, 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol and diacetone alcohol; ethers can be, for example, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether , propylene glycol dimethyl ether, diethylene glycol dimethyl ether; esters can be, for example, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, 3-ethoxypropionic acid methyl ester, 3-ethoxypropionic acid ethyl ester, tert-butyl acetate, tert-butyl propionate and propylene glycol monotert-butyl ether acetate; lactones can be, for example, γ-butyrolactone; high boiling point alcohol solvents can be, for example, diethylene glycol, propylene glycol, glycerol, 1,4-butanediol, 1,3-butanediol. The developer can be a mixture of one or more of the above solvents. In some embodiments, after development, rinsing and baking are also included to remove impurities on the surface of the patterned film and improve the structural reliability of the patterned film.
[0076] In some embodiments of the present application, a patterned substrate can be obtained by coating a substrate to be patterned with the patterning composition, exposing and developing the formed film layer (ie, patterned film), and then etching the film layer.
[0077] The embodiment of the present application also provides a semiconductor device, which is made by using the patterned film provided by the embodiment of the present application or includes the above-mentioned patterned substrate. Due to the use of the patterned film provided by the embodiment of the present application, the semiconductor device provided by the embodiment of the present application has high precision.
[0078] In the embodiments of the present application, there is no special limitation on the structure of the semiconductor device, and those skilled in the art can design it based on actual application requirements and prepare it based on the patterned composition provided in the embodiments of the present application.
[0079] In the embodiments of the present application, there is no limitation on the specific type of semiconductor device. In some embodiments of the present application, the semiconductor device may be an integrated circuit device including a chip. In the preparation process of the chip, other functional layers may be prepared after the aforementioned patterning process is completed.
[0080] The present application also provides a method for preparing a semiconductor device, comprising: S201, coating the aforementioned patterned composition provided in the embodiment of the present application on a substrate to form a film layer on the substrate; S202, exposing and developing the film layer through a photomask to form a patterned thin film on the substrate.
[0081] The process parameters involved in the above process can all be found in the relevant description of the method for preparing the patterned film in the previous text, and will not be repeated here.
[0082] In some embodiments of the present application, after forming a patterned thin film on a substrate, the method for preparing the semiconductor device further includes: S203 , etching or electron injection is performed on the substrate to be patterned to form a patterned substrate, thereby obtaining a semiconductor device.
[0083] The technical solution of the present application is described in detail below with multiple embodiments.
[0084] Example 1 A patterned composition comprises a film-forming resin polymethacrylate resin, a photoacid generator, a photodecomposition base, an anti-aging agent as shown in formula (1), a solvent propylene glycol methyl ether acetate (PGMEA), and a fluorine-containing resin polymethacrylate resin containing a fluorine element; wherein the cation of the photoacid generator is , the anionic fragment is ; Photolysis of alkali to ; Specifically, based on the total mass of the patterned composition, the mass percentage of the film-forming resin is 3%, the mass percentage of the photoacid generator is 0.72%, the mass percentage of the photodecomposition base is 0.013%, the mass percentage of the anti-aging agent is 0.0125%, the mass percentage of the solvent is 96.1545%, and the mass percentage of the fluorine-containing resin is 0.1%; .
[0085] Example 2 The difference from Example 1 is that the anti-aging agent shown in formula (1) is replaced by the anti-aging agent shown in formula (13); based on the total mass of the patterned composition, the mass percentage of the anti-aging agent is 0.5%, and the mass percentage of the solvent is 95.667%; . (13) Example 3 The difference from Example 2 is that, based on the total mass of the patterned composition, the mass percentage of the film-forming resin is 4%, the mass percentage of the photoacid generator is 0.7%, the mass percentage of the photodecomposition base is 0.035%, the mass percentage of the anti-aging agent is 0.0049%, the mass percentage of the solvent is 95.1401%, and the mass percentage of the fluorine-containing resin is 0.12%, wherein the solvent is propylene glycol methyl ether (PGME), and the cation of the photoacid generator is , the anionic fragment is ; Photolysis of alkali to .
[0087] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples are provided.
[0088] Comparative Example 1 The difference from Example 1 is that the anti-aging agent shown in formula (1) is replaced by the anti-aging agent shown in formula (14): based on the total mass of the patterned composition, the mass percentage of the anti-aging agent is 0.5%; . (14) Comparative Example 2 The difference from Example 1 is that the anti-aging agent shown in formula (1) is replaced by the anti-aging agent shown in formula (15): based on the total mass of the patterned composition, the mass percentage of the anti-aging agent is 0.5%; . (15) Comparative Example 3 The difference from Example 1 is that the anti-aging agent shown in formula (1) is replaced by the anti-aging agent shown in formula (16): based on the total mass of the patterned composition, the mass percentage of the anti-aging agent is 0.5%; . (16) Comparative Example 4 The difference from Example 1 is that the patterning composition does not contain an anti-aging agent.
[0092] Comparative Example 5 The difference from Example 3 is that the patterning composition does not contain an anti-aging agent.
[0093] Performance Testing (1) The patterned compositions of the above-mentioned embodiments and comparative examples were placed at 40°C in the dark for aging test, and the changes of the residual acid concentration in the patterned compositions over time were monitored. The results are summarized in Figure 1-Figure 3 Among them, the time is measured in weeks.
[0094] (2) Exposure performance test: The patterned compositions of Example 2, Example 3 and Comparative Examples 1 to 3 were subjected to an exposure performance test. Specifically: Example 2: The patterned composition of Example 2 stored at 0°C and 40°C for 28 days (4 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 4A middle; Comparative Example 1: The patterned composition of Comparative Example 1 stored at 0°C and 40°C for 28 days (4 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 4B middle; Comparative Example 2: The patterned composition of Comparative Example 2 stored at 0°C and 40°C for 28 days (4 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 4C middle; Comparative Example 3: The patterned composition of Example 2 stored at 0°C and 40°C for 28 days (4 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 4D middle; Example 3: The patterned composition of Example 3 stored at 0°C and 40°C for 14 days (2 weeks), 28 days (4 weeks) and 42 days (6 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 5 middle; Comparative Example 5: The patterned composition of Comparative Example 5 stored at 0°C and 40°C for 14 days (2 weeks), 28 days (4 weeks) and 42 days (6 weeks) was exposed at different exposure doses (Dose). The variation curves of the film thickness FTK (Film Thickness) of the patterned composition with Dose are summarized in Figure 6 middle; Specifically, Figure 4A , Figure 4B , Figure 4C , Figure 4DThere are platform areas in each curve. The closer the starting point of the platform area of the curve corresponding to storage at 40°C for 28 days (4 weeks) is to the starting point of the platform area of the curve corresponding to 0°C, the more stable the patterned composition is and the better the exposure performance is.
[0095] In addition, Table 1 also summarizes the exposure parameters involved in the exposure of the patterned compositions of Example 2 and Comparative Example 4 to form a S56P90->50 pattern. In Table 1, EE (Energy) is exposure energy, FO (Focus) is focal length, K is the rate of change of feature size with energy, EL (Exposure) is exposure energy margin, DOF (Depth of Focus) is depth of focus, LCDU (Local Critical Dimension Uniformity) is line width uniformity, and CER (Circular Edge Roughness) is circular edge roughness.
[0096] Table 1
[0097] Combination Figure 1-Figure 3 It can be seen that the acid residual concentration of the patterned compositions provided in Examples 1 to 3 of the present application during long-term high-temperature (40°C) storage is significantly lower than that of Comparative Examples 4 and 5 without adding anti-aging agents and Comparative Examples 1 to 3 with adding other additives. In particular, the acid residual concentration remains relatively low after storage for 6 weeks (42 days). The lower the acid residual concentration, the better the anti-aging effect and the higher the stability. Although the compositions of Comparative Examples 1 to 3 also have epoxy structures, the carbon bridges in their structures have large steric hindrances, which will seriously hinder the ring opening of the epoxy structure in the compound, thereby affecting its anti-aging effect. In addition, Figure 1 and Figure 3 It is proved that the same patterned composition provided in the present application maintains a low acid residual concentration after being stored in different systems for 6 weeks (42 days), which means that the patterned composition provided in the embodiments of the present application has good stability and good anti-aging effect in different systems.
[0098] Combination Figure 4A , Figure 4B , Figure 4C , Figure 4D , Figure 5-Figure 6 , and the exposure performance test results in Table 1 show that the patterned composition provided in the embodiment of the present application still exhibits excellent exposure performance after being stored at a high temperature of 40° C. for 6 weeks (42 days). Therefore, the patterned composition provided in the present application has both good stability and excellent exposure performance.
Claims
1. A patterned composition, It is characterized in that The patterning composition comprises a film-forming resin, a photoacid generator, a solvent and an additive, wherein the additive comprises an anti-aging agent, and the anti-aging agent comprises a compound as shown in formula (I): (Ⅰ) Among them, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 are independently selected from hydrogen, substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 、-(C=O)OR 12 ; The R 11 is selected from a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group; said R 12 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, or substituted or unsubstituted aryl; x is an integer from 1 to 12.
2. The patterned composition according to claim 1, It is characterized in that When the R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 When it is a substituted alkyl, substituted alkenyl, substituted alkynyl or substituted alkoxy, the substituent group is selected from one or more of a halogen atom, a hydroxyl group, a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, a substituted or unsubstituted alkynyl, a substituted or unsubstituted alkoxy, a substituted or unsubstituted aryl, and a substituted or unsubstituted aryloxy group.
3. The patterned composition according to claim 1, It is characterized in that The R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 At least one of them is not a hydrogen atom.
4. The patterned composition according to claim 1, It is characterized in that The R 4 and the R 5 At least one of them is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 ; and / or, the R 6 and the R 7 At least one of them is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl, substituted or unsubstituted alkoxy, -(C=O)-R 11 OR-(C=O)OR 12 .
5. The patterned composition according to claim 1, It is characterized in that The R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 The number of carbon atoms is less than or equal to 15.
6. The patterned composition according to claim 1, It is characterized in that The anti-aging agent includes one or more compounds represented by formula (1) to formula (12): (1) ; (2) ; (3) ; (4); (5); (6); (7); (8); (9); (10); (11); (12); Wherein, m is an integer of 1-18, and n is an integer of 1-18.
7. The patterned composition according to claim 1, It is characterized in that The weight percentage of the anti-aging agent in the patterned composition is 0.001%-2%.
8. The patterned composition according to claim 1, It is characterized in that The additive further comprises a fluorine-containing resin, and the mass percentage of the fluorine-containing resin in the patterning composition is 0.05%-2%.
9. The patterned composition according to claim 1, It is characterized in that In the patterning composition, the mass percentage of the film-forming resin is 2%-20%; and / or the mass percentage of the photoacid generator is 0.1%-10%; and / or the mass percentage of the solvent is 50%-98%.
10. The patterned composition according to claim 1, It is characterized in that The film-forming resin includes an acrylic polymer.
11. The patterned composition according to claim 1, It is characterized in that The patterned composition further comprises a photodecomposable base; the mass percentage of the photodecomposable base in the patterned composition is 0.1%-10%.
12. The patterned composition according to claim 1, It is characterized in that The acid residual concentration of the patterned composition after aging at 40°C for 42 days is less than or equal to 5×10 -3 mol / kg.
13. A patterned film, It is characterized in that The patterned film is formed by using the patterned composition according to any one of claims 1 to 12.
14. A semiconductor device, It is characterized in that The semiconductor device is obtained by coating the patterned composition according to any one of claims 1 to 12 on a substrate, followed by exposure and development, or by exposing the patterned film according to claim 13 to light and developing.
15. A method for preparing a semiconductor device, It is characterized in that include: Applying the patterning composition according to any one of claims 1 to 12 on a substrate to form a film layer on the substrate; The film layer is exposed and developed through a photomask to form a patterned film on the substrate.
Citation Information
Patent Citations
Pattern formation material
JP1998163085A
Positive chemically amplifying photosensitive resin composition and method for manufacturing resist image
JP2002214765A
Photosensitive resin composition, pattern manufacturing method, cured film, organic el display device manufacturing method, and liquid crystal display device manufacturing method
WO2015064555A1
Active-ray-sensitive or radiation-sensitive resin composition, active-ray-sensitive or radiation-sensitive film, pattern formation method, and electronic device production method
WO2024004598A1