High frequency polishing of ceramics
Through the grinding, fine research and elliptical vibration polishing technology of polycrystalline sintered ceramic bodies, the corrosion problem of ceramic components in the semiconductor plasma processing chamber is solved, and the production of large-size sintered ceramic bodies with high smoothness and corrosion resistance is achieved, improving the production of high-smooth and corrosion resistance. Productivity and component life.
Patent Information
- Application Number
- CN202380027559.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-01
AI Technical Summary
It is difficult to produce large-size sintered ceramic bodies with high smoothness and corrosion resistance, especially in semiconductor plasma processing chambers, where ceramic components are susceptible to corrosion and contamination by plasma, resulting in loss of yield.
Polycrystal sintered ceramic body is polished by grinding and fine grinding using multiple orbital sand mills with elliptical vibration. Combined with polishing pads and slurries of different particle sizes, the surface smoothness is less than 2 micro-inches and the porosity is less than 0.045%. goal.
It realizes high smoothness and corrosion resistance of large-sized sintered ceramic bodies, improves resistance to plasma etching, extends component life and reduces particle generation, and meets the high mechanical strength and corrosion resistance requirements of semiconductor processing.
Smart Images

Figure CN118891131A_ABST
Abstract
Description
Background Art
[0001] The present invention relates to a method and apparatus for polishing a dense sintered ceramic body to a very high degree of surface smoothness, the sintered ceramic body being suitable for use as a corrosion resistant component within a semiconductor plasma processing chamber.
[0002] Semiconductor processing requires the use of halogen-based gases in combination with high electric and magnetic fields to create a plasma environment. The plasma environment is created within a vacuum chamber for etching or depositing materials on semiconductor substrates. These vacuum chambers include component parts such as trays or windows, gaskets, injectors, rings, and cylinders. During semiconductor plasma processing, the substrate is typically supported within the vacuum chamber by a substrate holder, as disclosed, for example, in US 5,262,029 and US 5,838,529. The process gas used to create the plasma processing environment can be supplied to the chamber by various gas supply systems. Some processes involve the use of radio frequency (RF) fields, and the process gas is introduced into the processing chamber while the RF field is applied to the process gas to generate a plasma of the process gas. Ceramic materials used to form these components, especially those used for RF applications, need to have a relative humidity of approximately 1×10 -3 and a lower dielectric loss tangent. Dielectric losses higher than this cause overheating and hot spots within the components during use, resulting in process variability and yield loss. The use of components made from high purity starting powders and manufacturing processes that maintain initial purity will provide sintered ceramics that meet these low loss requirements. Harsh plasma processing environments require the use of highly corrosion and erosion resistant materials for chamber components. These components have been formed from materials that provide corrosion and erosion resistance in plasma environments and have been described, for example, in US 5,798,016, US 5,911,852, US 6,123,791 and US 6,352,611. In addition, plasma processing chambers have been designed to include components such as disks, rings and cylinders that confine the plasma to the wafer being processed. However, these parts used in plasma processing chambers are constantly attacked by plasma and are therefore corroded, eroded or accumulate contaminants and polymer accumulation. Plasma etching and deposition conditions cause corrosion and roughening of the surfaces of chamber parts exposed to the plasma. Such corrosion contributes to wafer-level contamination by releasing particles from component surfaces into the chamber, resulting in yield loss of semiconductor devices.
[0003] To address this problem, chamber components typically have a surface layer that is corrosion-resistant and erosion-resistant when exposed to process gases. The surface layer may be formed on a substrate or substrate that may have excellent mechanical properties, electrical properties, or other preferred properties. It is known that corrosion-resistant films or coatings such as yttrium oxide or yttrium aluminum garnet (YAG) are deposited on substrates or substrates formed of different materials, and the corrosion-resistant films or coatings are cheaper and stronger than most corrosion-resistant materials. Such films or coatings have been made by several methods. Vapor deposition has been used to deposit corrosion-resistant films on substrates, but due to internal film stress, vapor deposition is limited to relatively thin layers, and small holes are usually present in the film. These internal film stresses produce poor interlayer adhesion and lead to delamination at the interface between the corrosion-resistant film and the substrate, causing these layers to be prone to cracking and peeling, thereby causing undesirable particulate contamination. Corrosion-resistant coatings or films made by aerosol or plasma spraying techniques typically exhibit a high level of porosity of 3% to about 50%, and a corresponding low density. Furthermore, these films produced by aerosol or spray coating methods exhibit poor interfacial adhesion between the substrate material and the corrosion resistant layer, leading to chipping and flaking and subsequent chamber contamination.
[0004] Therefore, there is a need to produce hard ceramic materials with highly polished surfaces having surface roughness uniformly less than about 2 microinches for high strength sintered ceramic bodies of large size (greater than 100 mm, such as, for example, from 100 mm to 625 mm) to enable large-scale manufacturing of corrosion-resistant semiconductor devices. Summary of the invention
[0005] Advantageously, the present disclosure provides a method for polishing the surface of a large-sized sintered ceramic body to a uniform surface smoothness of about 2 micro-inches to about 1.5 micro-inches. A method for polishing the surface of a polycrystalline sintered ceramic body is disclosed herein, the method comprising the following steps: a) providing a sintered ceramic body comprising a polycrystalline material and having a density of about 99.5% to about 99.999% of the theoretical density of the polycrystalline material, wherein the sintered ceramic body has at least one surface; b) grinding the at least one surface until the surface has (i) an average flatness of no more than 25 microns as measured using a spherometer at angles of 0°, 90°, 180°, and 270° on four quadrants of the at least one surface, (ii) an Ra of less than 14 micro-inches, and (iii) an Rz of less than 160 micro-inches; c) after the grinding step, lapping the at least one surface with a lapping plate and a lapping medium slurry. d) after lapping, continuously polishing the at least one surface in a series of polishing steps until the at least one surface exhibits an Ra value of ≤ 2 micro-inches and an Rz of ≤ 2 micro-inches and an absolute value of flatness greater than 15 microns (as measured using a spherometer), wherein the polishing is performed using an apparatus comprising a plurality of elliptically vibrating orbital sanders (also referred to as orbital sanders), each of the orbital sanders comprising a polishing pad to contact the at least one surface during polishing, wherein the series of polishing steps comprises: i) a first polishing step in which the polishing pad is used with a slurry of 4 to 10 micron coarse grit particles; and ii) a second polishing step in which the polishing pad is used with a slurry of 1 to 3 micron coarse grit particles.
[0006] In another aspect, the present invention provides a polycrystalline sintered ceramic body comprising at least 99.99% YAG and having at least one upper surface having a surface area greater than 400 square inches, the surface having an absolute spherometer measurement greater than 15 microns over four quadrants of the disk, and an Ra and Rz less than or equal to 2 microinches each over the surface area, and a porosity less than 0.045% over the surface area, wherein the sintered ceramic disk has a thickness of at least 20 mm.
[0007] In yet another aspect, the present invention provides a polishing apparatus comprising a plate including a plurality of elliptically vibrating orbital sanders, each of the orbital sanders including a polishing pad; and a rotatable table adapted to rotate a part to be polished, wherein the plate remains stationary during polishing while the part rotates on the table, and wherein the orbital sanders are mounted on the plate so that the polishing pad faces the rotatable table.
[0008] The embodiments of the present invention may be used alone or in combination with each other. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a perspective view of an embodiment disclosed herein;
[0010] Figure 2 is a perspective view of an exemplary mounting plate;
[0011] Figure 3 is a diagrammatic representation of an embodiment of a random orbital sander for use in embodiments disclosed herein;
[0012] Figure 4 is a perspective view of an embodiment of a housing for a random orbital sander used in embodiments disclosed herein;
[0013] Figure 5 In the embodiments disclosed herein, the Figure 2 an illustration of an embodiment of a random orbital sander on a plate of; and
[0014] Figure 6 is an embodiment of an exemplary polishing apparatus for use in the disclosed method. DETAILED DESCRIPTION
[0015] The subsequent detailed description only provides preferred exemplary embodiments and is not intended to limit the scope, applicability or configuration of the present invention. On the contrary, the subsequent detailed description of the preferred exemplary embodiments will provide an enabling description for implementing the preferred exemplary embodiments of the present invention to those skilled in the art. Various changes may be made to the functions and arrangements of the elements without departing from the spirit and scope of the present invention as set forth in the appended claims.
[0016] The term "about" means approximately or close to, and in the context of numerical values or ranges recited herein, means in one embodiment ±20%, ±10%, ±5%, or ±3% of the recited or claimed numerical value or range.
[0017] The terms "one", "a", "the / said" and similar references used in the context of describing the present disclosure (particularly in the context of the claims) are understood to cover both the singular and the plural, unless otherwise specified herein or clearly contradictory to the context. The enumeration of the range of values herein is intended only to be used as a shorthand method for individually referring to each individual value within the range. Unless otherwise specified herein, each individual value is incorporated into the specification as if it were individually listed herein. Unless otherwise specified herein or clearly contradictory to the context, all methods described herein can be performed in any suitable order. The use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the present disclosure, rather than to impose limitations on the scope of the claims. Any language in the specification should not be understood to indicate that any element not protected by the claims is necessary for implementing the present disclosure.
[0018] Unless explicitly stated otherwise, the term "comprising" is used in the context of this document to indicate that in addition to the members of the list introduced by "comprising", there may be additional members optionally present. However, it is contemplated that as a specific embodiment of the present disclosure, the term "comprising" encompasses the possibility that there are no additional members, that is, for the purpose of this embodiment, "comprising" should be understood to have the meaning of "consisting of..." or "consisting essentially of...".
[0019] As used herein, the following terms are defined as follows: "alumina" is understood to be aluminum oxide including Al2O3, "zirconia" is understood to be zirconium oxide including ZrO2, and "yttria" is understood to be yttria including Y2O3.
[0020] As used herein, the terms "semiconductor wafer," "wafer," "substrate," and "wafer substrate" may be used interchangeably. Wafers or substrates used in the semiconductor device industry typically have a diameter of 200 mm, or 300 mm, or 450 mm.
[0021] As used herein, the term "sintered ceramic body" is synonymous with "multilayer sintered ceramic body," "multilayer corrosion-resistant ceramic," "corrosion-resistant body," "sintered ceramic," "multilayer monolith," and similar terms, and refers to a monolithic, unitary sintered ceramic article formed by co-compacting more than one powder mixture by applying pressure and heat, which produces a monolithic, dense, multilayer sintered ceramic body. The monolithic, multilayer sintered ceramic body can be machined into a monolithic, multilayer sintered ceramic component that can be used as a chamber component in plasma processing applications. Thus, the multilayer sintered ceramic bodies disclosed herein are not formed by laminating preformed layers together, i.e., the multilayer sintered ceramic bodies disclosed herein are not laminated materials.
[0022] As used herein, the term "layer" is understood to mean a certain thickness of material, typically one of several. The material may be, for example, a ceramic powder, a powder mixture, a calcined powder mixture or a sintered region or a sintered portion.
[0023] As used herein, "ambient temperature" refers to a temperature range of about 22°C to 25°C.
[0024] Semiconductor etching and deposition reactors require reactor components with surfaces that are highly resistant to corrosion and erosion by the halogen-containing plasmas necessary for processing. These surfaces preferably minimize the release of particles from the component surfaces into the chamber. In addition, the chamber components must have sufficient mechanical strength for handling and use, especially in large (e.g., diameter>100mm) component sizes. Sintered ceramic bodies can be machined into sintered components, and therefore, must be capable of being handled and machined in large sizes while providing corrosion resistance, low particle generation, and high mechanical strength.
[0025] Disclosed herein is a method for polishing a surface of a polycrystalline sintered ceramic body, the method comprising the steps of: a) providing a sintered ceramic body comprising a polycrystalline material and having a density of about 99.5% to about 99.999% of a theoretical density of the polycrystalline material, wherein the sintered ceramic body has at least one surface; b) grinding the at least one surface until the surface has (i) an average flatness of no more than 25 microns as measured using a spherometer at angles of 0°, 90°, 180°, and 270° on four quadrants of the at least one surface, (ii) an Ra of less than 14 microinches, and (iii) an Rz of less than 160 microinches; c) after the grinding step, polishing the surface of the at least one surface with a lapping plate and a lapping medium slurry; d) after lapping, continuously polishing the at least one surface in a series of polishing steps until the at least one surface exhibits an Ra value of ≤ 2 micro-inches and an Rz of ≤ 2 micro-inches and an absolute value of flatness greater than 15 microns (as measured using a spherometer), wherein the polishing is performed using an apparatus comprising a plurality of orbital sanders that oscillate elliptically, each of the orbital sanders comprising a polishing pad to contact the at least one surface during polishing, wherein the series of polishing steps comprises: i) a first polishing step in which the polishing pad is used with a slurry of 4 to 10 micron coarse grit particles; and ii) a second polishing step in which the polishing pad is used with a slurry of 1 to 3 micron coarse grit particles.
[0026] Sintered ceramic body
[0027] The first step of the method includes providing a sintered ceramic body comprising a polycrystalline material and having a density of about 99.5% to about 99.999% of the theoretical density of the polycrystalline material, wherein the sintered ceramic body has at least one surface. As used herein, the term "providing" means obtaining or starting the process using a sintered ceramic body having the recited properties.
[0028] The sintered ceramic body for polishing according to the disclosed method has a maximum dimension greater than 100 mm, such as, for example, 100 mm to about 625 mm, preferably 100 mm to 622 mm, preferably 200 mm to about 625 mm, preferably 300 mm to about 625 mm, preferably 400 mm to about 625 mm, preferably 500 mm to about 625 mm, preferably 300 mm to 622 mm, preferably 400 mm to 622 mm, and preferably 500 mm to 622 mm. Preferably, the sintered ceramic body has a surface area greater than 400 square inches, a thickness of at least 20 mm, and is opaque, although it may be translucent.
[0029] In some embodiments, the sintered ceramic body comprising a polycrystalline material is a single-layer sintered ceramic body, and in other embodiments, the sintered ceramic body is a multilayer sintered ceramic body. Suitable single-layer sintered ceramic bodies are disclosed, for example, in WO 2020 / 206389 (yttrium oxide), WO 2021 / 141676 (yttrium aluminum oxide), WO 2022 / 015688 (magnesium aluminate spinel), and PCT / US2021 / 054947 (zirconia toughened alumina), PCT / US2021 / 052989 (yttrium oxide), the disclosures of which are incorporated herein by reference in their entirety. Suitable multilayer sintered ceramic bodies are disclosed, for example, in PCT / US2021 / 054773, PCT / US2021 / 063973, PCT / US2021 / 052981 (large-sized sintered ceramic bodies and methods for making the same), and WO 2021 / 141676 (yttrium aluminum oxide), the disclosures of which are incorporated herein by reference in their entirety. In addition to the methods disclosed in the above-mentioned reference patent application documents, suitable apparatus and methods for making high-density, large-sized sintered ceramic bodies for polishing according to the disclosed methods are disclosed in PCT / US2021 / 052978 (apparatus for preparing large-sized sintered ceramic bodies) and PCT / US2021 / 052981 (large-sized sintered ceramic bodies and methods for making the same), the disclosures of which are incorporated herein by reference in their entirety.
[0030] The preparation of sintered ceramic bodies as disclosed herein may also be achieved by using a pressure-assisted sintering process such as uniaxial hot pressing, wherein the mold configuration or tool set is heated by an externally applied heat source such as induction heating.
[0031] The polycrystalline material of the sintered ceramic body is preferably at least one selected from the group consisting of: YAG, yttrium oxide, aluminum oxide, magnesium aluminate spinel, and a combination of yttrium oxide and zirconium oxide. If it is a multilayer embodiment, each layer can be selected from at least one of the following: YAG, yttrium oxide, aluminum oxide, magnesium aluminate spinel, and a combination of yttrium oxide and zirconium oxide.
[0032] In certain embodiments, a sintered ceramic body as disclosed herein comprises at least one first layer having at least one polycrystalline ceramic material comprising a garnet-type structure having a composition comprising yttrium oxide and aluminum oxide in a ratio of about 3:5. 12 YAG (yttrium aluminum oxide or yttrium aluminate), spinel (magnesium aluminate spinel, MgAl2O4) and yttrium oxide and zirconium oxide, wherein zirconium oxide is present in the yttrium oxide in an amount of not less than 10 mol % ZrO2 and not more than 25 mol % ZrO2. According to the disclosed method, the at least one first layer provides a surface to be polished.
[0033] In a preferred embodiment, the sintered ceramic body as disclosed herein comprises at least one first layer having at least one polycrystalline ceramic material comprising YAG. Thus, the surface to be polished comprises YAG.
[0034] The sintered ceramic bodies used in the disclosed methods have a density of about 99.5% to about 99.999% of the theoretical density of the polycrystalline material, such as, for example, about 99.5% to about 99.99%, and about 99.56% to about 99.78%.
[0035] Due to the difference in the density of the layer, the density measurement of the multilayer body has been proven to be challenging. The density of the multilayer sintered ceramic body can be measured by dividing the sample cut from the full thickness of the multilayer sintered body into its first and second layers and measuring the density of these layers separately. The density measurement of the two-layer sintered ceramic body manufactured by Example 4 of PCT / US2021 / 063973 will now be illustrated, and the sintered ceramic body includes YAG as a thinner first layer and zirconia toughened alumina as a thicker second layer. Density measurements are performed according to the Archimedes immersion method of ASTM B962-17, and the density is measured to be 4.55g / cc to 4.57g / cc for at least one first layer of polycrystalline YAG, preferably about 4.56g / cc. The reported density value is the average of 5 measurements, and the standard deviation of the measured value (using a known standard) is about 0.002. The density of commercially available bulk YAG single crystal samples is measured using the method disclosed herein. An Archimedean density of 4.56 g / cc was obtained in 5 measurements, and this value was taken as the theoretical density of YAG as used herein. Therefore, at least one first layer of the multilayer sintered ceramic body including YAG according to one embodiment has a theoretical density of 99.5% to 99.999% of the theoretical density of YAG. The density of at least one second layer including about 16 volume % of at least one of stabilized zirconia and partially stabilized zirconia (and the balance being alumina) was measured according to the Archimedean impregnation method of ASTM B962-17, and the density was calculated to be about 4.32 g / cc. The volume mixing rule known in the art is used to calculate the theoretical density of at least one second layer including alumina and about 16 volume % of at least one of stabilized zirconia and partially stabilized zirconia, and the density was measured to be 4.31 g / cc to 4.33 g / cc, preferably about 4.32 g / cc and taken as the theoretical density of at least one second layer 102. Therefore, the theoretical density percentage of at least one second layer 102 of the multilayer sintered ceramic body (comprising about 16 volume % zirconium oxide and the balance being aluminum oxide) is 98% to 100%, preferably 99% to 100%, preferably 99.5% to 100%, preferably about 100% of the theoretical density. The monolithic multilayer sintered ceramic body disclosed according to this embodiment has at least one first layer and at least one second layer, each having a theoretical density percentage (also expressed as relative density, RD) greater than 98%, preferably 98% to 100%, preferably 99% to 100%, preferably 99.5% to 99.999%, preferably about 100% of the theoretical density of the monolithic multilayer sintered ceramic body.
[0036] The relative density (RD) of a given material is defined as the ratio of the measured density of the sample to the theoretical density of the same material, as shown in the following formula. The volume porosity (Vp) is calculated from the density measurement as follows:
[0037]
[0038] Wherein rsample is the (Archimedean) density measured according to ASTM B962-17, rtheoretical is the theoretical density as disclosed herein, and RD is the relative fractional density. Using this calculation, the volume porosity (Vp) level in percentage is calculated from the measured density values of each of at least one first layer comprising YAG and at least one second layer comprising alumina and about 16 volume % of partially stabilized zirconia of the multilayer ceramic sintered body of Example 4 of PCT / US2021 / 063973 to be 0.04% to 2%, preferably 0.04% to 1%, preferably 0.04% to 0.8%, preferably 0.04% to 0.6%, preferably 0.04% to 0.5% and preferably 0.04% to 0.4%.
[0039] The sintered ceramic body disclosed above can be obtained with an average density of 99.5% to 99.999%, wherein the variation of the density over the largest dimension is 5% or less, preferably 4% or less, preferably 3% or less, preferably 2% or less, preferably 1% or less, wherein the largest dimension can be, for example, about 625 mm and less, 622 mm and less, 610 mm and less, preferably 575 mm and less, preferably 525 mm and less, preferably 100 mm to 625 mm, preferably 100 mm to 622 mm, preferably 100 mm to 575 mm, preferably 200 mm to 625 mm, preferably 200 mm to 510 mm, preferably 400 mm to 625 mm, preferably 500 mm to 625 mm.
[0040] The high density of the sintered ceramic body to be polished according to the disclosed method translates into a high hardness value for the surface, which can provide resistance to the corrosive effects of ion bombardment used during typical plasma processes. Erosion or spalling can be caused by ion bombardment of the surface of a component or layer using an inert plasma gas such as Ar. Those materials having high hardness values can be preferably used as materials for the component, since their increased hardness values provide greater resistance to ion bombardment and, thereby, greater resistance to erosion. Thus, the sintered ceramic body exhibits a high Vickers hardness. For example, hardness measurements were performed on an exemplary sintered ceramic body including a YAG layer providing a surface to be polished according to ASTM Standard C1327 "Standard Test Method for Vickers Indentation Hardness of Advanced Ceramics". The test equipment used for all hardness measurements was a Wilson microhardness tester model VH1202. For YAG surfaces, the measured hardness value is at least 1200HV, preferably at least 1400HV, preferably at least 1800HV, preferably at least 2000HV, 1300HV to 1600HV, 1300HV to 1500HV, 1300HV to 1450HV, 1300HV to 1400HV, 1400HV to 1600HV, 1450HV to 1600HV, 1450HV to 1550HV. The measured values obtained using the Vickers hardness method known in the art are converted into SI units of GPa. The hardness values were measured to be 12.75 GPa to 15.69 GPa, 12.75 GPa to 14.71 GPa, 12.75 GPa to 14.22 GPa, 12.75 GPa to 13.73 GPa, 13.73 GPa to 15.69 GPa, 14.22 GPa to 15.69 GPa, preferably 14.22 GPa to 15.20 GPa. These high hardness values can help to enhance resistance to ion bombardment during semiconductor etching processes and reduce corrosion during use, thereby providing extended component life when machining the multilayer sintered ceramic body into sintered ceramic components with fine-scale features.
[0041] In one embodiment, the sintered ceramic body has an average hardness of 13.0 GPa to 16.0 GPa calculated from eight test repetitions using an applied load of 0.2 kgf as measured according to ASTM Standard C1327. In another embodiment, the sintered ceramic body has an average hardness of about 13.5 GPa to 15 GPa calculated from eight test repetitions using an applied load of 0.2 kgf as measured according to ASTM Standard C1327. In other embodiments, the average hardness of the sintered ceramic body is about 13.8 GPa to 15.8 GPa calculated from eight test repetitions using an applied load of 0.025 kgf.
[0042] The sintered ceramic body to be polished according to the methods disclosed herein is translucent and not of optical grade. In embodiments, the sintered ceramic body transmits less than 60% of light.
[0043] The sintered ceramic body to be polished according to the methods disclosed herein typically has a thickness of at least 10 mm, preferably 10 mm to 30 mm, and more preferably 25 mm to 28 mm.
[0044] Grinding steps
[0045] The disclosed method includes performing the step of grinding at least one surface to modify the surface of the sintered ceramic body to (i) an average flatness of no greater than 25 microns as measured using a spherometer at angles of 0°, 90°, 180°, and 270° on four quadrants of the at least one surface, (ii) an Ra of less than 14 microinches, and (iii) an Rz of less than 160 microinches.
[0046] The effect of the grinding step is to flatten the surface to be ground of the sintered ceramic body. The flatness of the surface can be measured using a spherometer, such as the Mahr meter, model Millimess 1003 spherometer, available from the Mahr Group of Mahr GmbH, Gottingen Germany, in Gottingen, Germany. Flatness is preferably measured using a spherometer at an angle of 0, 90, 180 and 270 degrees across the surface or in some embodiments on four quadrants of the surface, using a plane fixture with the above-mentioned Mahr meter calibrated to the main plane, such as the surface plate available from Standridge Granite Corp., Santa Fe Springs, California, in Santa Fe Springs, California.
[0047] Ra and Rz are different parameters of roughness. Ra is the average roughness of a surface. Rz is the difference between the highest "peak" and the deepest "valley" in a surface.
[0048] Ra is the integer average of all absolute roughness profiles deviating from the center line within the measuring length. Rz is the absolute peak-to-valley average of five consecutive sampling lengths within the measuring length. Ra compares all dimensions and has no discriminating value when it comes to separating rejects from suitable cylinders.
[0049] The average roughness value Ra (DIN 4768) is the arithmetic mean of all values of the roughness profile R within a measuring distance 1 m. It therefore specifies the average deviation of the surface profile from the mean line.
[0050] The mean roughness depth Rz (DIN 4768) is the average of five individual roughness depths measured at separate distances in succession. In other words, it is calculated from five Rt values. Deviations from the mean are concentrated particularly at the highest peaks and valleys.
[0051] In one embodiment, the disclosed process includes the steps of grinding the surface of the sintered ceramic body using a Blanchard machine until the ceramic surface has a flatness of no greater than 25 microns measured at 0, 90, 180, and 270 degrees on four quadrants of the surface. In addition, Ra must be less than 14 micro-inches, and Rz should be less than 160 micro-inches, and more preferably less than 150 micro-inches.
[0052] Ra and Rz can be measured using, for example, a digital microscope, such as the Keyence VK-X200 series available from Keyence Corporation of America, Itasca, Illinois, USA.
[0053] Research
[0054] The method disclosed herein includes the step of lapping at least one surface using a lapping plate and a lapping medium slurry. Lapping is a process known in the art and involves contacting at least one surface of a sintered ceramic body with a surface of a lapping plate while at least one of the ceramic body and the plate is rotated so as to remove material from the surface of the sintered ceramic body and provide a flatter and / or smoother surface relative to before the lapping step. This includes at least partially removing scratches in the surface, if present. Abrasive media (e.g., diamond grit or aluminum oxide) may be used to help remove material from the surface to make it smoother. Abrasive material may be fixed to the lapping plate and / or dispensed onto the surface of the lapping plate during lapping (e.g., as an abrasive slurry).
[0055] The lapping steps disclosed herein may include more than one lapping process to achieve the desired flatness and / or smoothness. In one embodiment, the lapping steps include (i) a first lapping step, wherein the lapping medium is aluminum oxide having an average particle size of 30 to 50 microns; (ii) a second lapping step, wherein the lapping medium is aluminum oxide having an average particle size of 10 to 20 microns; and (iii) a third lapping step, wherein the lapping medium is aluminum oxide having an average particle size of 5 to 10 microns. In another embodiment, the lapping medium in the first lapping step has a particle size of 40 microns; (ii) the lapping medium in the second lapping step has a particle size of 12 microns; and (iii) the lapping medium in the third lapping step has a particle size of 6 microns.
[0056] Lapping is performed by mounting a sintered ceramic body on a support (platen) with the ceramic surface to be polished facing upward. The lapping plate is pressed against the ceramic surface and oscillates back and forth across the ceramic surface while the ceramic surface rotates. Lapping also allows rotation, and the lapping plate and support can rotate in the same direction or in opposite directions. At a given grit size and fluid viscosity, varying the lapping pressure produces higher or lower material removal rates, thicker or thinner films, and rougher or finer surface finishes. Therefore, in practice, the pressure is usually lighter at the beginning of the process, increased as the work proceeds, and reduced near the end. This results in optimal material removal rate, surface finish, and flatness, resulting in a perfect overall surface finish quality. Waviness (also known as peaks and valleys) is a calculation of surface irregularities with a spacing greater than the surface roughness. These usually occur due to warping, vibration, or deflection during the machining process.
[0057] Preferably, after the lapping step, the surface smoothness is about 6 micro inches.
[0058] Vibration polishing
[0059] The disclosed method comprises the steps of: after lapping, continuously polishing at least one surface in a series of polishing steps until the at least one surface exhibits an Ra value of ≤2 microinches and an Rz of ≤2 microinches and an absolute value of flatness greater than 15 micrometers (as measured using a spherometer), wherein the polishing is performed using an apparatus comprising a plurality of orbital sanders that oscillate elliptically, each of the orbital sanders comprising a polishing pad to contact the at least one surface during polishing, wherein the series of polishing steps comprises: i) a first polishing step, wherein the polishing pad is used with a polishing slurry comprising coarse sand particles of 4 to 10 micrometers; and ii) a second polishing step, wherein the polishing pad is used with a polishing slurry comprising coarse sand particles of 1 to 3 micrometers.
[0060] Polishing according to the disclosed method is accomplished using an apparatus comprising a plurality of elliptically oscillating orbital sanders, each of the orbital sanders comprising a polishing pad to contact the at least one surface during polishing. Figure 1, an apparatus 10 is shown including a plate 2 including a plurality of orbital sanders 4 (also referred to herein as "orbital sanders") that oscillate elliptically, each of which includes a polishing pad 8. Each of the plurality of orbital sanders 4 is mounted to the plate 2 using a screw / bolt assembly 6. Orbital sanders are known in the art and are powered by electricity or pneumatic pressure. Non-limiting examples of orbital sanders 4 suitable for use in the disclosed polishing method include random orbital sanders described in U.S. Patent Nos. 5,934,985; 5,595,531; 5,580,302; 5,411,386; 5,392,568 and 5,384,984, all of which are incorporated herein by reference in their entirety, and / or commercially available orbital sanders, such as those available from Dynabrade in Clarence, NY, USA.
[0061] Figure 2 A plate 2 is illustrated that includes a hole 5 for receiving a screw / bolt assembly 6 for mounting each of a plurality of orbital sanders 4 and a mounting portion 7 for mounting the plate 2 to an apparatus for a polishing operation. The plate 2 may be made of any durable material known in the art and suitable for withstanding the pressures of polishing, including steel. In the illustrated embodiment, the plate 2 is circular, however, it may have any shape as long as it can rotate.
[0062] Figures 3 to 5 The orbital sander 4, the housing 9 and the assembled orbital sander 4 are illustrated respectively ready to be mounted to the plate 2. Figure 3 , a pneumatic orbital sander is shown having a pneumatic opening assembly 12 that includes an air inlet and an air outlet to provide air and exhaust air as needed. In an exemplary embodiment, compressed air at about 100 psi is used to power the orbital sander. Connections and hoses to a pressurized air supply are not shown.
[0063] The polishing pad 8 includes a press plate, which may or may not include abrasive particles (also referred to herein as "grit particles") for polishing at least one surface of the sintered ceramic body. In an embodiment where the press plate does not include abrasive particles incorporated therein, a slurry containing an abrasive is then applied between the sintered ceramic body and the press plate for polishing. In any case, the phrase "wherein the polishing pad includes X micron grit particles" is intended to include particles delivered by a liquid slurry. The press plate is secured to the bearing via a plurality of threaded screws extending through an opening in the press plate. The bearing is eccentrically disposed relative to the drive spindle of the motor so that when the press plate is rotationally driven by the motor, the bearing imparts orbital motion to the press plate. The press plate can be any size desired, such as, for example, a diameter of 80 mm to 300 mm. In one embodiment, the press plate is 6 inches (152.4 mm).
[0064] In some embodiments, the polishing pad 8 is an unfilled microporous foam elastomeric pad, such as commercially available from Universal Photonics Incorporated, Central Islip, NY, USA. https: / / www.universalphotonics.com / UPIProducts / Consumables / tabid / 102 / prtype / 1105 / prid / 490 / Default.aspx ) of polyurethane pad.
[0065] The slurry suitable for use in the polishing step of the disclosed method includes abrasive particles of the desired size and a liquid delivery medium, such as, for example, water. The slurry may include other components commonly found in such slurries, such as, for example, lubricants. The abrasive (grit) particles should be harder than the surface to be polished, and may be selected from, for example, polycrystalline diamond particles and aluminum oxide particles. Preferably, the abrasive particles used in the polishing step are polycrystalline diamond particles in an aqueous suspension.
[0066] refer to Figure 4 The housing 9 has an opening 11 to receive an air supply hose in the case of a pneumatic motor or an electrical connection in the case of an electric motor. Figure 5 The assembled orbital sander is shown equipped with a screw / bolt assembly ready for mounting on a board 2. The orbital sander 4 may be mounted on a board 2 in any suitable configuration.
[0067] The orbital sander 4 typically exhibits a speed of 5,000 RPM to 15,000 RPM. In some embodiments, the orbital sander exhibits a speed of 10,000 RPM to 15,000 RPM, and in a preferred embodiment, the speed is 12,000 RPM (maximum). Such speeds can provide high shear rates for polishing. In some embodiments, when a slurry is used, the shear rate of the slurry relative to the sintered ceramic body is about 1 m / s to about 10 m / s, and preferably about 6 m / s.
[0068] Figure 6 An exemplary polishing apparatus 20 for use in the polishing step of the disclosed method is shown. The plate 2 is fixed and the rotatable table 22 is adapted to rotate a part 24 having a surface 26 which is to be polished with a slurry delivered by a slurry delivery apparatus 28. In the illustrated embodiment, there are four orbital sanders 4, however, in other embodiments there may be two or three or five. The orbital sanders 4 are mounted on the plate 2 so that the polishing pads face the rotatable table and thus the sintered ceramic body is fixed to the table. During the polishing step, at least one surface of the sintered ceramic body rotates in the illustrated embodiment and the orbital sanders are stationary. Exemplary polishing apparatus as shown Figure 6 as shown in .
[0069] The polishing step is preferably performed in a number of consecutive sub-steps, each sub-step using a coarse sand of a reduced particle size relative to the previous step. In one embodiment, a series of polishing steps includes: i) a first polishing step in which the polishing pad includes 4 microns to 10 microns of coarse sand particles; and ii) a second polishing step in which the polishing pad includes 1 micron to 3 microns of coarse sand particles. In one embodiment, a 6 micron coarse sand slurry is used for the first polishing step and a 2 micron coarse sand slurry is used for the second polishing step. In another embodiment, a 6 micron coarse sand slurry is used for the first polishing step and a 1 micron coarse sand slurry is used for the second polishing step. Typically, the pressure on the surface of the sintered ceramic body during the polishing step is 0.2 psi to 2 psi, more preferably 0.3 psi to 1 psi, and the RPM of the rotary table is preferably 100 RPM to 200 RPM, more preferably 130 RPM to 160 RPM, and even more preferably 140 RPM to 150 RPM.
[0070] After performing the method disclosed herein, as measured from SEM images and using ImageJ software, the porosity of the polished surface is preferably less than 0.045% on the polished surface area. Typically, measurements across 7 SEM images are performed. In some embodiments, as measured from SEM images and using ImageJ software, the porosity as a percentage of total area is presented as an amount of 0.0005% to 0.045%. Thus, for example, in an image of an area of about 54 μm×54 μm, the polished surface of the sintered ceramic body disclosed herein includes a very low (by total area <0.045%) percentage of porosity, thereby providing a corrosion-resistant and erosion-resistant surface for a plasma processing chamber.
[0071] The disclosed method produces a polycrystalline sintered ceramic body having at least one upper surface having a surface area greater than 400 square inches, the surface having an absolute spherometer measurement greater than 15 microns over four quadrants of the disk, and an Ra and Rz less than or equal to 2 microinches each over the surface area, and a porosity less than 0.045% over the surface area, wherein the sintered ceramic disk has a thickness of at least 20 mm.
[0072] In one embodiment where the sintered ceramic body comprises YAG, the disclosed method produces a polycrystalline sintered ceramic body comprising at least 99.99% YAG and having at least one upper surface having a surface area greater than 400 square inches, the surface having an absolute spherometer measurement greater than 15 microns over four quadrants of the disk, and an Ra and Rz less than or equal to 2 microinches each over the surface area, and a porosity less than 0.045% over the surface area, wherein the sintered ceramic disk has a thickness of at least 20 mm.
[0073] One advantage of the disclosed method is that particle pullout is prevented. Particle pullout is the breaking off of particles on a surface to create pits, resulting in significant deviations in surface smoothness, which can be easily attacked by plasma etching gases.
[0074] Example
[0075] A 24" disk having a 99.99% YAG surface was obtained, with a YAG density averaging at least 99.5% of the maximum theoretical density of YAG. When lapped and polished as described herein, the 24" disk produced the average final Ra, Rz, and RSm values shown in the following table:
[0076] Measuring direction Ra(μm) Rz(micrometer) RSm(micrometer) Vertically across the plate 0.0191 0.1495 5.1144 Horizontally across the plate 0.0181 0.1405 6.918
[0077] For comparison, a 22 inch diameter example disk was prepared from 99.99% YAG, but with an average density of only about 97% of the maximum theoretical density of YAG. Lapping and polishing this example disk as previously described produced the average final Ra, Rz, and RSm values shown in the following table:
[0078] Measuring direction Ra(μm) Rz(micrometer) RSm(micrometer) Vertically across the plate 0.025 0.212 5.742 Horizontally across the plate 0.028 0.275 10.533
[0079] By comparing the values in the two tables above, it can be seen that the comparative 22 inch diameter example disc has a significantly rougher surface. Since the lapping and polishing steps were identical for both discs, this is believed to be due to the difference in the average density of the YAG surface polished on the discs. Specifically, the disc with the lower density surface results in a greater surface roughness than the disc with the greater density.
[0080] A number of embodiments as disclosed herein have been described. However, it should be understood that various modifications may be made without departing from the spirit and scope of the embodiments disclosed herein. Therefore, other embodiments are within the scope of the following claims.
Claims
1. A method for polishing the surface of a polycrystalline sintered ceramic body, the method comprising the following steps: a. providing a sintered ceramic body comprising a polycrystalline material and having a density of about 99.5% to about 99.999% of a theoretical density of the polycrystalline material, wherein the sintered ceramic body has at least one surface; b. grinding the at least one surface until the surface has (i) an average flatness of no more than 25 microns as measured using a spherometer, measured at angles of 0°, 90°, 180°, and 270° on four quadrants of the at least one surface, (ii) an Ra of less than 0.3556 μm (14 microinches), and (iii) an Rz of less than 4.064 μm (160 microinches), wherein Ra means the average roughness of the surface as the integer average of all absolute roughness profiles offset from a centerline within a measurement length, and Rz means the difference between the highest peak and the deepest valley in the surface as the absolute peak-to-valley average of five consecutive sampling lengths within the measurement length; c. after the grinding step, lapping the at least one surface with a lapping plate and a lapping medium slurry; d. After lapping, continuously polishing the at least one surface in a series of polishing steps until the at least one surface exhibits an Ra value of ≤ 0.0508 μm (2 microinches) and an Rz of ≤ 0.0508 μm (2 microinches) and an absolute value of flatness greater than 15 micrometers as measured using a spherometer, wherein the polishing is performed using an apparatus comprising a plurality of orbital sanders that oscillate elliptically, each of the orbital sanders comprising a polishing pad to contact the at least one surface during polishing, wherein the series of polishing steps comprises: i. a first polishing step, wherein the polishing pad is used with a slurry of 4 to 10 micron grit particles; as well as ii. A second polishing step wherein the polishing pad is used with a slurry of 1 micron to 3 micron grit particles.
2. The method of claim 1, wherein the lapping step comprises (i) a first lapping step, wherein the lapping medium is aluminum oxide having an average particle size of 30 microns to 50 microns; (ii) a second lapping step, wherein the lapping medium is aluminum oxide having an average particle size of 10 μm to 20 μm; and (iii) a third lapping step, wherein the lapping medium is alumina having an average particle size of 5 microns to 10 microns.
3. The method of claim 2, wherein the grinding medium in the first grinding step has a particle size of 40 microns; (ii) the grinding medium in the second grinding step has a particle size of 12 microns; and (iii) the grinding medium in the third grinding step has a particle size of 6 microns.
4. The method according to any one of the preceding claims, wherein the polycrystalline material is selected from the group consisting of: YAG, yttria, alumina, magnesium aluminate spinel, and a combination of yttria and zirconia.
5. A method according to any one of the preceding claims, wherein the grit particles of the first polishing step are 6 microns and the grit particles of the second polishing step are 2 microns.
6. The method according to any one of claims 1 to 5, wherein the grit particles of the first polishing step are 6 microns and the grit particles of the second polishing step are 1 micron.
7. The method of any one of the preceding claims, wherein the Ra after the polishing step is less than 0.0381 μm (1.5 microinches).
8. A method according to any one of the preceding claims, wherein during the polishing step, the at least one surface is rotating and the orbital sander is stationary.
9. A method according to any one of the preceding claims, wherein the polycrystalline material is YAG.
10. The method of claim 9, wherein the density of the sintered ceramic body is about 99.56% to about 99.78% of the theoretical density of YAG.
11. The method of any one of the preceding claims, wherein the polycrystalline sintered ceramic body has a diameter of about 100 mm to about 625 mm.
12. A method according to any one of the preceding claims, wherein the sanding pad is rotated in an elliptical orbit at a rate of up to 12,000 RPM, thereby producing a shear velocity of 0.5 m / s to 5.0 m / s on the at least one surface.
13. The method of any one of the preceding claims, wherein the plurality of orbital sanders is selected from three and four.
14. The method of claim 13, wherein the plurality of orbital sanders is three.
15. The method of claim 13, wherein the plurality of orbital sanders is four.
16. The method of any of the preceding claims, wherein the sintered ceramic body comprising polycrystalline material has an average hardness of 13.0 GPa to 16.0 GPa as measured according to ASTM Standard C1327, calculated from eight test repetitions using an applied load of 0.2 kgf.
17. A polycrystalline sintered ceramic body comprising at least 99.99% YAG and having at least one upper surface, said at least one upper surface having a surface area greater than 400 square inches, said surface having an absolute spherometer measurement greater than 15 microns over four quadrants of the disk, and an Ra and Rz less than or equal to 2 microinches each over said surface area, and a porosity less than 0.045% over said surface area, wherein the sintered ceramic disk has a thickness of at least 20 mm.
18. A polishing device, comprising: a plate comprising a plurality of elliptical vibrating orbital sanders, each of the orbital sanders comprising a polishing pad; and A rotatable table adapted to rotate a part to be polished, wherein the plate remains stationary during polishing while the part rotates on the table, and wherein the orbital sander is mounted on the plate so that the polishing pad faces the rotatable table.