Method for testing insulation distance of crystalline silicon photovoltaic module
By intercepting samples on the back panel of the photovoltaic module and measuring their thickness under a confocal microscope, the problem that the existing technology cannot simulate the actual environment is solved, and effective detection and evaluation of the insulation distance of the crystalline silicon photovoltaic module is achieved, providing the extreme Performance reference under conditions.
Patent Information
- Application Number
- CN202410917917.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art cannot effectively simulate the actual use environment, and cannot fully test the insulation distance of the crystalline silicon photovoltaic module backplane, resulting in the inability to accurately evaluate its electrical insulation performance under extreme conditions.
By intercepting samples of different thicknesses on the back panel of the photovoltaic module, making metallographic samples, and measuring the thickness of the intermediate layer under a confocal microscope, calculating the average value of the shallow and deep layers, determining the risk of insulation distance, and simulating the actual use environment Perform a test.
It realizes effective detection of the electrical insulation performance of the backplane insulation layer of the finished photovoltaic module, provides a performance reference in actual use scenarios, and can effectively evaluate the risks of the components under extreme conditions.
Smart Images

Figure CN118890002A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaic module performance testing, and in particular relates to a method for testing the insulation distance of a crystalline silicon photovoltaic module. Background Art
[0002] Crystalline silicon photovoltaic modules have been widely used in the construction of ground photovoltaic power stations, distributed photovoltaic power stations, and water photovoltaic power stations. The areas where they are used are mostly characterized by extreme climate and meteorological conditions. They need to face strong ultraviolet radiation, high temperature and humidity, high altitude, strong wind and hail, blizzards, and extremely low temperatures. Therefore, the performance requirements of photovoltaic modules are extremely stringent. The backplane is a key component to protect photovoltaic modules, isolating the cells and module packaging materials from the atmosphere. Therefore, it is necessary to ensure that the backplane has good electrical insulation performance in a long-term use environment. In order to ensure the insulation performance, there are certain requirements for the thickness of the insulation layer of the insulating backplane used in photovoltaic modules. The insulation distance is an important indicator to test whether the material meets the requirements of good insulation.
[0003] At present, the method for testing the insulation distance of the backplane is usually for independent backplanes, not for finished photovoltaic modules in operation, so the current inspection method cannot fully simulate the actual use environment.
[0004] Therefore, it is necessary to provide a method for detecting and determining the insulation distance of crystalline silicon photovoltaic modules. Summary of the invention
[0005] The purpose of the present invention is to provide a crystalline silicon photovoltaic module insulation distance testing method to solve the above technical problems existing in the prior art.
[0006] To achieve the above object, the present invention provides the following solution: a method for testing the insulation distance of a crystalline silicon photovoltaic module, comprising the following steps:
[0007] Step S1, sample selection: two backsheet samples to be tested with different thicknesses are respectively intercepted from n different position areas on the backsheet surface of the photovoltaic module;
[0008] Step S2, sample preparation: cutting a backplane sample to be tested of a suitable size and bonding it to the side of the sub-sample made of cold mounting material, and using the same mounting material to perform secondary mounting on the sub-sample with the backplane sample to be tested, to obtain a metallographic sample; polishing the surface of the metallographic sample until a clear backplane layer structure is exposed;
[0009] Step S3, insulation distance test: place the metallographic sample under a calibrated confocal microscope to measure the thickness of the middle layer of the backplane sample to be tested, and record the data as JY 1深 , JY 2深 ...JYn 深 and JY1浅 , JY 2浅 ...JYn 浅 ;
[0010] Step S4, result processing: Calculate the recorded data to obtain JY 浅均 =(JY 1浅 +JY 2浅 +……+JY n浅 ) / n; according to the thickness of the intermediate layer of each backplane sample to be tested and JY 浅均 The difference in the insulation distance of the photovoltaic module is used to determine the risk.
[0011] Preferably, four corner positions and a middle position on the back panel surface of the photovoltaic module are respectively selected as sampling areas.
[0012] Preferably, when selecting samples, a layer of copy paper is laid on the surface of each sampling area, and a glass is laid flat on the copy paper. A 1 kg weight is used to roll the surface of each glass at a uniform speed for the same number of times to dye each sampling area.
[0013] Preferably, when selecting samples, two backplane samples to be tested, one with dark dyeing and the other with light dyeing, are selected in each sampling area.
[0014] Preferably, the sampling depth of the backplane sample to be tested extends from the backplane surface to the glass surface of the photovoltaic module.
[0015] Preferably, the sample preparation includes:
[0016] Use cold mounting material to make a sub-sample of 1 / 2 the size of the mounting mold according to the specifications of the mounting mold;
[0017] According to the height of the sub-sample, cut a backboard sample to be tested that is 4 mm shorter than the sub-sample, cut the backboard sample to be tested and stick it on the side of the sub-sample;
[0018] The sub-sample with the back plate sample to be tested is mounted for a second time and then polished to obtain a metallographic specimen.
[0019] Preferably, the cold mounting material is epoxy resin.
[0020] Preferably, the insulation distance test includes:
[0021] The confocal microscope was calibrated with a standard mass block, and the measurement uncertainty U of the confocal microscope was calculated. A confocal microscope with U ≤ 5% was selected for insulation distance test.
[0022] Preferably, the standard mass block is a feeler gauge or a gauge block with a nominal value.
[0023] Preferably, when the result is processed,1深 , JY 2深 ...JYn 深 Average ≥ JY 浅均 When the insulation distance of the PV panels is considered to be risk-free.
[0024] Compared with the prior art, the present invention at least discloses the following beneficial effects:
[0025] The method of the present invention can effectively simulate the actual use environment of photovoltaic modules and determine the risks of crystalline silicon photovoltaic modules during use by the change of insulation distance. It can effectively detect the electrical insulation performance of the backplane insulation layer of the finished photovoltaic module, providing an important reference for the performance of photovoltaic modules in actual use scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 It is a flow chart of the insulation distance testing method of the crystalline silicon photovoltaic module of the present invention;
[0028] Figure 2 It is a schematic diagram of sampling positions in the testing method of the present invention;
[0029] Figure 3 A schematic diagram of the process of sample preparation in the testing method of the present invention;
[0030] In the figure: 1. The first sampling area; 2. The second sampling area; 3. The third sampling area; 4. The fourth sampling area; 5. The fifth sampling area; 6. The photovoltaic module; 7. The junction box; 8. The sub-sample; 9. The metallographic specimen; 10. The backplane sample to be tested. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0033] Reference Figure 1As shown, the present invention provides a method for testing the insulation distance of a crystalline silicon photovoltaic module 6, comprising the following steps:
[0034] Step S1, sample selection: two backsheet samples 10 to be tested with different thicknesses are respectively cut from n different position areas on the backsheet surface of the photovoltaic module 6;
[0035] Step S2, sample preparation: cutting a backplane sample 10 to be tested of a suitable size and bonding it to the side of a sub-sample 8 made of a cold embedding material, and using the same embedding material to perform a secondary embedding on the sub-sample 8 to which the backplane sample 10 to be tested is bonded, to obtain a metallographic sample 9; polishing the surface of the metallographic sample 9 until a clear backplane layer structure is exposed;
[0036] Step S3, insulation distance test: place the metallographic sample 9 under a calibrated confocal microscope to measure the thickness of the middle layer of the back plate, and record the data as JY 1深 , JY 2深 ...JYn 深 and JY 1浅 , JY 2浅 ...JYn 浅 ;
[0037] Step S4, result processing: Calculate the recorded data to obtain JY 浅均 =(JY 1浅 +JY 2浅 +……+JY n浅 ) / n; when JY 1深 , JY 2深 ...JYn 深 Average ≥ JY 浅均 When , it is considered that the insulation distance of PV module 6 is risk-free.
[0038] In a specific embodiment:
[0039] Step S1, sample selection, comprising:
[0040] Five sampling areas are marked at the four corners and the middle of the back panel of the photovoltaic module 6, namely: the first sampling area 1, the second sampling area 2, the third sampling area 3, the fourth sampling area 4 and the fifth sampling area 5. The fifth sampling area 5 is located at the center of the back panel between the two junction boxes 7. Figure 2 As shown;
[0041] Lay a layer of copy paper on the surface of the five sampling areas. The size of the copy paper should cover the entire sampling area.
[0042] Take a 30*30cm glass, lay it flat on the copy paper, and roll a 1kg weight on the glass surface at a constant speed for 3 times;
[0043] The sampling positions are selected according to the depth of the color of the copy paper remaining on the backplane surface, and 5 dark positions and 5 light positions are selected respectively. A 2*2cm backplane sample 10 to be tested is intercepted at each position. The sampling depth of the backplane sample 10 to be tested needs to extend from the backplane surface to the glass surface of the photovoltaic module 6;
[0044] Complete sampling of 5 sampling areas in sequence to obtain dark samples 1深 , dark samples 2深 , dark samples 3深 , dark samples 4深 , dark samples 5深 , light-colored samples 1浅 , light-colored samples 2浅 , light-colored samples 3浅 , light-colored samples 4浅 , light-colored samples 5浅 .
[0045] It should be understood that, according to the size of the photovoltaic module 6, a plurality of different positions on the back panel surface may be selected for sampling, and the size of each sampling area is not limited to 30*30 cm.
[0046] Step S2, sample preparation, comprising:
[0047] First, a sub-sample 8 with a size of 1 / 2 of the mounting mold is prepared using a cold mounting material according to the specifications of the mounting mold; wherein the cold mounting material is used to fix and protect the backplane sample 10 to be tested, and epoxy resin can be selected.
[0048] According to the height of the sub-sample 8, a backboard sample 10 to be tested that is 4 mm shorter than the sub-sample 8 is cut, and then the cut backboard sample 10 to be tested is integrally attached to the sub-sample 8 with tape or adhesive;
[0049] The sub-sample 8 with the back plate sample 10 to be tested attached thereto is secondarily inlaid, specifically, the sub-sample 8 is inlaid using the same inlay material through an inlay mold to obtain a metallographic sample 9;
[0050] The surface of the metallographic sample 9 is polished by a grinding and polishing device until each layer structure of the backplane sample 10 to be tested can be clearly measured. Figure 3 shown.
[0051] Step S3, insulation distance test, including:
[0052] Use a feeler gauge or a gauge block with a nominal value to calibrate the confocal microscope, calculate the measurement uncertainty U of the confocal microscope, and select a confocal microscope with U≤5% for insulation distance test; when U>5%, it is considered that the test error of the confocal microscope is large and cannot meet the test; the measurement uncertainty U can be estimated by dividing the standard deviation by the square root of the number of measurements;
[0053] Place the metallographic sample 9 under a confocal microscope to measure the thickness of the middle layer of the back plate and record it as JY 1深 , JY 2深 , JY 3深 , JY 4深 , JY 5深 , JY 1浅 , JY 2浅 , JY 3浅 , JY 4浅 , JY 5浅 .
[0054] Step S4, result processing, includes:
[0055] The average insulation distance of the light-colored samples is calculated based on the insulation distance measurement values of the five light-colored samples, JY 浅均 =(JY 1浅 +JY 2浅 +JY 3浅 +JY 4浅 +JY 5浅 ) / 5;
[0056] The insulation distance measurements of the five dark-colored samples were compared with the average insulation distance of the light-colored samples. 1深 , JY 2深 , JY 3深 , JY 4深 , JY 5深 ≥90%JY 浅均 When the insulation distance of the photovoltaic module 6 is considered to be risk-free; when JY 1深 , JY 2深 , JY 3深 , JY 4深 , JY 5深 Any one of them is less than 90%JY 浅均 When , it is considered that there is a risk in the insulation distance of photovoltaic module 6.
[0057] The details not described in detail in the present invention are all conventional technical means known to those skilled in the art.
[0058] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0059] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for testing the insulation distance of a crystalline silicon photovoltaic module, characterized in that: The following steps are involved: Step S1, sample selection: two backsheet samples to be tested with different thicknesses are respectively intercepted from n different position areas on the backsheet surface of the photovoltaic module; Step S2, sample preparation: cutting a backplane sample to be tested of a suitable size and bonding it to the side of the sub-sample made of cold mounting material, and using the same mounting material to perform secondary mounting on the sub-sample with the backplane sample to be tested, to obtain a metallographic sample; polishing the surface of the metallographic sample until a clear backplane layer structure is exposed; Step S3, insulation distance test: place the metallographic sample under a calibrated confocal microscope to measure the thickness of the middle layer of the backplane sample to be tested, and record the data as JY 1深 , JY 2深 ...JYn 深 and JY 1浅 , JY 2浅 ...JYn 浅 ; Step S4, result processing: Calculate the recorded data to obtain JY 浅均 =(JY 1浅 +JY 2浅 +……+JY n浅 ) / n; according to the thickness of the intermediate layer of each backplane sample to be tested and JY 浅均 The difference in the insulation distance of the photovoltaic module is used to determine the risk.
2. The crystalline silicon photovoltaic module insulation distance testing method according to claim 1, characterized in that: Four corner positions and a middle position on the back panel of the photovoltaic module are selected as sampling areas.
3. The crystalline silicon photovoltaic module insulation distance testing method according to claim 2, characterized in that: When selecting samples, a layer of copy paper is laid on the surface of each sampling area, and a glass is laid flat on the copy paper. A 1 kg weight is used to roll the surface of each glass at a uniform speed for the same number of times to dye each sampling area.
4. The crystalline silicon photovoltaic module insulation distance testing method according to claim 3, characterized in that: When selecting samples, two backboard samples to be tested, one with dark dyeing and the other with light dyeing, are selected in each sampling area.
5. The crystalline silicon photovoltaic module insulation distance testing method according to claim 4, characterized in that: The sampling depth of the back sheet sample to be tested extends from the back sheet surface to the glass surface of the photovoltaic module.
6. The crystalline silicon photovoltaic module insulation distance testing method according to claim 1, characterized in that: Sample preparation includes: Use cold mounting material to make a sub-sample of 1 / 2 the size of the mounting mold according to the specifications of the mounting mold; According to the height of the sub-sample, cut a backboard sample to be tested that is 4 mm shorter than the sub-sample, cut the backboard sample to be tested and stick it on the side of the sub-sample; The sub-sample with the back plate sample to be tested is mounted for a second time and then polished to obtain a metallographic specimen.
7. The crystalline silicon photovoltaic module insulation distance testing method according to claim 6, characterized in that: The cold mounting material is epoxy resin.
8. The crystalline silicon photovoltaic module insulation distance testing method according to claim 1, characterized in that: Insulation distance tests include: The confocal microscope was calibrated with a standard mass block, and the measurement uncertainty U of the confocal microscope was calculated. A confocal microscope with U ≤ 5% was selected for insulation distance test.
9. The crystalline silicon photovoltaic module insulation distance testing method according to claim 8, characterized in that: The standard mass block is a feeler gauge or a gauge block with a nominal value.
10. The crystalline silicon photovoltaic module insulation distance testing method according to claim 4, characterized in that: When the result is processed, 1深 , JY 2深 ...JYn 深 Average ≥ JY 浅均 When the insulation distance of the PV panels is considered to be risk-free.