Carbon-coated aluminum foil for sheet battery and preparation process of carbon-coated aluminum foil
Through spraying, the carbon material is uniformly applied to the surface of the aluminum foil, which solves the problem of insufficient conductivity and stability of the aluminum foil, achieves uniform coverage and adhesion of the coating, and extends the service life of the thin-filled battery.
Patent Information
- Application Number
- CN202410900373.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
AI Technical Summary
The poor conductivity and insufficient surface stability of traditional aluminum foil in thin-filled batteries affect the charging and discharging efficiency and life of the battery. The preparation process of carbon coated aluminum foil is complicated, and problems of carbon material adhesion, uniformity and coating thickness need to be solved.
The carbon material is uniformly coated on the surface of the aluminum foil by spraying. Through ultrasonic dispersion and control of the viscosity, dispersant and binder concentration of the carbon coating slurry, optimize the spray parameters, ensure that the carbon material is evenly dispersed and coated evenly covered, and use deionized Water and neutral detergent are pretreated and dried.
It improves the conductivity and surface stability of aluminum foil, reduces uneven coating thickness and voids, enhances the adhesion effect of carbon materials, and extends the service life of the battery.
Abstract
Description
Technical Field
[0001] The invention relates to a preparation process of a carbon-coated aluminum foil, and more particularly to a carbon-coated aluminum foil for a thin-sheet battery and a preparation process thereof. Background Art
[0002] With the rapid development of modern electronic devices, thin-film batteries have become an important part of the market due to their high energy density, long cycle life and excellent safety performance. Thin-film batteries are widely used in various electronic products such as mobile phones, laptops, tablets and wearable devices. In order to further improve the performance and service life of thin-film batteries, researchers are constantly seeking ways to improve their electrode materials and preparation processes.
[0003] As one of the key materials in thin-film batteries, the performance of aluminum foil directly affects the overall performance of the battery. Traditional aluminum foil usually has problems such as poor conductivity and low surface stability, which affects the charging and discharging efficiency and life of the battery. In recent years, carbon-coated aluminum foil has gradually attracted attention as a new type of modified aluminum foil material. Carbon-coated aluminum foil can not only improve the conductivity of aluminum foil, but also enhance its surface stability and prevent corrosion and oxidation during battery operation by coating a layer of carbon material with good conductivity on the surface of aluminum foil.
[0004] Although carbon-coated aluminum foil has many advantages, its preparation process is relatively complicated and requires solving problems such as the adhesion between the carbon material and the aluminum foil, uniformity, and coating thickness. Summary of the invention
[0005] In order to solve the problems existing in the prior art, a carbon-coated aluminum foil for thin-film batteries and a preparation process thereof are provided. The specific scheme is as follows:
[0006] A process for preparing a carbon-coated aluminum foil for a thin-film battery comprises the following steps:
[0007] S1. Aluminum foil pretreatment:
[0008] Select high-purity aluminum foil with a thickness of 10 to 20 μm; put the aluminum foil into an ultrasonic cleaning machine and use deionized water and a neutral detergent to clean it for 10 to 15 minutes to remove oil and impurities on the surface; put the cleaned aluminum foil into an oven, set the temperature to 80 to 100°C, and dry it for 30 to 45 minutes to ensure that there is no moisture residue on the surface of the aluminum foil;
[0009] S2, preparing carbon coating slurry:
[0010] Adding carbon material to deionized water, adding dispersant and binder to control the viscosity of carbon coating slurry; the concentration of carbon material is controlled at 1-5wt%, and the concentration of dispersant is controlled at 0.5-2wt%;
[0011] S3, using a spraying method to evenly coat the carbon-coated material on the pretreated surface of the aluminum foil;
[0012] S4, drying and curing the aluminum foil coated with the carbon-coated material in an oven.
[0013] Furthermore, the parameters for coating S3 by spraying method are as follows: using a spraying device with an air pressure of 0.2-0.4 MPa, the distance between the nozzle and the surface of the aluminum foil is 15-20 cm, and the spraying speed is controlled at 10-20 cm / s to ensure uniform coating.
[0014] Furthermore, the parameters of drying and curing in S4 are to place the aluminum foil coated with the carbon material in an oven, set the temperature to 80-120° C., and dry for 30-60 min to ensure that the coating is completely dried.
[0015] Furthermore, the parameters of using an ultrasonic disperser to disperse the carbon material in S2 are an ultrasonic frequency of 20 to 40 kHz and a time of 30 to 60 minutes to ensure that the carbon material is evenly dispersed in the liquid.
[0016] Furthermore, the carbon material in S2 is at least one of carbon nanotubes, graphene and acetylene black.
[0017] Furthermore, the dispersant in S2 is one or a combination of polyvinylpyrrolidone, sodium polyacrylate and sodium dodecylbenzene sulfonate.
[0018] Furthermore, the nozzle has a diameter of 0.4 to 0.6 mm.
[0019] Furthermore, the concentration of the carbon material in S2 is controlled at 1-5 wt %, and the concentration of the dispersant is controlled at 0.5-2 wt %.
[0020] Furthermore, the viscosity of the carbon coating slurry is 100 cp to 300 cp.
[0021] The carbon-coated aluminum foil for thin-film batteries is prepared by the above-mentioned preparation process.
[0022] Beneficial effects:
[0023] The present invention provides a carbon-coated aluminum foil for thin-film batteries and a preparation process thereof. By strictly controlling the concentrations of carbon materials, dispersants and binders in the carbon-coated slurry and ultrasonic dispersion parameters, the carbon material is evenly dispersed in the coating liquid, thereby ensuring a consistent coating thickness. The spraying parameters are optimized, including the nozzle diameter, spraying speed and air pressure, to ensure that the coating is evenly coated on the surface of the aluminum foil, effectively reducing local uneven thickness and gaps. At the same time, the viscosity is controlled within the range of 100cP to 300cP, which can effectively avoid uneven spraying caused by excessively thick slurry and unstable coating caused by too thin slurry, and the appropriate coating viscosity enables the binder to fully play its role, ensuring that the carbon-coated material has a good adhesion effect on the surface of the aluminum foil. DETAILED DESCRIPTION
[0024] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0025] Embodiment 1:
[0026] (1) Aluminum foil pretreatment:
[0027] Select high-purity aluminum foil with a thickness of 15 μm.
[0028] The aluminum foil was placed in an ultrasonic cleaner and cleaned with deionized water and a neutral detergent for 12 min to remove oil and impurities on the surface.
[0029] Put the cleaned aluminum foil into the oven, set the temperature to 90℃, and dry it for 35 minutes to ensure that there is no moisture left on the surface of the aluminum foil.
[0030] (2) Preparation of carbon coating slurry:
[0031] Carbon nanotubes and graphene were mixed in a ratio of 3:2 and added into deionized water.
[0032] Polyvinylpyrrolidone was added as a dispersant, and the concentration of the dispersant was controlled at 1.5 wt %.
[0033] Polyvinylidene fluoride is added as a binder, and the concentration of the binder is controlled at 2 wt %.
[0034] An ultrasonic disperser was used with the ultrasonic frequency set to 30 kHz and the dispersion time set to 45 min to ensure that the carbon material was evenly dispersed in the liquid.
[0035] (3) Coating:
[0036] The carbon coating slurry is evenly coated on the pretreated surface of the aluminum foil by spraying.
[0037] Use a spraying device with an air pressure of 0.3 MPa, the distance between the nozzle and the aluminum foil surface is 18 cm, and the spraying speed is controlled at 15 cm / s to ensure uniform coating.
[0038] (4) Drying and curing:
[0039] The aluminum foil coated with the carbon-coated material was placed in an oven with the temperature set at 100 °C and the drying time set at 45 min to ensure that the coating was completely dry.
[0040] Embodiment 2:
[0041] (1) Aluminum foil pretreatment:
[0042] Select high-purity aluminum foil with a thickness of 12 μm.
[0043] Place the aluminum foil in an ultrasonic cleaner and clean it with deionized water and a neutral detergent for 10 min to remove oil and impurities on the surface.
[0044] Put the cleaned aluminum foil into the oven, set the temperature to 85℃, and dry it for 40 minutes to ensure that there is no moisture left on the surface of the aluminum foil.
[0045] (2) Preparation of carbon coating slurry:
[0046] Acetylene black was added into deionized water, and the concentration of carbon material was controlled at 3 wt %.
[0047] Sodium polyacrylate was added as a dispersant, and the concentration of the dispersant was controlled at 1 wt %.
[0048] Polyvinylidene fluoride was added as a binder, and the concentration of the binder was controlled at 1.5 wt %.
[0049] An ultrasonic disperser was used with the ultrasonic frequency set to 25 kHz and the dispersion time to 50 min to ensure that the carbon material was evenly dispersed in the liquid.
[0050] (3) Coating:
[0051] The carbon coating slurry is evenly coated on the pretreated surface of the aluminum foil by spraying.
[0052] Use a spraying device with an air pressure of 0.25 MPa, the distance between the nozzle and the aluminum foil surface is 17 cm, and the spraying speed is controlled at 12 cm / s to ensure uniform coating.
[0053] (4) Drying and curing:
[0054] The aluminum foil coated with the carbon-coated material was placed in an oven with the temperature set at 110 °C and the drying time set at 50 min to ensure that the coating was completely dry.
[0055] Embodiment 3:
[0056] (1) Aluminum foil pretreatment:
[0057] Select high-purity aluminum foil with a thickness of 18 μm.
[0058] Place the aluminum foil in an ultrasonic cleaner and clean it with deionized water and a neutral detergent for 15 minutes to remove oil and impurities on the surface.
[0059] Put the cleaned aluminum foil into the oven, set the temperature to 95℃, and dry it for 40 minutes to ensure that there is no moisture left on the surface of the aluminum foil.
[0060] (2) Preparation of carbon coating slurry:
[0061] Graphene was added into deionized water, and the concentration of carbon material was controlled at 4 wt%.
[0062] Sodium dodecylbenzene sulfonate was added as a dispersant, and the concentration of the dispersant was controlled at 1.8 wt %.
[0063] Polyvinylidene fluoride (PVDF) was added as a binder, and the concentration of the binder was controlled at 2 wt %.
[0064] An ultrasonic disperser was used with the ultrasonic frequency set to 35 kHz and the dispersion time to 40 min to ensure that the carbon material was evenly dispersed in the liquid.
[0065] (3) Coating:
[0066] The carbon coating slurry is evenly coated on the pretreated surface of the aluminum foil by spraying.
[0067] Use a spraying device with an air pressure of 0.35 MPa, the distance between the nozzle and the aluminum foil surface is 16 cm, and the spraying speed is controlled at 18 cm / s to ensure uniform coating.
[0068] (4) Drying and curing:
[0069] The aluminum foil coated with the carbon-coated material was placed in an oven with the temperature set at 120 °C and the drying time set at 60 min to ensure that the coating was completely dry.
[0070] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for preparing a carbon-coated aluminum foil for a thin-film battery, characterized in that: The following steps are involved: S1. Aluminum foil pretreatment: Select high-purity aluminum foil with a thickness of 10 to 20 μm; put the aluminum foil into an ultrasonic cleaning machine and use deionized water and a neutral detergent to clean it for 10 to 15 minutes to remove oil and impurities on the surface; put the cleaned aluminum foil into an oven, set the temperature to 80 to 100°C, and dry it for 30 to 45 minutes to ensure that there is no moisture residue on the surface of the aluminum foil; S2, preparing carbon coating slurry: Adding carbon material to deionized water, adding dispersant and binder to control the viscosity of carbon coating slurry; the concentration of carbon material is controlled at 1-5wt%, and the concentration of dispersant is controlled at 0.5-2wt%; S3, using a spraying method to evenly coat the carbon-coated material on the pretreated surface of the aluminum foil; S4, drying and curing the aluminum foil coated with the carbon-coated material in an oven.
2. The process for preparing a carbon-coated aluminum foil for thin-film batteries according to claim 1, characterized in that: The parameters for coating S3 by spraying method are as follows: using spraying equipment with air pressure of 0.2-0.4 MPa, the distance between the nozzle and the surface of the aluminum foil is 15-20 cm, and the spraying speed is controlled at 10-20 cm / s to ensure uniform coating.
3. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 1, characterized in that: The parameters for drying and curing in S4 are as follows: placing the aluminum foil coated with the carbon material in an oven, setting the temperature to 80-120° C., and drying time to 30-60 min to ensure that the coating is completely dried.
4. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 1, characterized in that: In S2, the parameters of using an ultrasonic disperser to disperse the carbon material are an ultrasonic frequency of 20 to 40 kHz and a time of 30 to 60 minutes to ensure that the carbon material is evenly dispersed in the liquid.
5. The process for preparing a carbon-coated aluminum foil for thin-film batteries according to claim 1, characterized in that: The carbon material in S2 is at least one of carbon nanotubes, graphene and acetylene black.
6. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 1, characterized in that: The dispersant in S2 is one or a combination of polyvinylpyrrolidone, sodium polyacrylate and sodium dodecylbenzene sulfonate.
7. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 2, characterized in that: The nozzle diameter is 0.4 to 0.6 mm.
8. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 1, characterized in that: The concentration of the carbon material in S2 is controlled at 1-5 wt %, and the concentration of the dispersant is controlled at 0.5-2 wt %.
9. The process for preparing a carbon-coated aluminum foil for thin-sheet batteries according to claim 1, characterized in that: The viscosity of the carbon coating slurry is 100cp~300cp.
10. Carbon-coated aluminum foil for thin-film batteries prepared by any one of the preparation processes of claims 1 to 9.