Preparation method of photoelectric detector
Through rare earth doping CsPbI3 perovskite quantum dot material and quantum dot heterojunction, combined with quantum cutting fluorescence conversion film, an efficient and stable deep ultraviolet-visible-near-infrared broadband photodetector is achieved, solving the existing medium-wide wide technology The poor effect and high cost of spectral photodetectors have achieved efficient and stable photodetection effects.
Patent Information
- Application Number
- CN202410918904.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing wide-spectrum photodetectors have limited detection effects in the deep ultraviolet-visible-near-infrared wavelength range, and are costly and have high system complexity, making it difficult to achieve efficient and stable broadband photodetection.
Using rare earth-doped CsPbI3 perovskite quantum dot material, CsPbI3:RE3+-PbS quantum dot heterojunction was constructed, and efficient and stable quantum tailored fluorescence conversion film was prepared to achieve deep ultraviolet-visible-near-infrared broadband photoelectricity through these technical means. Preparation of detectors.
Achieve efficient and stable 200nm-1700nm broadband photodetector, with a fluorescent quantum yield of more than 90%. After storage for one year, it still maintains luminous performance of more than 95%, widens the light detection wavelength, improves the photoelectric response capability, and the overall detection rate Achieved above 1013 Jones.
Smart Images

Figure CN118890944A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photoelectric detection, and in particular to a method for preparing a photoelectric detector. Background Art
[0002] As one of the basic optoelectronic components, photodetectors play an important role in applications such as remote sensing, reconnaissance, medical detection and imaging. Conventional photodetectors select corresponding photoelectric response materials according to the different light response wavelengths and are suitable for different scenarios. For example, ultraviolet wavelength detection is based on GaN photodetectors; Si photodetectors are selected for visible to near-infrared wavelengths; and InGaAs photodetectors are used for near-infrared wavelengths.
[0003] As the demand for photoelectric detection becomes increasingly complex, photoelectric detectors working in different bands are gradually integrated and used for wide-spectrum detection of the same scene. Limited by the volume and mission modules of the integrated system, conventional wide-spectrum detection tasks often require multiple photoelectric detectors with different wavelength responses to work together, which greatly increases the complexity of the system and is costly. Summary of the invention
[0004] At present, the research on deep ultraviolet-visible-near-infrared broadband photodetectors is mainly based on the following two modes: 1. Selecting narrow bandgap semiconductor materials with wide spectral absorption; 2. Constructing a stacked heterostructure and utilizing the synergistic effect of materials with different wavelength responses to achieve broadband detection. Although the above method can achieve deep ultraviolet-visible-near-infrared broadband detection, it is limited by the material light absorption coefficient and device preparation process. There are still many challenges in broadband photodetectors, such as technology, performance and cost. The applicant has previously studied rare earth (RE 3+ ) Based on the synthesis of CsPbX3 perovskite quantum dots and the research on photoelectric detectors, we intend to systematically study the effect of rare earth doping on the photoelectric properties of CsPbI3 perovskite quantum dots; in-depth study of CsPbI3:RE 3+ -PbS quantum dot heterojunction luminescence mechanism, charge transport and interface interaction; preparation of efficient and stable quantum tailored fluorescence conversion films and the same CsPbI3:RE 3+ -Effective coupling of PbS quantum dot heterojunction. Ultimately, the goal is to achieve efficient and stable deep ultraviolet-visible-near infrared (200nm-1700nm) broadband response photodetectors, providing a new solution for the preparation of efficient and stable broadband photodetectors.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a photoelectric detector comprises the following steps:
[0007] Synthetic RE3+ Doping CsPbI3 PQDs: Prepare cesium oleate precursor. Dissolve 0.375mM PbI2 and 0.375mM rare earth iodide in the reaction solution under nitrogen environment. The reaction solution is a mixture of 15mL octadecene, 1.5mL oleic acid and 1.5mL oleylamine. React at 110-130 degrees Celsius for 1h, then heat to 210-230 degrees Celsius and inject 1mL cesium oleate precursor. Cool and centrifuge to obtain RE 3+ Doped CsPbI3 PQDs;
[0008] Preparation of CsPbI3:RE 3+ -PbS quantum dot heterojunction: synthesize PbS quantum dots and mix PbS quantum dots with RE at a mass ratio of 2:1 3+ Doped CsPbI3 PQDs were mixed, stirred for 20-26h in the dark, and centrifuged to obtain CsPbI3:RE 3+ -PbS quantum dot heterojunction;
[0009] Preparation of quantum tailored fluorescence conversion film: prepare cesium oleate precursor, add YbCl3 and PbCl2 in a molar ratio of 1:1 to the reaction solution, the reaction solution is a mixture of 15mL octadecene, 1.5mL oleic acid and 1.5mL oleylamine, react for 1h in a nitrogen environment at 110-130 degrees Celsius, heat to 220-260 degrees Celsius and inject cesium oleate precursor, quickly cool after 10s, add toluene solution and centrifuge to obtain quantum tailored luminescent quantum dots, use short-chain ligands to exchange with long-chain ligands on the surface of quantum tailored luminescent quantum dots and use highly hydrophobic and antioxidant organic polymers to modify the quantum tailored luminescent quantum dots to obtain quantum tailored fluorescence conversion film;
[0010] Preparation of photodetector: coupling quantum tailored fluorescence conversion film on the outer layer of conductive glass, and then setting electron transport layer, CsPbI3:RE on the upper layer of conductive glass 3+ -PbS quantum dot heterojunction, hole transport layer and electrode layer to obtain a photodetector.
[0011] As a further solution of the present invention: the steps of preparing the cesium oleate precursor are as follows: 0.8g CsCO3 is dissolved in 25mL octadecene and 1.5mL oleic acid, and reacted in a nitrogen atmosphere at 100-130 degrees Celsius for 2h to completely dissolve it, thereby obtaining the cesium oleate precursor.
[0012] As a further solution of the present invention: the iodide rare earth adopts at least one of CeI3, NdI3, ErI3, TmI3 and PrI3.
[0013] As a further scheme of the present invention: the steps of synthesizing PbS quantum dots are as follows: add 0.5mM lead oxide to a mixed solution of oleic acid and octadecene, stir for 1h under a nitrogen atmosphere at 130-160 degrees Celsius, then add 0.25mM bis(trimethylsilyl) sulfide, react for 5h, cool to room temperature, add toluene solution and centrifuge to obtain PbS quantum dots.
[0014] As a further solution of the present invention: the short-chain ligand is ethanedithiol, mercaptopropionic acid, etc.
[0015] As a further solution of the present invention: the electrode layer is a gold electrode layer.
[0016] As a further solution of the present invention: the electron transport layer, CsPbI3:RE 3+ -PbS quantum dot heterojunction and hole transport layer are arranged on the upper layer of conductive glass, and the electrode layer is arranged on the upper layer of the hole transport layer by evaporation.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention obtains RE with excellent photoelectric performance 3+ The CsPbI3-doped PQDs material has a photoluminescence quantum yield (PLQYs) of more than 90%, and can still maintain more than 95% of the initial value of luminescence performance after one year of storage;
[0019] By constructing CsPbI3:RE 3+ -PbS quantum dot heterojunction, broadening the light detection wavelength to the near-infrared range, while promoting charge transfer between the two, improving the photoelectric response capability of the overall device; preparing efficient and stable quantum tailored fluorescence conversion films, based on efficient light-light-electricity conversion mechanism, enhancing the device's response capability in deep ultraviolet to ultraviolet wavelengths;
[0020] A 200nm-1700nm broadband photodetector was prepared, with an overall detection rate of more than 1013Jones; the device was properly packaged so that it could still maintain an initial detection rate of more than 95% after being stored for one year. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the structure of a photoelectric detector prepared by the method for preparing a photoelectric detector in an embodiment of the present invention.
[0022] In the figure: 1-Quantum tailored fluorescence conversion film, 2-Conductive glass, 3-Electron transport layer, 4-CsPbI3:RE 3+-PbS quantum dot heterojunction, 5-hole transport layer, 6-electrode layer. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] To achieve efficient deep UV-visible-near infrared broadband perovskite PDs, the following aspects need to be explored in depth: 1. Systematic research on RE 3+ Control of photoelectric properties of CsPbI3 PQDs by doping; 2. Mastering CsPbI3:RE 3+ -PbS heterojunction interface interaction and charge transport mechanism; 3. Prepare efficient and stable UV absorption and near-infrared emission quantum tailored fluorescence conversion films to enhance the deep UV-UV response of PDs. Thus, a deep UV-visible-near infrared (200nm-1700nm) broadband, high detection sensitivity and low-cost photodetector is obtained.
[0025] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0026] See also Figure 1 , a method for preparing a photoelectric detector provided by an embodiment of the present invention comprises the following steps:
[0027] A.RE 3+ Synthesis of doped CsPbI3 PQDs
[0028] Taking the preparation of CsPbI3 PQDs as an example, an improved hot injection method was used for synthesis. First, the required cesium oleate precursor was prepared, that is, 0.8g CsCO3 was dissolved in 25mL octadecene and 1.5mL oleic acid, and reacted at 120 degrees Celsius under nitrogen protection for 2h to completely dissolve it to obtain the cesium oleate precursor. In addition, 0.375mM PbI2 was dissolved in 15mL octadecene, 1.5mL oleic acid and 1.5mL oleylamine in a nitrogen-filled environment. React at 120 degrees Celsius for 1h until PbI2 is completely dissolved and clear. Subsequently, the temperature was raised to 220 degrees Celsius and 1mL of cesium oleate precursor was injected. After reacting for 10s, it was quickly transferred to an ice water bath and cooled to room temperature. Finally, toluene solution was added to the solution for centrifugation and washing to obtain CsPbI3 PQDs. For RE 3+The synthesis of doped CsPbI3 PQDs was similar. When PbI2 was added, rare earth iodide (such as CeI3, NdI3, ErI3, TmI3, PrI3) was added to the reaction solution at a molar ratio of 1:1, and the reaction was carried out at 120 degrees Celsius for 1 hour. Then the temperature was raised to 220 degrees Celsius, 1 mL of cesium oleate precursor was injected, cooled and centrifuged, and RE was obtained. 3+ Doped CsPbI3 PQDs. By changing the ratio of PbI2 to REI3 in the solution, perovskite quantum dots (PQDs) with different doping concentrations were synthesized; a variety of rare earth iodide ion pairs were introduced, such as Ce 3+ -Nd 3+ , Ce 3+ -Nd 3+ -Er 3+ Etc., to prepare RE 3+ Double-doped or triple-doped CsPbI3PQDs.
[0029] B. Preparation of CsPbI3:RE 3+ -PbS quantum dot heterojunction
[0030] Preparation of CsPbI3:RE 3+ -The following two synthesis methods are commonly used for PbS quantum dot heterojunctions: liquid phase epitaxial growth method and self-assembly method. This application intends to use the self-assembly method to prepare quantum dot heterojunctions, mainly based on the different surface ligands of the two materials, which make them carry different charges. Stirring at room temperature, constructing the heterojunction by electrostatic adsorption, this method has the advantages of simple operation and high repeatability. PbS quantum dot synthesis, that is, lead oxide (0.5mM), oleic acid and octadecene are stirred at 150 degrees Celsius under nitrogen conditions for 1h, and then bis(trimethylsilyl) sulfide (0.25mM) is added to the above solution. After reacting for 5h, it is cooled to room temperature, and toluene solution is added for centrifugation to obtain PbS quantum dots. PbS quantum dots are mixed with RE 3+ CsPbI3:RE was obtained by mixing the doped CsPbI3 PQDs (mass ratio of 1:0.5), stirring for 24 h in the dark, and then centrifuging. 3+ -PbS quantum dot heterojunction. By comparing different preparation conditions, different CsPbI3:RE 3+ -PbS quantum dot heterojunction, and determine the optimal experimental scheme. Finally, spin coating was used to prepare visible-near infrared CsPbI3:RE 3+ -PbS quantum dot heterojunction light absorption layer film, for PDs response test.
[0031] C. Preparation of efficient and stable quantum tailored fluorescence conversion films
[0032] For the preparation of quantum tailored fluorescence conversion film 1, it is still necessary to prepare efficient quantum tailored luminescent quantum dots. Yb 3+ Doped CsPbCl3 PQDs, the preparation of cesium oleate precursor is the same as the above experimental steps, add YbCl3 and PbCl2 reagents with a molar ratio of 1:1 to a solution of octadecene (15mL), oleic acid (1.5mL) and oleylamine (1.5mL), and react for 1h at 120 degrees Celsius under nitrogen conditions. Subsequently, the temperature is raised to 240 degrees Celsius and the cesium oleate precursor is injected. The reaction is rapidly cooled for 10s, and then the toluene solution is added for centrifugation to obtain efficient quantum tailored luminescent quantum dots. By controlling the reaction temperature and regulating the doping types and ratios of RECl3 and PbCl2, the quantum tailoring luminescence performance can be further improved. The prepared quantum tailored luminescent quantum dots are exchanged with the long-chain ligands on the surface of the quantum tailored luminescent quantum dots using short-chain ligands (e.g., ethanedithiol, mercaptopropionic acid, etc.) to prevent the agglomeration of the quantum tailored luminescent quantum dots during the film formation process; at the same time, organic polymers with high hydrophobicity and antioxidant properties are selected to modify the surface of the quantum tailored luminescent quantum dots to further improve the stability, thereby obtaining the quantum tailored fluorescent conversion film 1. Based on the above experiments, the quantum tailored fluorescent conversion film 1 is used as a light conversion layer by self-assembly method and prepared on the light-facing side of PDs, thereby improving the device's light detection performance from deep ultraviolet to ultraviolet.
[0033] D. Designing the Optimal Photodetector
[0034] The PDs device structure to be prepared in this application is as follows Figure 1 As shown, the prepared quantum tailored fluorescence conversion film 1 is coupled to the outer layer of the conductive glass 2 (FTO), and then the electron transport layer 3 and CsPbI3:RE are spin-coated on the upper layer of the conductive glass 2. 3+ -PbS quantum dot heterojunction 4, hole transport layer 5 and evaporated electrode layer 6. The preparation of each layer is very critical and determines the photoelectric response performance of PDs. In the selection of the electron transport layer 3, it is necessary not only to consider the electron migration rate, but also to study whether it matches the energy level of the light absorption layer; and for the selection of the hole transport layer 5, it is also necessary to take both the hole migration rate and the energy level position into consideration. 2,2",7,7"-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD) was selected as the material for the hole transport layer 5 for device preparation. At the same time, CsPbI3:RE 3+ -PbS quantum dot heterojunction 4 thickness can be regulated by changing the spin coating rate, time, number of times, etc. to select the best preparation conditions. 3+When the thickness of the PbS quantum dot heterojunction 4 is 120nm, 235nm, 420nm and 550nm, the detection performance of the visible light wavelength increases from 2.36×10 12 Jones increased to 5.05×10 12 Jones, 8.05 x 10 12 Jones and 1.05×10 13 Jones. Subsequently, CsPbI3:RE 3+ When the thickness of the PbS quantum dot heterojunction 4 reaches 640nm, the device performance begins to decline to 9.17×10 12 Jones. The above shows that CsPbI3:RE 3+ -The thickness of the PbS quantum dot heterojunction 4 has an important influence on the detection performance of the device. In addition, for the study of the quantum tailored fluorescence conversion film 1 on the light-facing side of FTO, it is also necessary to regulate the thickness of the quantum tailored fluorescence conversion film 1 so as not to affect the transmission of visible to near-infrared light. By testing the transmittance of the quantum tailored fluorescence conversion film 1, it was found that when the thickness of the quantum tailored fluorescence conversion film 1 is increased from 20nm to 55nm, 110nm and 180nm, its visible-infrared (400-1700nm) wavelength transmittance can maintain an intrinsic 98% or more. When the thickness of the quantum tailored fluorescence conversion film 1 is further increased to 260nm, its visible-infrared wavelength transmittance is reduced to 82.5%, which is not conducive to the device's detection response to visible-infrared wavelengths.
[0035] In order to study the detection performance of the deep ultraviolet-visible-near infrared (200nm-1700nm) broadband, the test light source needs to choose a UV-enhanced xenon lamp. The IV response curve, photocurrent and dark current of the device were tested, and the photoresponsivity and detection rate were calculated. The results showed that the detection rate of the photodetector in the ultraviolet (260nm) reached 3.19×10 12 Jones, visible (460nm) with a detection rate of 1.05×10 13 Jones, infrared (1550nm), its detection rate is 2.15×10 12 Jones, and the photoresponsivity of the device in the ultraviolet, visible and infrared wavelengths is 180.5 mA W respectively. -1 , 636.57mA W -1 and 124.3mA W -1; The external quantum efficiency of the photodetector was tested to determine the ability of the photodetector to absorb photons and convert them into electron-hole pairs. The results showed that the external quantum efficiency of the photodetector was 45.3% in the ultraviolet (260nm), 84.6% in the visible (460nm), and 7.2% in the infrared (1550nm); the light response time of PDs was studied to achieve fast light detection applications. The results showed that the photodetector achieved a rising edge response time of 82 microseconds and a falling edge response time of 83 microseconds; the external storage conditions of PDs were changed to explore the response performance under high humidity, high temperature and UV light conditions. The results showed that the photodetector can still maintain more than 89% of the initial response performance under 100-hour storage conditions, and can maintain 99.3% of the performance indicators after 10 hours of UV irradiation.
[0036] It should be noted that in the present invention, unless otherwise clearly specified and limited, the terms "slide", "rotate", "fix", "have" and the like should be understood in a broad sense, for example, it can be a welding connection, a bolt connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0037] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a photoelectric detector, characterized in that: The following steps are involved: Synthetic RE 3+ Doping CsPbI3 PQDs: Prepare cesium oleate precursor. Dissolve 0.375mM PbI2 and 0.375mM rare earth iodide in the reaction solution under nitrogen environment. The reaction solution is a mixture of 15mL octadecene, 1.5mL oleic acid and 1.5mL oleylamine. React at 110-130 degrees Celsius for 1h, then heat to 210-230 degrees Celsius and inject 1mL cesium oleate precursor. Cool and centrifuge to obtain RE 3+ Doped CsPbI3 PQDs; Preparation of CsPbI3:RE 3+ -PbS quantum dot heterojunction: synthesize PbS quantum dots and mix PbS quantum dots with RE at a mass ratio of 2:1 3 + Doped CsPbI3 PQDs were mixed, stirred for 20-26h in the dark, and centrifuged to obtain CsPbI3:RE 3+ -PbS quantum dot heterojunction; Preparation of quantum tailored fluorescence conversion film: prepare cesium oleate precursor, add YbCl3 and PbCl2 in a molar ratio of 1:1 to the reaction solution, the reaction solution is a mixture of 15mL octadecene, 1.5mL oleic acid and 1.5mL oleylamine, react for 1h in a nitrogen environment at 110-130 degrees Celsius, heat to 220-260 degrees Celsius and inject cesium oleate precursor, quickly cool after 10s, add toluene solution and centrifuge to obtain quantum tailored luminescent quantum dots, use short-chain ligands to exchange with long-chain ligands on the surface of quantum tailored luminescent quantum dots and use highly hydrophobic and antioxidant organic polymers to modify the quantum tailored luminescent quantum dots to obtain quantum tailored fluorescence conversion film; Preparation of photodetector: coupling quantum tailored fluorescence conversion film on the outer layer of conductive glass, and then setting electron transport layer, CsPbI3:RE on the upper layer of conductive glass 3+ -PbS quantum dot heterojunction, hole transport layer and electrode layer to obtain a photodetector.
2. The method for preparing a photoelectric detector according to claim 1, characterized in that: The steps of preparing the cesium oleate precursor are as follows: 0.8 g CsCO3 is dissolved in 25 mL octadecene and 1.5 mL oleic acid, and reacted for 2 hours in a nitrogen atmosphere at 100-130 degrees Celsius to completely dissolve the cesium oleate precursor.
3. The method for preparing a photoelectric detector according to claim 1 or 2, characterized in that: The iodide rare earth is at least one of CeI3, NdI3, ErI3, TmI3 and PrI3.
4. The method for preparing a photoelectric detector according to claim 1, characterized in that: The steps for synthesizing PbS quantum dots are as follows: 0.5 mM lead oxide is added to a mixture of oleic acid and octadecene, stirred for 1 hour under a nitrogen atmosphere at 130-160 degrees Celsius, and then 0.25 mM bis(trimethylsilyl) sulfide is added thereto. After reacting for 5 hours, the mixture is cooled to room temperature, and a toluene solution is added thereto and centrifuged to obtain PbS quantum dots.
5. The method for preparing a photodetector according to claim 1 or 4, characterized in that: The short-chain ligand is any one of ethanedithiol and mercaptopropionic acid.
6. The method for preparing a photoelectric detector according to claim 1, characterized in that: The electrode layer is a gold electrode layer.
7. The method for preparing a photodetector according to claim 1, characterized in that: The electron transport layer, CsPbI3:RE 3+ -PbS quantum dot heterojunction and hole transport layer are arranged on the conductive glass layer.