Bismuth ferrite ferroelectric memory based on flexible substrate and preparation method thereof

By growing a multi-layer stacked ferroelectric memory on a flexible substrate, the problem that traditional silicon-based ferroelectric memory is difficult to grow high-quality films on a flexible substrate is solved, and high-performance data storage and reading of flexible ferroelectric memory is realized It can be used in wearable devices and other fields.

CN118890957APending Publication Date: 2024-11-01GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921181.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional silicon-based ferroelectric memory is difficult to grow high-quality ferroelectric films on flexible substrates, limiting the application of inorganic perovskite ferroelectric materials in the field of flexible electronics.

Method used

Mica is used as the base material, SrTiO3 is used as the buffer layer, La0.65Sr0.35MnO3 is used as the bottom electrode, BiFeO3 is used as the ferroelectric functional oxide, and Pt is used as the upper electrode to form a multi-layer stack structure, and the film is grown through a pulsed laser deposition system, combined with in-situ Annealing and RF magnetron sputtering technology to prepare ferroelectric memory for flexible substrates.

Benefits of technology

It realizes the high-performance data storage and reading functions of flexible ferroelectric memory, has flexible performance, high dielectric constant and excellent electronic transmission performance, and is suitable for wearable devices and flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890957A_ABST
    Figure CN118890957A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of microelectronic storage, and discloses a bismuth ferrite ferroelectric memory based on a flexible substrate and a preparation method thereof, the bismuth ferrite ferroelectric memory based on the flexible substrate comprises a mica substrate layer, a SrTiO3 buffer layer, a La0. 65Sr0. 35MnO3 bottom electrode layer, a BiFeO3 ferroelectric functional oxide layer and a Pt upper electrode layer from bottom to top in sequence; the preparation method comprises the following steps: S1, removing impurities on the surface of mica, and waiting for film growth; s2, preparing a buffer layer; s3, preparing a bottom electrode layer; s4, performing in-situ annealing; s5 to S6, preparing a BiFeO3 ferroelectric functional oxide layer; s7, performing in-situ annealing; and S8, preparing a Pt upper electrode layer. According to the invention, mica is used as a substrate material, SrTiO3 is used as a buffer layer, La0. 65Sr0. 35MnO3 is used as a bottom electrode, BiFeO3 is used as a ferroelectric functional oxide, and Pt metal is used as an upper electrode, so that a multi-layer stacked structure is formed, and data reading and storage functions can be realized in a flexible device. The method is suitable for the fields of wearable equipment, flexible artificial synapses and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microelectronic memory, and in particular to a bismuth ferrite ferroelectric memory based on a flexible substrate and a preparation method thereof. Background Art

[0002] Ferroelectric RAM (FRAM) is a non-volatile memory technology that uses the special properties of ferroelectric materials to store and erase data. Ferroelectric materials have the property that a polarized electric field can flip the polarization direction, which allows them to maintain the storage state of data without power. The working principle of FRAM is similar to that of traditional dynamic random access memory (DRAM), but in comparison, in addition to the characteristics of high-density information storage and fast erasing, FRAM also has significant advantages such as low voltage, low cost, low loss, and small size, and has great industrialization potential.

[0003] In recent years, with the rapid development of Internet of Things technology and people's increasing attention to the quality of life, wearable electronic devices have attracted widespread attention. Electronic products such as sensors and displays are also increasingly inclined to be thinner and lighter. In order to meet the requirements of foldable electronic devices in the future, flexibility and ductility are the basic properties of such devices. However, in traditional silicon-based electronic devices, FRAM is usually prepared on a silicon substrate, and the thickness of silicon is as high as several hundred microns, which is generally considered to be inflexible.

[0004] Inorganic perovskite ferroelectric materials have many advantages over silicon-based materials, including higher ferroelectric polarization values ​​and excellent fatigue resistance. These characteristics make inorganic perovskite ferroelectric materials have potential advantages in information storage and data processing. However, due to the limitation of high-temperature growth conditions on flexible substrates, inorganic perovskite ferroelectric materials (such as BiFeO3 and BaTiO3) cannot be directly grown on flexible substrates to form high-quality ferroelectric films. This problem limits their application in the field of flexible electronics. Summary of the invention

[0005] The present invention is intended to provide a bismuth ferrite ferroelectric memory based on a flexible substrate and a preparation method thereof. The present invention uses mica as a base material, SrTiO3 as a buffer layer, La 0.65 Sr 0.35 MnO3 is used as the bottom electrode, BiFeO3 as the ferroelectric functional oxide, and Pt metal as the upper electrode to form a multilayer stack structure, so that the ferroelectric memory on the flexible substrate can achieve high-performance data storage and reading functions in flexible devices.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A bismuth ferrite ferroelectric memory based on a flexible substrate comprises, from bottom to top, a mica base layer, a buffer layer, a bottom electrode layer, a BiFeO3 ferroelectric functional oxide layer and a Pt top electrode layer.

[0008] Furthermore, the buffer layer is a SrTiO3 buffer layer, and the thickness of the SrTiO3 buffer layer is 50-80 nm.

[0009] Furthermore, the bottom electrode layer is La 0.65 Sr 0.35 MnO3 bottom electrode layer, La 0.65 Sr 0.35 The thickness of the MnO3 bottom electrode layer is 30 to 50 nm.

[0010] Furthermore, the thickness of the BiFeO3 ferroelectric functional oxide layer is 150-200 nm.

[0011] The above-mentioned method for preparing a bismuth ferrite ferroelectric memory based on a flexible substrate comprises the following steps:

[0012] S1. First, put the mica into acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes each, then blow dry the cleaned mica, put it into the pulsed laser deposition system PLD chamber, heat it up and wait for the film to grow;

[0013] S2. When the temperature in the PLD chamber rises to 600-900°C, 2-8 Pa of oxygen is introduced, and SrTiO3 is grown for 15-25 min at 1-5 Hz and 300-350 mJ to prepare a SrTiO3 buffer layer;

[0014] S3, raise the oxygen to 20-50Pa, use 3-5Hz, 300-350mJ to grow La for 25-50min 0.65 Sr 0.35 MnO3, prepared La 0.65 Sr 0.35 MnO3 bottom electrode layer;

[0015] S4, annealing the film in situ at 600-900°C and 10-30Pa for 10-30min, then cooling the film to 250-300°C at a rate of 5-9°C / min, and taking it out;

[0016] S5. Cover part La 0.65 Sr 0.35 The MnO3 bottom electrode layer is sent into the PLD chamber again;

[0017] S6, at 600-900° C., introduce 5-15 Pa of oxygen, use 2-5 Hz, 150-400 mJ to grow BiFeO3 for 20-60 min, and obtain a BiFeO3 ferroelectric functional oxide layer;

[0018] S7, annealing in situ again at 600-900°C, 5-15Pa for 10-30min, then cooling to 250-300°C at a rate of 2-8°C / min, and taking it out;

[0019] S8. Grow a Pt upper electrode layer using a lift-off process and radio frequency magnetron sputtering.

[0020] Further, in S8, the thickness of the Pt upper electrode layer is 50-100 nm, and the surface size is 50 um*50 um-100 um*100 um.

[0021] The beneficial effects of the technical solution are:

[0022] 1. The ferroelectric memory based on a flexible substrate provided by the present invention has the advantages of flexibility, high dielectric constant and excellent electronic transmission performance, including:

[0023] (1) Due to the use of a flexible substrate layer, the memory can adapt to deformations such as bending and folding, and has good flexibility, which facilitates its application in wearable devices, flexible artificial synapses and other fields.

[0024] (2) The BiFeO3 ferroelectric functional oxide layer it includes has a higher dielectric constant and a larger spontaneous polarization value, and can provide a larger capacitance storage capacity.

[0025] (3) The SrTiO3 buffer layer has good lattice matching with the upper epitaxial film, which provides a guarantee for high-quality epitaxy of the BiFeO3 ferroelectric functional layer, and is beneficial to improving the stability and reliability of the memory.

[0026] (4)La 0.65 Sr 0.35 The MnO3 bottom electrode layer as the bottom electrode layer can reduce oxygen vacancies at the interface with the BiFeO3 ferroelectric functional oxide layer, which helps to improve the performance and reliability of the device.

[0027] In summary, the ferroelectric memory based on a flexible substrate provided by the present invention has good flexibility, high dielectric constant and excellent electronic transmission performance, is suitable for flexible electronic devices, and has potential application prospects.

[0028] 2. The preparation method of the ferroelectric memory based on the flexible substrate provided by the present invention has a simple overall concept and is easy to operate. The ferroelectric memory can be prepared by growing different material layers layer by layer, which specifically includes:

[0029] (1) Implementing the growth steps of each layer in the PLD chamber enables precise material growth and control;

[0030] (2) In-situ annealing can improve the crystallinity and stability of the film;

[0031] (3) Using the growth of different material layers, the memory structure can be constructed;

[0032] (4) The upper electrode layer is grown using a lift-off process and radio frequency magnetron sputtering to complete the final step of memory preparation.

[0033] In summary, the method provided by the present invention can not only realize the preparation of ferroelectric memory based on flexible substrate, but also has good control performance and repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the XRD diagram of the BFO / LSMO / STO / Mica structure in the embodiment of the present invention;

[0035] Figure 2 This is an AFM morphology image of a BFO film in an embodiment of the present invention;

[0036] Figure 3 PV test diagram of the Pt / BFO / LSMO / STO / Mica structure at different voltages in an embodiment of the present invention;

[0037] Figure 4 This is a combined curve of polarization reversal current and hysteresis loop of BFO / LSMO / STO / Mica structure in a specific embodiment of the present invention;

[0038] Figure 5 This is an IV test diagram of the Pt / BFO / LSMO / STO / Mica structure in an embodiment of the present invention;

[0039] Figure 6 and Figure 7 This is a fatigue test diagram of the Pt / BFO / LSMO / STO / Mica structure at a fatigue frequency of 100kHz in an embodiment of the present invention;

[0040] Figure 8 This is a test diagram of the holding force of the Pt / BFO / LSMO / STO / Mica structure under a 2V bias in an embodiment of the present invention;

[0041] Fig. 9 This is a PFM test diagram of the Pt / BFO / LSMO / STO / Mica structure in an embodiment of the present invention;

[0042] Fig.10 This is an amplitude-phase diagram of the BFO / LSMO / STO / Mica structure in an embodiment of the present invention. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:

[0044] The method for preparing a ferroelectric memory based on a flexible substrate comprises the following steps:

[0045] S1. Use acetone, ethanol and deionized water to ultrasonically clean the impurities on the surface of mica for 5 minutes, then use a high-pressure nitrogen gun to blow dry the mica; finally, put the cleaned and dried mica into the pulsed laser deposition system (PLD) chamber, heat it up and wait for the film to grow;

[0046] S2, wait for the PLD temperature to reach 750°C, introduce 5Pa of oxygen, use 3Hz, 300mJ to grow SrTiO3 for 20min, with a thickness of 60nm;

[0047] S3, at 750 ° C, increase the oxygen pressure to 30Pa, use 3Hz, 300mJ to grow La for 40min 0.65 Sr 0.35 MnO3, thickness 45nm;

[0048] S4, annealing the film in situ at 750°C and 20Pa for 20min, then cooling it to 280°C at a rate of 8°C / min and taking it out;

[0049] S5. Cover part La 0.65 Sr 0.35 MnO3, and then sent into the PLD chamber again;

[0050] S6, at 650 ° C, oxygen pressure of 10Pa, using 3Hz, 300mJ to grow BiFeO3 for 60min, with a thickness of 150nm;

[0051] S7, perform in-situ annealing again, perform in-situ annealing at 650°C and 20Pa for 30min, then cool down to 350°C at a rate of 7°C / min and take it out;

[0052] S8. Use lift-off process and RF magnetron sputtering to grow 60nm 70um*70um Pt top electrode.

[0053] Finally, a ferroelectric memory with a flexible substrate is obtained, which includes a mica base layer, a SrTiO3 buffer layer, a La 0.65 Sr 0.35MnO3 bottom electrode layer, BiFeO3 ferroelectric functional oxide layer and Pt top electrode layer; the thickness of SrTiO3 buffer layer is 60nm, La 0.65 Sr 0.35 The thickness of the MnO3 bottom electrode layer is 45 nm, and the thickness of the BiFeO3 ferroelectric functional oxide layer is 150 nm.

[0054] Experimental analysis:

[0055] In order to explore the components of the device, the BFO / LSMO / STO / Mica structure was scanned at 2θ using an X-ray diffractometer. Figure 1 As shown: the (111) diffraction peak of the BFO film is found at 39.113°; the (111) diffraction peak of the STO film is found at 39.981°; and the (022) diffraction peak of the LSMO is found at 40.366°. Since the lattice constant of BFO is Its lattice constant is larger than that of STO Therefore, it is located on the left side of the STO diffraction peak, and the lattice constant of LSMO is The lattice constant is smaller than that of STO, and its diffraction peak is located to the right of the STO diffraction peak. Figure 1 In the experiment, only the (111) related diffraction peak was observed. Except for the substrate peak, no other film related diffraction peaks were seen. Therefore, the results show that by growing a buffer layer LSMO / STO on a flexible mica substrate, a bismuth ferrite BFO ferroelectric film with high-quality epitaxial (111) crystal phase was successfully obtained on the mica of the flexible substrate.

[0056] The surface morphology and roughness of the BFO film were measured using a scanning probe microscope. Figure 2 The surface morphology of BFO / LSMO / STO / Mica (area 10*10um 2 ), it can be seen that the root mean square roughness (RMS) of the BFO film is 12.6nm.

[0057] In order to verify the ferroelectricity of BFO film, a Pt top electrode was added to the BFO / LSMO / STO / Mica structure. Figure 3 As shown, the electrical properties of the Pt / BFO / LSMO / STO / Mica structure were tested by using a ferroelectric analyzer. Figure 3The PV hysteresis loop of the Pt / BFO / LSMO / STO / Mica structure at different voltages under a 1000Hz triangular wave frequency is shown. When the test voltage is 21V, the PV hysteresis loop begins to appear. As the test voltage increases, the shape of the BFO hysteresis loop gradually becomes clearer. At 21V, the BFO hysteresis loop is not closed. This is because the coercive field of BFO is large and the test voltage does not reach its coercive field voltage. When the voltage is applied to 25V, the residual polarization value of the BFO ferroelectric film reaches 67.386μC / cm 2 , the saturation polarization value reaches 68.094μC / cm 2 The larger polarization intensity originates from the high-quality growth of the flexible BFO ferroelectric film on LSMO / STO.

[0058] Figure 4 The hysteresis loop and transient current curve of the film are shown. It can be seen that the residual polarization intensity of the film is as high as 66.654μC / cm2 and the saturation polarization value is 67.971μC / cm2. The coercive field (Ec+) is 16.18V and the coercive field (Ec-) is -15.57V. The main reason for the two obvious peaks near the coercive field is that when the forward voltage is applied, the polarization reverses rapidly, and the polarization reversal current gradually increases. At the coercive field (Ec+), the polarization reversal current reaches the maximum, forming the first current peak. As the voltage continues to increase, the polarization intensity gradually saturates, and the polarization current decreases accordingly. When the applied voltage decreases, since there is no polarization reversal in the process, the polarization current approaches 0. When the reverse voltage is applied, the polarization reverses rapidly, and at the coercive field (Ec-), the polarization reversal current reaches the maximum, causing the current peak to appear again, forming a double peak. The existence of the current double peak further verifies the ferroelectricity of the BFO film.

[0059] The IV curve was tested by using Keithley 2400digital source meter. Figure 5 As shown in Figure 2, the Pt / BFO / LSMO / STO / Mica structure still maintains a 10 -8 A level, the use of LSMO oxide bottom electrode reduces the oxygen vacancies at the interface between the ferroelectric film and the bottom electrode, reduces the generation of leakage current, and is more conducive to improving the reliability of the device.

[0060] The polarization flip in ferroelectric memory is represented as "0" and "1" in digital logic, so the repeated reading and writing of data requires stronger ability. Therefore, we conducted fatigue tests on Pt / BFO / LSMO / STO / Mica ferroelectric memory. The change of residual polarization value with the number of flips is shown in the figure below. Figure 6 and Figure 7 As shown. The initial residual polarization value Pr after 1012 After the first cycle, the temperature dropped from 68.121uC / cm 2 becomes 67.709uC / cm 2 , decreased by 0.323uC / cm 2 , the saturation polarization value Ps after 10 10 After the first cycle, the temperature dropped from 69.448uC / cm 2 becomes 67.728uC / cm 2 , decreased by 1.72uC / cm 2 . The fluctuation of the coercive field is caused by the transport process of charges in the ferroelectric film being affected by the fatigue test. Under the long-term application of the electric field, the charges may accumulate or diffuse in the film, resulting in changes in the coercive field. The results show that the Pt / BFO / LSMO / STO / Mica ferroelectric memory we prepared has excellent fatigue resistance. The flexible substrate also makes it possible to be used in smart wearable scenarios.

[0061] The retention test of ferroelectric thin films is a test method to evaluate whether ferroelectric materials can maintain their ferroelectric properties after a long period of applied electric field. In the test, the ferroelectric film is usually first subjected to a period of polarization process, and then the electric field is removed to observe whether the film can maintain its polarization state. Figure 8 This is the retention test diagram of Pt / BFO / LSMO / STO / Mica ferroelectric memory. After 3550s of waiting, the initial residual polarization value Pr is reduced from 67.845uC / cm 2 Increased to 69.044uC / cm 2 This shows that the Pt / BFO / LSMO / STO / Mica ferroelectric memory we prepared has good stability and application reliability.

[0062] Piezoelectric Force Microscope (PFM) is the most intuitive means to measure the ferroelectricity of ferroelectric films. Fig. 9 This is the PFM phase diagram of the Pt / BFO / LSMO / STO / Mica structure. First, we used a probe at 6×6um 2 Apply +30V voltage to the square area, and then apply +30V voltage to the middle 2×2um 2 A voltage of -30V is applied to the square area, and then a small voltage of 1V is used to read the 10×10um 2 The light and dark contrast in the PFM image corresponds to two different polarization directions of ferroelectricity, indicating that the ferroelectric domains of the BFO film are reversible, further confirming the ferroelectricity of the BFO film.

[0063] Fig.10This is the amplitude-phase diagram of the BFO / LSMO / STO / Mica structure. It can be seen that the phase curve presents a phase difference of 180 degrees and the amplitude curve presents a butterfly shape, indicating that the BFO film we prepared has good ferroelectric properties.

[0064] In summary, the bismuth ferrite ferroelectric memory based on a flexible substrate provided by the present invention has the advantages of flexibility, high dielectric constant and excellent electronic transmission performance.

[0065] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the technical solution of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A bismuth ferrite ferroelectric memory based on a flexible substrate, characterized in that: The ferroelectric memory comprises, from bottom to top, a mica substrate layer, a buffer layer, a bottom electrode layer, a BiFeO3 ferroelectric functional oxide layer and a Pt top electrode layer.

2. The bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 1, characterized in that: The buffer layer is a SrTiO3 buffer layer.

3. The bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 1, characterized in that: The bottom electrode layer is La 0.65 Sr 0.35 MnO3 bottom electrode layer.

4. The bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 2, characterized in that: The thickness of the SrTiO3 buffer layer is 50-80 nm.

5. The bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 3, characterized in that: The La 0.65 Sr 0.35 The thickness of the MnO3 bottom electrode layer is 30 to 50 nm.

6. The bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 1, characterized in that: The thickness of the BiFeO3 ferroelectric functional oxide layer is 150-200 nm.

7. A method for preparing a bismuth ferrite ferroelectric memory based on a flexible substrate according to any one of claims 1 to 6, comprising the following steps: S1. First, wash the impurities on the surface of the mica, then blow dry the washed mica, put the dried mica into the PLD chamber of the pulsed laser deposition system, heat it up and wait for the film to grow; S2. When the temperature in the PLD chamber rises to 600-900°C, 2-8 Pa of oxygen is introduced, and SrTiO3 is grown for 15-25 min at 1-5 Hz and 300-350 mJ to prepare a SrTiO3 buffer layer; S3, raise the oxygen to 20-50Pa, use 3-5Hz, 300-350mJ to grow La for 25-50min 0.65 Sr 0.35 MnO3, prepared La 0.65 Sr 0.35 MnO3 bottom electrode layer; S4, annealing the film in situ at 600-900°C and 10-30Pa for 10-30min, then cooling the film to 250-300°C at a rate of 5-9°C / min, and taking it out; S5. Cover part La 0.65 Sr 0.35 The MnO3 bottom electrode layer is sent into the PLD chamber again; S6, at 600-900° C., introduce 5-15 Pa of oxygen, use 2-8 Hz, 150-400 mJ to grow BiFeO3 for 20-60 min, and obtain a BiFeO3 ferroelectric functional oxide layer; S7, annealing in situ at 600-900°C, 5-15Pa for 10-30min, then cooling to 250-300°C at a rate of 2-8°C / min, and taking it out; S8. Grow a Pt upper electrode layer using a lift-off process and radio frequency magnetron sputtering.

8. The method for preparing a bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 7, characterized in that: In step S1, acetone, ethanol and deionized water are used to ultrasonically clean the mica for 5 minutes in sequence to clean impurities on its surface.

9. The method for preparing a bismuth ferrite ferroelectric memory based on a flexible substrate according to claim 7, characterized in that: In step S8, the thickness of the Pt upper electrode layer is 50-100 nm, and the surface size is 50 um*50 um-100 um*100 um.