Oxide-containing plate-shaped copper particles, paste composition, semiconductor device, electrical component, and electronic component
By using plate-shaped copper particles composed of Cu, Cu2O and Cu64O, the Cu64O content and sintering conditions are controlled, and the problem of low bonding layer density in the prior art is solved, and a paste composition with high bonding strength and reliability is achieved. Thermal conduction and stability of semiconductors and electronic components are improved.
Patent Information
- Application Number
- CN202380026665.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-19
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-01
AI Technical Summary
The existing paste compositions containing copper oxide particles are prone to hollows during sintering and bonding, and have low density, resulting in insufficient bonding strength and reliability.
The plate-shaped copper particles composed of Cu, Cu2O and Cu64O are used to control the Cu64O content in the range of 2.1% to 25.0%, combined with X-ray diffraction and scanning electron microscopy technology, ensure the sintering and bonding properties of copper particles, and use stable shape The agent and the reducing compound are subjected to a reduction treatment to form a bonding layer with high density and high bonding strength.
The bonding layer with high density, high bonding strength and high bonding reliability is achieved, which improves the thermal conductivity and stability of semiconductor devices and electronic components, and reduces the thermal resistance change rate.
Smart Images

Figure BDA0005035998480000131 
Figure HDA0005035998490000011 
Figure HDA0005035998490000012
Abstract
Description
Technical Field
[0001] The present invention relates to plate-like copper particles containing oxides, a paste composition using the plate-like copper particles containing oxides, and a semiconductor device, an electric component, and an electronic component. Background Art
[0002] In semiconductor devices, various electric components, and electronic components, highly thermally conductive pastes are used as adhesives for bonding the components.
[0003] For semiconductor devices, the heat generation increases with high integration and high-speed operation. In order to obtain stable operation, for example, a countermeasure is adopted, such as using a high thermal conductivity adhesive (paste) to bond heat-generating components such as semiconductor elements to heat-dissipating components to diffuse the heat. In addition, a high thermal conductivity conductive paste is used for bonding bare chips, bonding LED chips, or bonding electrodes and wires.
[0004] As one of the conductive pastes with high thermal conductivity, a paste composition containing copper particles has been proposed. Application of such a paste composition to printed electronics has also been studied. For example, Patent Documents 1 and 2 disclose that oxide-containing copper particles obtained by sintering a copper raw material at a low temperature are used as a constituent material of a conductive paste.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent document 1: Japanese Patent Application Publication No. 2020-29392.
[0008] Patent document 2: International Publication No. 2022 / 045252. Summary of the invention
[0009] The present invention relates to the following contents.
[0010] [1] A plate-like copper particle containing copper oxide, wherein the plate-like copper particle contains Cu, Cu 2 O and Cu 64 O, relative to Cu, Cu 2 O and Cu 64 Total O 100 mass%, Cu 64 The content of O is 2.1 mass % to 25.0 mass %. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is an image of the plate-like copper particles containing oxide in Example 4 observed by a scanning electron microscope.
[0012] Figure 2 This is an image of the oxide-containing copper particles of Comparative Example 2 observed by a scanning electron microscope. DETAILED DESCRIPTION
[0013] Conductive pastes using copper oxide particles as described in Patent Documents 1 and 2 are substantially spherical particles. Therefore, during sintering and bonding, voids are generated in the bonding layer, resulting in low density, and it is difficult to obtain sufficient bonding strength, which may reduce bonding reliability.
[0014] The present invention provides oxide-containing copper particles, a paste composition using the oxide-containing copper particles, and a semiconductor device, an electric component, and an electronic component. The oxide-containing copper particles can provide a paste composition capable of forming a bonding layer with high density, high bonding strength, and high bonding reliability.
[0015] Hereinafter, the present invention will be described in detail with reference to one embodiment.
[0016] The plate-like copper particles containing oxides in the present invention are particles containing metallic copper and at least one type of copper oxide and having a plate-like particle shape. Hereinafter, they are also simply referred to as copper particles.
[0017] In this specification, the description of "XX to YY" means "more than XX and less than YY". In addition, in this specification, regarding the numerical range (for example, the range of content, etc.), the lower limit and upper limit described in stages can be independently combined. In addition, in the numerical range described in this specification, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.
[0018] [Plate-like copper particles containing oxide]
[0019] The plate-like copper particles containing oxides of the present invention contain Cu, Cu 2 O and Cu 64 O, relative to Cu, Cu 2 O and Cu 64 Total O 100 mass%, Cu 64 The content of O is 2.1 to 25.0 mass %.
[0020] The copper particles of the present invention contain Cu and Cu as copper oxide. 2 O and Cu 64 O, good sintering and reducibility. In addition, the Cu 64 When the content of O is within the above range, a paste composition capable of forming a bonding layer having high density, high bonding strength, and high bonding reliability can be obtained.
[0021] With CuO and Cu 2 Compared with CuO, 64 O has a low ratio of oxygen atoms and low phase stability. 64The high content of O makes it easy to self-oxidize and decompose during sintering, making it difficult to be reduced. On the other hand, heating makes the Cu 64 The copper atoms of O can easily move or diffuse, which promotes sintering.
[0022] If Cu 64 When the content of O is 2.1 mass % or more, the Cu 64 The movement or diffusion of copper atoms in O facilitates sintering. 64 The content of O is 25.0 mass % or less, Cu 64 O is sufficiently reduced, and copper particles with good sinterability can be obtained.
[0023] Cu 64 The content of O may be 2.5 to 25.0 mass %, or 3.0 to 20.0 mass %.
[0024] The copper particles include Cu 2 O, from the viewpoint of good sintering property of copper particles, is relatively 2 O and Cu 64 The content of O may be 5.0 mass % or less, 0.1 to 4.5 mass %, or 1.0 to 4.0 mass %, based on 100 mass % of the total amount of O.
[0025] Relative to Cu and Cu in copper particles 64 O and Cu 2 Total O 100 mass%, Cu 64 O and Cu 2 The contents of O were determined from the X-ray diffraction (XRD) pattern by the reference intensity ratio (RIR) method. The XRD pattern was obtained by irradiating characteristic X-rays of CuKα rays (wavelength 0.15418 nm) and performing XRD measurement. Specifically, it was measured by the method described in the examples. In the XRD pattern, the strongest lines of each component (Cu(111), Cu 64 O(044) and Cu 2 O(111)), the integrated intensity obtained by subtracting the background intensity and each RIR value (Cu: 8.86; Cu 64 O: 4.89; Cu 2 O: 8.28) can be calculated. It should be noted that the diffraction angle 2θ of each peak is 43.298° for Cu(111) and 8.28° for Cu(111). 64 O(044) is 40.710°, Cu 2 O(111) is 36.419°.
[0026] When the copper particles are heated at 200° C. in a nitrogen environment, the ratio (C2 / C1) of the crystallite diameter (crystallite diameter) (C2) of the Cu (111) after heating to the crystallite diameter (C1) of the Cu (111) before heating can be 2.0 or more. That is, from the viewpoints of sinterability, density, and bonding strength, the ratio C2 / C1 of the crystallite diameter of the Cu (111) before and after heating at 200° C. in a nitrogen environment can be 2.0 or more, can be 3.0 to 10.0, or can be 4.0 to 8.0.
[0027] From a practical point of view, heating at 200° C. in a nitrogen atmosphere is a heating condition that takes into account the environment and temperature when a paste composition of copper particles is used as a bonding material and bonding is performed by sintering of the copper particles.
[0028] From the viewpoint of sinterability, density, and bonding strength, the crystallite diameter (C2) may be 55.0 nm or more, 57.0 to 80.0 nm, or 58.0 to 75.0 nm.
[0029] From the viewpoint of sinterability, density, and bonding strength, the crystallite diameter (C1) may be 5.0 to 30.0 nm, 7.0 to 25.0 nm, or 8.0 to 20.0 nm.
[0030] The crystallite diameter of Cu(111) of the copper particles is determined from the XRD pattern. Specifically, the crystallite diameter is determined by the method described in Examples.
[0031] The copper particles are plate-shaped particles.
[0032] The copper particles may have a thickness of 5 to 50 nm, 8 to 40 nm, or 10 to 30 nm.
[0033] The major diameter of the copper particles may be 30 to 300 nm, 50 to 200 nm, or 75 to 150 nm, and the major diameter may be greater than the thickness.
[0034] The aspect ratio (aspect ratio, long diameter / thickness) of the copper particles may be 1.5 to 10.0, 2.0 to 9.0, or 3.0 to 8.0.
[0035] Since the copper particles are plate-shaped particles as described above, the contact area between the particles is larger than that of spherical particles. It is estimated that the density of the bonding layer formed by the paste composition using the plate-shaped particles is increased, the bonding strength is increased, and the bonding reliability is likely to be increased.
[0036] The thickness and major diameter of the copper particles are respectively the median of the measured length values of at least 200 particles extracted from an image taken during observation under a scanning electron microscope (SEM). Specifically, the thickness and major diameter of the copper particles can be measured by the method described in the embodiment. It should be noted that the plate-like particles are in the shape of a pair of roughly parallel planes, and the distance between the pair of planes is taken as "thickness", and the longest diameter in the plane is taken as "major diameter".
[0037] The copper particles are usually sintered by heating to 100 to 250° C. in an inert gas environment.
[0038] Examples of the inert gas include nitrogen, argon, and helium. From the viewpoint of availability and price, nitrogen may be used.
[0039] From the viewpoint of good sinterability, the heating temperature may be 120 to 230°C, or 150 to 200°C.
[0040] Sintering can be carried out under normal pressure or under pressure.
[0041] The heating time is appropriately set depending on the heating temperature, the form of the sintered body, etc. From the viewpoint of sufficient sintering, the heating time may be, for example, 5 to 180 minutes, 10 to 120 minutes, or 30 to 90 minutes.
[0042] [Method for producing plate-like copper particles containing oxide]
[0043] The method for producing the plate-like copper particles containing oxides of the present invention is not particularly limited. For example, a method of reducing a copper compound using a reducing compound in the presence of a shape stabilizer can be mentioned. The copper compound, the shape stabilizer and the reducing compound can be mixed in an organic solvent.
[0044] (Copper compounds)
[0045] Examples of the copper compound include copper oxide, copper hydroxide, copper nitride, and copper carboxylate. From the perspective of obtaining the copper particles of the present invention at a high yield, the copper compound may be copper oxide. The copper compound may be used alone or in combination of two or more.
[0046] Examples of copper oxide include copper (I) oxide (cuprous oxide: Cu 2 O), copper (II) oxide (CuO). From the viewpoint of productivity, copper (I) oxide may be used.
[0047] Examples of copper hydroxide include copper (II) hydroxide and copper (I) hydroxide.
[0048] Examples of copper nitride include copper (II) nitride and copper (I) nitride.
[0049] As copper carboxylates, for example, copper formate (I), copper acetate (I), copper propionate (I), copper butyrate (I), copper valerate (I), copper hexanoate (I), copper octanoate (I), copper decanoate (I), etc. can be cited. In addition, copper carboxylates anhydrates or hydrates such as copper formate (II), copper acetate (II), copper propionate (II), copper butyrate (II), copper valerate (II), copper hexanoate (II), copper octanoate (II), copper decanoate (II), and copper citrate (II) can also be cited. Commercially available copper carboxylates can be used. Materials synthesized by known methods can also be used. As copper carboxylates, copper acetate (II) monohydrate can also be used from the viewpoint of ease of acquisition and the manufacturing efficiency of the copper particles of the present invention.
[0050] (Shape stabilizer)
[0051] The shape stabilizer may be, for example, at least one selected from the group consisting of an amine compound, a carboxylic acid, and a phosphoric acid ester, or may be a combination of an amine compound and a carboxylic acid.
[0052] The shape stabilizer covers at least a portion of the oxide-containing copper of the copper particles of the present invention, thereby making it easier to obtain the predetermined light absorption characteristics of the present invention. In addition, the fluidity of the paste composition using the copper particles is improved.
[0053] Examples of the amine compound include dipropylamine, butylamine, dibutylamine, hexylamine, cyclohexylamine, heptylamine, octylamine, nonylamine, decylamine, 3-aminopropyltriethoxysilane, dodecylamine, oleylamine, monoethanolamine, 2-aminoethoxy-2-ethanol, 3-amino-1-propanol, 3-amino-2-propanol, 4-amino-1-butanol, 3-amino-1-hexanol, and 2-(2-aminoethoxy)ethanol; and monoamines such as ethylenediamine, N,N-dimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-diethylethylenediamine, and the like. The amine compound may be a diamine such as diamine, N,N'-diethylethylenediamine, 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, N,N-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N-diethyl-1,3-diaminopropane, 1,4-diaminobutane, 1,5-diamino-2-methylpentane, 1,6-diaminohexane, N,N'-dimethyl-1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane. The amine compound may be used alone or in combination of two or more. The amine compound may be an amino alcohol, and the molecular weight of the amino alcohol may be 80 or more or 150 or less.
[0054] As carboxylic acids, for example, monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, heptanoic acid, octanoic acid, octylic acid, nonanoic acid, capric acid, oleic acid, stearic acid, and isostearic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and diglycolic acid can be mentioned. The carboxylic acid can be an aromatic carboxylic acid such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, and gallic acid, or a hydroxy acid such as glycolic acid, lactic acid, tartronic acid, malic acid, glyceric acid, hydroxybutyric acid, tartaric acid, citric acid, and isocitric acid. The carboxylic acid can be used alone or in combination of two or more. The carboxylic acid can also be a monocarboxylic acid. The molecular weight of the monocarboxylic acid can be 80 or more, or 150 or less.
[0055] Phosphate ester can remove the oxide film on the surface of copper particles generated by heating in the air, and can improve the sintering property of copper particles. In addition, phosphoric acid ester can improve the lubricity of copper particles in the paste composition. Phosphate ester can also be added after the reduction reaction.
[0056] Examples of the phosphoric acid ester include alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkylphenyl ether phosphates. The acid value and amine value of the phosphoric acid ester may be 130 mgKOH / g or less, 120 mgKOH / g or less, or 110 mgKOH / g or less. The ratio of the acid value to the amine value (acid value / amine value) may be 0 to 1.5, or 0 to 1.2.
[0057] In addition, the acid value is calculated|required by the method based on JISK0070:1992, and the amine value is calculated|required by the method based on JISK7237:1995.
[0058] The total amount of the shape stabilizer used may be 0.1 to 10 mol, 0.5 to 8 mol, or 1 to 5 mol, relative to 1 mol of the copper compound.
[0059] When an amine compound and a carboxylic acid are used as the shape stabilizer, for example, the molar ratio of the amine compound to the carboxylic acid may be 1 / 5 to 5 / 1, 1 / 3 to 3 / 1, or 1 / 2 to 2 / 1.
[0060] (Reducing compound)
[0061] The reducing compound is not particularly limited as long as it has a reducing ability to reduce the copper compound and release metallic copper. Examples of the reducing compound include hydrazine derivatives. The reducing compound may be used alone or in combination of two or more.
[0062] Examples of the hydrazine derivative include hydrazine monohydrate, methylhydrazine, ethylhydrazine, n-propylhydrazine, isopropylhydrazine, n-butylhydrazine, isobutylhydrazine, sec-butylhydrazine, tert-butylhydrazine, n-pentylhydrazine, isopentylhydrazine, neopentylhydrazine, tert-pentylhydrazine, n-hexylhydrazine, isohexylhydrazine, n-heptylhydrazine, n-octylhydrazine, n-nonylhydrazine, n-decylhydrazine, n-undecylhydrazine, n-dodecylhydrazine, cyclohexylhydrazine, phenylhydrazine, 4-methylphenylhydrazine, benzylhydrazine, 2-phenylethylhydrazine, 2-hydrazinylethanol, and acetohydrazine.
[0063] The amount of the reducing compound used may be 0.1 to 10 mol, 0.5 to 5 mol, or 0.8 to 3 mol, relative to 1 mol of the copper compound.
[0064] (Organic Solvent)
[0065] The organic solvent is not particularly limited as long as it allows a uniform reaction without inhibiting the complex generated by mixing the copper compound, the shape stabilizer, and the reducing compound. The organic solvent may be a substance that is compatible with the reducing compound.
[0066] Examples of the organic solvent include alcohols such as 1-propanol, 2-propanol, butanol, pentanol, hexanol, heptanol, octanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, butyl cellosolve, ethyl carbitol, and butyl carbitol; butyl carbitol acetate, ethyl carbitol acetate, and diethylene glycol diethyl ether. The organic solvent may be used alone or in combination of two or more.
[0067] When an organic solvent is used, the amount used may be any amount as long as the copper compound, shape stabilizer and reducing compound can be uniformly mixed. For example, the amount used of the organic solvent may be 0.1 to 500 times by volume relative to the volume of the shape stabilizer.
[0068] From the perspective of sufficient reaction, the reduction reaction of the copper compound may be heated. The reaction temperature may be -20 to 140°C, 25 to 120°C, or 40 to 100°C. From the perspective of sufficient reaction, the reaction time may be 20 to 360 minutes, 30 to 300 minutes, or 40 to 240 minutes.
[0069] When the content of the container subjected to the reduction reaction is a liquid (mixed liquid), the solid matter may be separated by centrifugation, etc. The obtained solid matter may be washed with an organic solvent, and further, may be obtained as a copper particle cake by centrifugation, etc.
[0070] The washing method is not particularly limited as long as the shape stabilizer, reducing compound, etc. can be sufficiently removed.
[0071] The organic solvent for washing may be an alcohol. Examples of the alcohol include ethanol, 1-propanol, 2-propanol, butanol, pentanol, hexanol, heptanol, octanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, diethylene glycol, butyl cellosolve, ethyl carbitol, butyl carbitol, etc. The organic solvent for washing may be used alone or in combination of two or more.
[0072] [Ointment composition]
[0073] The paste composition of the present invention contains the above-mentioned plate-like copper particles containing the oxide of the present invention.
[0074] The content of the copper particles in the paste composition may be 10 to 95% by mass, 20 to 90% by mass, or 30 to 85% by mass.
[0075] In addition, in this invention, the component except the organic solvent in a paste composition, that is, a non-volatile component is regarded as the content of copper particles.
[0076] From the viewpoint of workability and viscosity during use, the paste composition may be diluted with an organic solvent.
[0077] As the organic solvent, from the viewpoint of the dispersibility of the copper particles and the volatility during the sintering of the paste composition, for example, 1-propanol, 2-propanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butylene glycol, 3-methyl-1,5-pentanediol, glycerol, polyethylene glycol, etc. can be cited. The organic solvent can be used alone or in combination of two or more. The organic solvent for dilution can be the same as the organic solvent for washing the copper particles.
[0078] The paste composition of the present invention contains copper particles, an organic solvent, and components derived from the production of the copper particles, and may appropriately contain known additives that are generally used in conductive pastes, as necessary.
[0079] Examples of additives include thermosetting resins, curing accelerators, stress reducing agents such as rubber and silicone, coupling agents, defoaming agents, surfactants, colorants such as pigments and dyes, polymerization inhibitors, antioxidants, etc. The additives may be used alone or in combination of two or more.
[0080] For example, the paste composition of the present invention can be prepared by kneading and degassing a mixture of copper particles, an organic solvent, and additives used as required using a kneading machine such as a disperser, a kneader, a three-roll mill, or a planetary mixer.
[0081] The cured product of the paste composition of the present invention includes a sintered body of the copper particles of the present invention, has high thermal conductivity, and has high heat dissipation. Therefore, when the paste composition of the present invention is used as a bonding material such as a substrate of an element or a heat dissipation component, the thermal conductivity of the device is improved, or the diffusivity of the heat inside the device to the outside is improved. Therefore, by using the paste composition of the present invention, the operation of various products such as semiconductor devices, electrical components, and electronic components can be stabilized.
[0082] [Semiconductor devices]
[0083] At least a portion of the semiconductor device of the present invention is bonded using the paste composition of the present invention. As a semiconductor device, for example, a device in which a semiconductor element and a substrate as an element support member are bonded using the paste composition can be cited. The paste composition can also be used as a chip adhesive.
[0084] By using the paste composition of the present invention for bonding, a bonding layer with high density and high bonding strength is formed. Even if the bonding layer is subjected to repeated temperature changes, the change rate of thermal resistance is low and the bonding reliability is high, so a semiconductor device with stable operation can be obtained.
[0085] The semiconductor element may be a known semiconductor element, for example, a transistor, a diode, etc., and also a wide bandgap semiconductor element using SiC, GaN, etc., and a light-emitting element such as an LED.
[0086] Examples of the element supporting member include a copper plate, a silver-plated copper plate, a lead frame plated with Ni / Pd, Ti / Pd / Au, Ni / Pd / Au, or the like (PPF; Pre-Plated Leadframe), a glass epoxy plate, and a ceramic member.
[0087] The bonding strength of the bonding layer formed by bonding the paste composition is also affected by the purpose and object of bonding, but may be 20 MPa or more, 30 MPa or more, or 40 MPa or more from the viewpoint of sufficient bonding strength.
[0088] The bonding strength is shear strength, and specifically, can be measured by the method described in Examples.
[0089] From the viewpoint of good bonding strength and high bonding reliability, the density of the bonding layer may be 78% or more, 80% or more, or 82% or more.
[0090] The density is the ratio of the sintered body portion in the bonding layer, and can be specifically measured by the method described in the Examples.
[0091] [Electrical and electronic components]
[0092] At least a portion of the electrical component or electronic component of the present invention is bonded using the paste composition of the present invention. As the electrical component or electronic component, for example, a component in which a heat generating component and a heat dissipating component are bonded using the paste composition can be cited. The paste composition can also be used as an adhesive for heat dissipating components.
[0093] By using the paste composition of the present invention for bonding, a bonding layer with high density and high bonding strength is formed. Even if the bonding layer is repeatedly subjected to hot and cold cycle (thermal cycle) loads, the change rate of thermal resistance is low and the bonding reliability is high. Therefore, the heat dissipation is high, the temperature rise of the heat generating component can be reduced, and an electrical component or electronic component with stable operation can be obtained.
[0094] Examples of the heat generating component include an optical pickup, a power transistor, etc. The heat generating component may be the semiconductor element or a component having the semiconductor element.
[0095] Examples of heat dissipation members include heat sinks and heat spreaders.
[0096] It should be noted that the heat-generating component and the heat-dissipating component may be directly bonded together via the paste composition, or may be indirectly bonded together by sandwiching another component having high thermal conductivity.
[0097] Example
[0098] Next, the present invention will be specifically described by way of Examples, but the present invention is not limited to these Examples at all.
[0099] [Production of Oxide-Containing Copper Particles]
[0100] The compounds used for producing the oxide-containing copper particles of each of Examples and Comparative Examples are as follows.
[0101] <Copper compounds>
[0102] FRC-D70: cuprous oxide; manufactured by FURUKAWA CHEMICAL S CO., LTD.; specific surface area 0.2 m 2 / g.
[0103] FRC-D30: cuprous oxide; manufactured by FURUKAWA CHEMICAL S CO., LTD.; specific surface area 0.5 m 2 / g.
[0104] FRC-05B: cuprous oxide; manufactured by FURUKAWA CHEMICAL S CO., LTD.; specific surface area 2.3 m2 / g.
[0105] <Amine compounds>
[0106] 4-Amino-1-butanol; manufactured by Tokyo Chemical Industry Co., Ltd.
[0107] 2-(2-Aminoethoxy)ethanol; manufactured by Tokyo Chemical Industry Co., Ltd.
[0108] ·6-Amino-1-hexanol; manufactured by Tokyo Chemical Industry Co., Ltd.
[0109] ·3-Amino-1-propanol; manufactured by Tokyo Chemical Industry Co., Ltd.
[0110] · n-Octylamine; manufactured by Tokyo Chemical Industry Co., Ltd.
[0111] <Carboxylic acid>
[0112] · Hexanoic acid: manufactured by Tokyo Chemical Industry Co., Ltd.
[0113] Caprylic acid; manufactured by Tokyo Chemical Industry Co., Ltd.
[0114] Acetic acid: manufactured by Tokyo Chemical Industry Co., Ltd.
[0115] · Decanoic acid; manufactured by Tokyo Chemical Industry Co., Ltd.
[0116] <Reducing compounds>
[0117] Hydrazine monohydrate; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0118] <Organic solvents>
[0119] 1-Propanol; manufactured by Tokyo Chemical Industry Co., Ltd.
[0120] ·Ethanol: manufactured by Tokyo Chemical Industry Co., Ltd.
[0121] ·Diethylene glycol: manufactured by Tokyo Chemical Industry Co., Ltd.
[0122] (Example 1)
[0123] 10 mmol of cuprous oxide (FRC-D70), 20 mmol of 4-amino-1-butanol, 20 mmol of hexanoic acid, 10 mmol of hydrazine monohydrate and 400 mL of 1-propanol were placed in a 2000 mL round-bottom flask, heated in an oil bath at 80°C while stirring at 250 rpm, and mixed for 180 minutes. The obtained mixed solution was centrifuged (25°C, 10000 rpm, 15 minutes; the same conditions are hereinafter applied), and the supernatant was removed. Ethanol was added to the residue, stirred and washed with a vacuum rotary mixer (25°C, 1000 rpm) for 10 minutes, centrifuged, and the supernatant was removed. This operation was repeated 4 times. Furthermore, ethanol was changed to diethylene glycol, and the same operation of washing, centrifugation and removal of the supernatant was repeated 2 times to obtain an oxide-containing copper particle cake.
[0124] (Examples 2 to 4, Comparative Examples 1 and 2)
[0125] The same operation as in Example 1 was carried out except that the raw material components shown in Table 1 were used to obtain each oxide-containing copper particle cake.
[0126] [Measurement and Evaluation of Oxide-Containing Copper Particles]
[0127] The oxide-containing copper particles (cakes) produced in Examples and Comparative Examples were subjected to the following measurement and evaluation.
[0128] (X-ray diffraction (XRD) measurement)
[0129] The oxide-containing copper particle cake was applied to a glass plate with a thickness of 200 μm, and XRD measurement was performed using an X-ray diffractometer ("SmartLabSE", manufactured by Rigaku Corporation; CuKα ray, focusing method). The obtained XRD pattern was fitted using a segmented pseudo-Voigt function.
[0130] <Cu 64 O and Cu 2 O mass ratio>
[0131] The XRD pattern was analyzed using the reference intensity ratio (RIR) method to determine the relative concentration of Cu and Cu 64 O and Cu 2 Cu O 100 mass% 64 O and Cu 2 Specifically, the strongest lines of each component (Cu(111), Cu 64 O(044) and Cu 2 O(111)), the integrated intensity obtained by subtracting the background intensity and each RIR value (Cu: 8.86; Cu 64 O: 4.89; Cu2 O: 8.28) to calculate the content.
[0132] <Cu(111) crystallite diameter>
[0133] The crystallite diameter C of Cu(111) was calculated from the half maximum width (half maximum width: FWHM): β and the Bragg angle: θ (1 / 2 of the diffraction angle 2θ) of the Cu(111) peak in the XRD pattern using the following Scherrer formula.
[0134] C=K·λ / (β·cosθ)
[0135] Wherein, Scherrer constant: K = 0.94, characteristic X-ray wavelength of CuKα ray: λ = 0.15418 [nm].
[0136] A sample obtained by heating the oxide-containing copper particle cake coated in a glass plate shape at 200° C. for 1 hour in a nitrogen atmosphere was similarly subjected to XRD measurement to determine the crystallite diameter of Cu (111).
[0137] Table 1 shows the crystallite diameter (C1) before heating (room temperature), the crystallite diameter (C2) after heating (200° C.), and the ratio C2 / C1 of the two.
[0138] (Scanning electron microscope (SEM) observation)
[0139] The oxide-containing copper particle cake was applied to a brass sample stand to which a carbon tape was attached, and dried at 90° C. for 3 hours in a nitrogen atmosphere to prepare a sample.
[0140] The sample was observed using a SEM (Schottky field emission scanning electron microscope "JSM-F100", manufactured by JEOL Ltd.; acceleration voltage 15 kV; magnification 100,000 times; the same below). The lengths of 200 particles in the SEM image were measured to determine the thickness and major diameter of the particles. In Table 1, the thickness and major diameter represent the median values of each.
[0141] In addition, as representative examples, SEM images of the samples of Example 4 and Comparative Example 2 are shown in Figure 1 and 2 .
[0142] [Evaluation of characteristics of sintered body]
[0143] The following measurements and evaluations were performed on the sintered bodies of the oxide-containing copper particles produced in Examples and Comparative Examples. These evaluation results are also shown in Table 1.
[0144] (Joint strength)
[0145] The oxide-containing copper particles (cake) produced in Examples and Comparative Examples were diluted with diethylene glycol to prepare paste compositions having a nonvolatile content of 80% by mass.
[0146] Using the prepared paste composition, an aluminum nitride sheet (3 mm × 3 mm, 200 μm thick) plated with Ti / Pd / Au was bonded to a copper substrate plated with Ni / Pd, and heated at 200°C for 60 minutes in a nitrogen environment (containing 3 vol% hydrogen) to produce a bonding test piece (a test piece without sealing resin) in which the copper particles were sintered.
[0147] The shear strength (bonding strength) of the bonded test piece was measured using a bond strength tester ("4000 Plus Bond Tester", manufactured by Nordon DAGE; room temperature (25°C), distance from substrate to load jig 0.15 mm, load speed 30 mm / min).
[0148] (Density)
[0149] After embedding the test piece without sealing resin with epoxy resin, the sample cut in the thickness direction was observed with SEM, and the area ratio occupied by the sintered body part in the binary image of the cross section of the bonding layer was calculated and regarded as the density.
[0150] (Hot and cold cycle test)
[0151] Using the paste composition, a silicon chip (3 mm × 3 mm, 200 μm thick) plated with Ti / Au was bonded to a die pad (4 mm × 4 mm) plated with Ni / Pd / Au on a QFP (Quad Flat Package) frame, and heated at 200°C for 60 minutes in a nitrogen atmosphere (containing 3% by volume of hydrogen) to sinter the copper particles. This was molded and sealed with an epoxy resin for sealing ("KE-G3000D", manufactured by Kyocera Corporation) to prepare a bonding test piece (test piece with sealing resin).
[0152] The test pieces without sealing resin and the test pieces with sealing resin were subjected to hot and cold cycle tests (one cycle: -40°C to 120°C / 30 minutes, 2000 cycles). The change rate of the thermal resistance of the joint before and after the test was measured using a transition thermal resistance measuring device ("Simcenter T3Ster", manufactured by Siemens Corporation). The change rate of the thermal resistance is shown in Table 1. The lower the change rate, the higher the bonding reliability. When the change rate is greater than 10%, the bonding reliability is low and is evaluated as poor.
[0153] Table 1
[0154]
[0155] Compared with Cu, Cu2 O and Cu 64 Total O 100 mass%, Cu 64 The particle shape of the oxide-containing copper particles (Examples 1 to 4) in which the content of O is within the range of 2.1 to 25.0 mass % is plate-like (see Figure 1 ), in contrast, Cu 64 The copper particles whose O content is outside the above range (Comparative Examples 1 and 2) have a substantially spherical particle shape (refer to Figure 2 ).
[0156] In addition, for the copper particles of Comparative Examples 1 and 2, the crystallite diameter of Cu (111) is greater than 30.0 nm in the non-heated state (room temperature), which is larger than that of Examples 1 to 4, and the change before and after heating at 200° C. is small. Therefore, it is speculated that the density of the bonding layer formed using the paste composition of Comparative Examples 1 and 2 is low, sufficient bonding strength cannot be obtained, and the bonding reliability is reduced.
[0157] It was confirmed that the paste compositions of Examples 1 to 4 can form a bonding layer having high density, high bonding strength, and high bonding reliability.
Claims
1. A plate-like copper particle containing copper oxide, wherein It contains Cu, Cu2O and Cu 64 O, relative to Cu, Cu2O and Cu 64 Total O 100 mass%, Cu 64 The content of O is 2.1 mass % to 25.0 mass %.
2. The plate-like copper particle containing oxide according to claim 1, wherein Compared with Cu, Cu2O and Cu 64 O in total is 100 mass %, and the content of Cu2O is 5.0 mass % or less.
3. The plate-like copper particle containing oxide according to claim 1 or 2, wherein When the copper particles are heated at 200° C. in a nitrogen environment, a ratio C2 / C1 of a Cu(111) crystallite diameter C2 measured by X-ray diffraction after heating to a Cu(111) crystallite diameter C1 measured by X-ray diffraction before heating is 2.0 or more.
4. The plate-like copper particle containing oxide according to claim 3, wherein The crystallite diameter C2 is greater than 55.0 nm. 5 . The plate-like copper particle containing an oxide according to claim 1 , wherein The thickness is 5nm to 50nm, the major diameter is 30nm to 300nm, and the major diameter is larger than the thickness.
6. A paste composition, wherein: The present invention comprises the plate-like copper particle containing the oxide according to any one of claims 1 to 5.
7. A semiconductor device, wherein: At least a portion of the semiconductor device is bonded using the paste composition according to claim 6.
8. An electrical component, wherein: At least a portion of the electrical component is joined using the paste composition according to claim 6.
9. An electronic component, wherein: At least a part of the electronic component is bonded using the paste composition according to claim 6.