Method for preparing positive electrode active material
By preparing a mixed metal composition and contacting it with water to form a solution, adding salts of nickel, cobalt, and manganese and reacting them with an alkaline solution to form a precipitate, and then adding a lithium compound and heat-treating it, the problem of recycling the positive electrode active material of waste lithium-ion batteries was solved, and the regeneration of high-performance positive electrode active material was achieved, exhibiting battery performance comparable to that of new materials.
Patent Information
- Application Number
- CN202380022153.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-12
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-01
AI Technical Summary
The lack of effective methods for recycling and reusing active materials from spent lithium-ion batteries in existing technologies leads to resource waste and poor performance.
A high-performance positive electrode active material is formed by preparing a mixed metal composition, contacting it with water to form a solution, adding salts of nickel, cobalt, and manganese and reacting them with an alkaline solution to form a precipitate, then adding a lithium compound and heat-treating it.
The prepared positive electrode active material exhibits excellent battery performance, including high discharge capacity and good cycle life, even exceeding the performance of batteries using the new material.
Smart Images

Figure CN118891231A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 341,270 filed on May 12, 2022 and U.S. Provisional Patent Application No. 63 / 311,535 filed on February 18, 2022, and all rights arising therefrom under 35 U.S.C. § 119, the contents of both of which are incorporated herein by reference in their entirety. Background Art
[0003] Lithium-ion batteries have become a popular power source in a variety of applications including consumer electronics and electric vehicles. Millions of batteries have been produced. Despite this, there remains a need for improved methods of recycling and reusing spent batteries. It would be particularly advantageous to provide improved methods for preparing positive active materials for new batteries from materials other than new raw materials. Summary of the invention
[0004] One aspect of the present disclosure is a method for preparing a cathode active material, the method comprising: contacting a mixed metal composition with water to form a first solution, the mixed metal composition comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof, based on the total weight of the mixed metal composition; adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; combining the second solution and an alkaline solution to form a precipitate; adding a lithium compound to the precipitate to form a mixture; and heat treating the mixture to form a cathode active material.
[0005] Another aspect is a positive electrode active material comprising: a first layered Li x MO2 phase; and a second phase; wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0<x<1.4; and the second phase is derived from recycled raw materials.
[0006] On the other hand is a positive electrode active material comprising: a first phase; and a second phase; wherein the first phase comprises a first domian having a formula of Li2MnO3 and a second domian having a formula of LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof; and the second phase is derived from recycled raw materials.
[0007] Another aspect is a method for preparing a purified mixed-metal composition, the method comprising: contacting a mixed-metal composition comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof based on the total weight of the mixed-metal composition; with water to form a first solution; adding a salt of the nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; combining the second solution with an alkaline solution to form a precipitate, the precipitate comprising the purified mixed-metal composition.
[0008] On the other hand is a purified mixed metal composition comprising Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125; and one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li or a combination thereof.
[0009] The above described and other features are exemplified by the following figures and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The following figures represent exemplary embodiments.
[0011] Figure 1A A scanning electron microscope (SEM) image of a precursor positive active material prepared according to Comparative Example 1 is shown. The scale bar is 5 μm.
[0012] Figure 1B Shown is a SEM image of the positive electrode active material prepared according to Comparative Example 1 after calcination at 750° C. under oxygen. The scale bar is 5 μm.
[0013] Figure 2A Shown is a SEM image of a precursor positive active material prepared according to Example 1. The scale bar is 5 μm.
[0014] Figure 2B Shown is a SEM image of the positive electrode active material prepared according to Example 1 after calcination at 750° C. under oxygen. The scale bar is 5 μm.
[0015] Figure 3A Shown is a SEM image of a precursor positive active material prepared according to Example 3. The scale bar is 5 μm.
[0016] Figure 3B Shown is a SEM image of the positive electrode active material prepared according to Example 3 after calcination at 750° C. under oxygen. The scale bar is 5 μm.
[0017] Figure 4AA SEM image of the precursor positive electrode active material prepared according to Example 4 is shown. Figure 4A The scale bar in is 5 μm.
[0018] Figure 4B A SEM image of the precursor positive electrode active material prepared according to Example 4 is shown. Figure 4B The scale bar in the figure is 20 μm.
[0019] Figure 4C An SEM image of the positive active material prepared according to Example 4 after calcination at 750° C. under oxygen is shown. Figure 4C The scale bar in is 5 μm.
[0020] Figure 4D An SEM image of the positive active material prepared according to Example 4 after calcination at 750° C. under oxygen is shown. Figure 4D The scale bar in the figure is 20 μm.
[0021] Figure 5 is a graph of discharge capacity (mAh / g) versus cycle number for half cells containing the positive electrode active materials according to Comparative Examples 1 and 2 and Examples 1 to 4. The inset is an enlarged view.
[0022] Fig. 6A The C / 3 discharge capacity (mAh / g) of Comparative Examples 1 and 2 and Examples 1 to 4 after charging to 4.2V is shown.
[0023] Figure 6B The C / 3 discharge capacity (mAh / g) of Comparative Examples 1 and 2 and Examples 1 to 4 after charging to 4.5V is shown.
[0024] Figure 7 is a graph of the discharge capacity (mAh / g) versus cycle number for Comparative Examples 1 and 2 and Examples 1 to 4 when cycled at a C / 3 charge / discharge rate.
[0025] Figure 8 is a graph showing the discharge capacity versus cycle number for the full cell cycle life of Comparative Example 1 (circles), Examples 1 (triangles) and 3 (diamonds) when charged and discharged at a C / 3 rate.
[0026] 9A to 9F Each is an area specific impedance (ohm-cm) showing the impedance analysis results at cycles 7, 53 and 99 of Comparative Example 1 (circles) and Examples 1 (diamonds) and 3 (inverted triangles). 2 )Relative volume (V relative to Li / Li + ). DETAILED DESCRIPTION
[0027] The inventors have discovered methods for remanufacturing batteries and battery materials, particularly positive active materials and precursors thereof. Despite utilizing a high percentage of raw materials derived from exhausted batteries or battery manufacturing waste, positive active materials prepared according to the methods described herein advantageously exhibit comparable or improved battery performance. While not wishing to be bound by theory, it is believed that the positive active materials prepared according to the methods include phases resulting from recycled raw materials, resulting in the observed improved capacity.
[0028] Therefore, one aspect of the present disclosure is a method for preparing a positive electrode active material from a mixed metal composition. In one aspect, the mixed metal composition comprises a mixed metal sulfate, a mixed metal nitrate, a mixed metal carbonate, a mixed metal halide, a mixed metal hydroxide, a mixed metal oxalate, or a combination thereof. In a specific aspect, the mixed metal composition comprises a mixed metal sulfate.
[0029] The mixed metal composition comprises nickel, cobalt, manganese, aluminum or a combination thereof. For example, the mixed metal composition may preferably comprise nickel and cobalt. Based on the gross weight of the mixed metal composition, the mixed metal composition may further comprise a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li or a combination thereof of greater than 0wt% to 2wt%. For example, the mixed metal composition may comprise a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li or a combination thereof of greater than 0 to 1.5 weight percent, or greater than 0.0001 to 1 weight percent, or greater than 0.001 to 0.5 weight percent, or greater than 0 to 0.1 weight percent, or greater than 0 to 0.01 weight percent (100 ppm). In one aspect, the mixed metal composition can include greater than 0 to 1000 ppm, or greater than 0 to 750 ppm, or 5 to 750 ppm, or 5 to 1000 ppm, or 25 to 1000 ppm, or 25 to 750 ppm, or 50 to 750 ppm, or 100 to 750 ppm of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof. For example, the mixed metal composition can include 50 to 300 ppm of Cu, 50 to 200 ppm of Al, 5 to 100 ppm of Fe, and 5 to 100 ppm of F, each based on the total weight of the mixed metal composition. In one aspect, the mixed metal composition can include lithium. When present, lithium can preferably be present in the mixed metal composition in an amount of 100 to 1000 ppm based on the total weight of the mixed metal composition.
[0030] In one aspect, the mixed-metal composition can include nickel and cobalt, and greater than 0 to 2 weight percent of Cu, Fe, Mg, F, Si, or a combination thereof, based on the total weight of the mixed-metal composition.
[0031] Mixed metal compositions can be obtained, for example, from depleted lithium ion batteries, lithium ion battery production waste, etc., or a combination thereof. For example, a portion or all of the mixed metal composition can be obtained from recycled raw materials, preferably post-industrial recycled raw materials, post-consumer recycled raw materials, or a combination thereof. In one aspect, Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof is derived from recycled raw materials, such as depleted batteries or battery manufacturing waste. Depleted lithium ion batteries (or any of the aforementioned lithium ion battery component sources) can be crushed, granulated, shredded, etc., and subjected to a physical separation process to separate solid battery components (e.g., housings, electrodes, etc.) from volatile components (e.g., electrolyte solvents). Electrolyte salts (e.g., LiPF6) can be removed by soaking in a suitable solvent (e.g., propylene carbonate), and the remaining undissolved materials (e.g., electrode materials, current collectors) can be separated, for example, by filtration. The electrode particles can be separated from the residual current collector by, for example, contact with a solvent suitable for dissolving the electrode particles, facilitating the removal of the solid metal conductor component. The separated electrode particles can be contacted with a leaching solution to extract elements such as Ni, Co, Mn, Al, Li and Fe. Exemplary leaching solutions may include, but are not limited to, sulfuric acid (e.g., 2 to 5M), optionally including hydrogen peroxide. The resulting solution may be centrifuged or filtered to remove any particles and subjected to conditions that effectively induce crystallization or precipitation of the desired mixed metal composition. For example, the filtered solution may be concentrated (e.g., in an evaporator) at 75°C to 85°C, or 78°C to 82°C, or 80°C. The concentrated solution may be cooled to a temperature, for example, less than 20°C, or 10-18°C, or 15°C to crystallize the mixed metal composition.
[0032] The precipitated or recrystallized mixed metal composition can be isolated, for example, using filtration, centrifugation, or the like, or a combination thereof. In one aspect, the mixed metal composition can be dehydrated to a moisture content of 10% or less, such as 1% to 10%, or 5% to 10%.
[0033] The mixed metal composition is contacted with water to form a first solution. The first solution can have a pH effective to dissolve the mixed metal composition, which can be selected by one skilled in the art without undue experimentation. In one aspect, the first solution can have a pH of less than 7, such as less than 6.5. For example, when the mixed metal composition comprises a mixed metal hydroxide, an acidic pH may be preferred to ensure dissolution of the mixed metal hydroxide.
[0034] The method further includes adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution. In one aspect, the aforementioned salt can be a raw material (i.e., not recovered or reused from a depleted lithium-ion battery). In one aspect, a salt of nickel, cobalt, manganese, aluminum, or a combination thereof is a sulfate or hydroxide thereof (e.g., nickel sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, nickel hydroxide, cobalt hydroxide, manganese hydroxide, aluminum hydroxide, or a combination thereof). In one aspect, the salt includes NiSO4, CoSO4, MnSO4, Al2(SO4)3, or a combination thereof.
[0035] Salts may be added in an amount effective to achieve the desired stoichiometry of nickel, cobalt, manganese, aluminum, or a combination thereof. For example, salts of nickel, cobalt, and manganese may be added to the first solution in an amount effective to provide a molar ratio of Ni:Co:Mn greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, such as 0.1 to 1: 0.1 to 1: 0.1 to 1, or 0.7 to 0.9: 0.05 to 0.15: 0.05 to 0.15. In one aspect, salts may be added to provide a Ni:Co:Mn molar ratio of 6:2:2. In one aspect, salts may be added to provide a Ni:Co:Mn molar ratio of 8:1:1 (e.g., 1:0.125:0.125).
[0036] The mixed metal composition of the first solution (e.g., recovered or reused from a depleted lithium-ion battery or manufacturing waste) can be contacted with the original salt in any amount to provide a stoichiometrically adjusted mixed metal composition. In one aspect, the mixed metal composition (i.e., of the first solution) can account for 10 to 95 weight percent of the stoichiometrically adjusted mixed metal composition of the second solution. Within this range, the mixed metal composition can account for 15 to 95 weight percent, or 20 to 95 weight percent, or 25 to 95 weight percent, or 30 to 90 weight percent of the stoichiometrically adjusted mixed metal composition.
[0037] In one aspect, the salt comprises NiSO4, CoSO4, Al2(SO4)3, or a combination thereof. In one aspect, salts of nickel, cobalt, and aluminum can be added to the first solution in an amount effective to provide a molar ratio of Ni:Co:Al greater than 0 to 1: greater than 0 to 1, such as 0.1 to 1: 0.1 to 0.5: 0.01 to 0.5, or 0.7 to 0.9: 0.05 to 0.15: 0.01 to 0.15. In one aspect, salts can be added to provide a Ni:Co:Al molar ratio of 0.8: 0.15: 0.05. In a specific aspect, the first solution can comprise Ni and Co, and salts comprising NiSO4, CoSO4, or a combination thereof can be added to provide a desired Ni:Co ratio. Separately, a first solution comprising Al can be provided, and Al2(SO4)3 can be added. The first solution comprising Ni and Co (after adjusting the stoichiometry) can then be combined with a solution comprising Al (after adding Al2(SO4)3) to provide a stoichiometrically adjusted mixed-metal composition comprising Ni, Co, and Al.
[0038] In one aspect, the salt comprises NiSO4, MnSO4, CoSO4, Al2(SO4)3, or a combination thereof. In one aspect, salts of nickel, cobalt, aluminum, and manganese may be added to the first solution in an amount effective to provide a molar ratio of Ni:Mn:Co:Al of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, such as 0.1 to 1: 0.1 to 0.5: 0.1 to 0.5: 0.01 to 0.5, or 0.7 to 0.9: 0.05 to 0.15: 0.05 to 0.15: 0.01 to 0.15. In one aspect, the salt may be added to provide a molar ratio of Ni:Mn:Co:Al of 0.8: 0.05: 0.05: 0.1.
[0039] The second solution may have a pH that is the same as or different from the pH of the first solution. In one aspect, the pH of the second solution may be less than 7 or less than 6.5. As described above, the salt is added to achieve the desired stoichiometry of nickel, cobalt, manganese, aluminum, or a combination thereof for the mixed metal composition of the second solution.
[0040] In addition to the stoichiometrically adjusted mixed metal composition, the second solution may further include 0.0001 to 2 weight percent of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof, based on the total weight of the stoichiometrically adjusted mixed metal composition. In other words, the aforementioned constituents of the mixed metal composition (e.g., Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof) are not removed and therefore remain present in the second solution. It should be noted that these constituents are not added to the first solution or the second solution. Instead, they are present at the beginning of the process and are derived from a mixed metal feedstock, such as recycled batteries or battery waste used in the process of the present disclosure.
[0041] The method further comprises combining the second solution with an alkaline solution to form a precipitate. In one aspect, an alkaline solution can be added to the second solution. In one aspect, the second solution is preferably added to the alkaline solution to form a precipitate. The alkaline solution is combined with the second solution in an amount that effectively maintains or provides a pH greater than or equal to 10, preferably 10-13, more preferably 11-12. In one aspect, no precipitate is produced or separated from the second solution at a pH less than 10. In one aspect, the combination of the alkaline solution and the second solution can be accompanied by stirring, for example at a speed of 500-1500RPM at a temperature of 25°C to 90°C.
[0042] The alkaline solution is preferably an aqueous alkaline solution and thus may include a suitable base in water. The base may include, for example, an alkali metal hydroxide, ammonia, or a combination thereof. In one aspect, the alkaline solution includes an alkali metal hydroxide (e.g., sodium hydroxide) and ammonia. When used in combination, the molar ratio of the alkali metal hydroxide to ammonia may be, for example, 2:1 to 1:2, 3:2 to 2:3, 1.04:1 to 1:1.04, preferably 1.01:1 to 1:1.01. In a specific aspect, the molar ratio of the alkali metal hydroxide to ammonia may be 1:1.
[0043] The combination of the alkaline solution and the second solution can co-precipitate a purified mixed metal composition having a desired ratio of, for example, Ni, Co, and Mn, which for simplicity is referred to herein as a "precipitate". For example, the precipitate can contain Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 6:2:2, 8:1:1 (1:0.125:0.125), or 9:0.5:0.5. The material precipitate can further include 5 to 100 ppm Li, such as 10 to 25 ppm Li, based on the total weight of the precipitate.
[0044] In one aspect, the combination of the alkaline solution and the second solution can coprecipitate a precursor positive electrode active material having a desired ratio of, for example, Ni, Co, and Al. For example, the precipitate can contain Ni(OH)2, Co(OH)2, and Al(OH)3, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 6:2:2, 8:1:1 (1:0.125:0.125), or 9:0.5:0.5. Based on the total weight of the precipitate, the precipitate can further include 5 to 100 ppm Li, such as 10 to 25 ppm Li.
[0045] In one aspect, the combination of the alkaline solution and the second solution can co-precipitate a purified mixed metal composition having a desired ratio of, for example, Ni, Mn, Co, and Al. For example, the precipitate can include Ni(OH)2, Mn(OH)2, Co(OH)2, and Al(OH)3, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1: greater than 0 to 1. The precipitate can further include 5 to 100 ppm Li, for example 10 to 25 ppm Li, based on the total weight of the precipitate.
[0046] Optionally, a chelating agent may be added to the second solution. When a chelating agent is added, it may be added to the second solution before, during, or after the addition of the alkaline solution. Exemplary chelating agents may include, but are not limited to, 5-sulfosalicylic acid. When present, the chelating agent may be added in an amount effective to provide a concentration of 0.1 to 10 M in the second solution.
[0047] In one aspect, the method may further include separating the precipitate. The separation may use any liquid-solid separation technique, including, for example, filtration, centrifugation, etc., or a combination thereof. The precipitate may be washed (e.g., with deionized water, distilled water, etc., or a combination thereof) and dried (e.g., in nitrogen at a temperature of 80 to 100° C., e.g., 85 to 95° C.).
[0048] The method further includes adding a lithium compound to the precipitate to form a lithiated precursor mixture (also referred to herein as a "mixture" for simplicity) and heat treating the precursor mixture under conditions effective to provide a positive electrode active material. Exemplary lithium compounds may include lithium hydroxide, lithium carbonate, lithium oxide, lithium oxalate, or a combination thereof. In one aspect, the lithium compound may include lithium hydroxide. Heat treating the mixture may include sintering at a temperature of 600 to 1000°C, 650 to 900°C, or 700 to 800°C for 2 to 24 hours.
[0049] In one aspect, the positive electrode active material may include a xIn one aspect, 0≤x≤1.1.
[0050] In one aspect, the positive electrode active material may be in a form corresponding to Formula 2: Li x Ni y Co z Mn v The amount of O2 includes Ni, Co, Mn, Al, or a combination thereof, wherein 0≤x≤1.4 and 0≤(y+z+v)≤1.1. In one aspect, 0≤x≤1.1. In one aspect, the resulting positive active material may include Li x Ni 0.6 Co 0.2 Mn 0.2 , Li x Ni 0.8 Co 0.1 Mn 0.1 , or Li x Ni 0.9 Co 0.5 Mn 0.5 , of which 0.9 <x<1.1。
[0051] In one aspect, the positive electrode active material may include Ni, Co, Mn, Al, or a combination thereof in an amount corresponding to Formula 3: mLi2MnO3·(1-m)LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0<m<1. For example, 0.2≤m≤0.5, or 0.33<m<0.5. In one aspect, M may be Ni, Co, and Mn. In one aspect, the ratio of Ni:Co:Mn may be greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.33:0.33 (ie, 6:2:2). In another aspect, M may be Ni, Co, and Al. In one aspect, the ratio of Ni:Co:Al may be greater than 0 to 1: greater than 0 to 1: greater than 0 to 1: preferably 1:0.056:0.056 (ie, 90:5:5).
[0052] For example, in a specific aspect, the positive electrode active material may include 0.33Li2MnO3·0.66LiNi 0.6 Co 0.2 Mn 0.2 O2.
[0053] Other positive electrode active materials may be obtained according to the methods described herein using alternative cell chemistries, alternative composition stoichiometries, or both.
[0054] Positive electrode active materials prepared according to the methods described herein represent another aspect of the present disclosure.
[0055] For example, in one aspect, the positive electrode active material may include a first layered Li x MO2 phase; and a second phase; wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0.9<x<1.4; and the second phase is derived from recycled raw materials. In one aspect, 0.9<x<1.1. For example, the second phase may include a compound containing one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof. In one aspect, the second phase derived from recycled raw materials is one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li, or a combination thereof. In one aspect, based on the total weight of the positive electrode active material, the second phase derived from the recycled raw material is present in an amount of 0.01 to 10 weight percent (wt%), 0.1 to 5 wt%, or 0.2 to 2 wt%.
[0056] In one aspect, the positive electrode active material may include layered Li x MO2 phase, wherein M is Ni, Co, Mn, Al, or a combination thereof and 0.9<x<1.4, and further comprises one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, and Li, which may be derived from recycled raw materials. In one aspect, 0.9<x<1.1.
[0057] In one aspect, the positive electrode active material may include a first phase and a second phase. The first phase may include a first phase domain having a formula of Li2MnO3 and a second phase domain having a formula of LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof. The second phase may be derived from recycled raw materials. For example, the second phase may include a compound containing one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof. In one aspect, the second phase derived from recycled raw materials is one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li, or a combination thereof. In one aspect, based on the gross weight of the positive electrode active material, the second phase derived from the recycled raw material is present in an amount of 0.01 to 10 weight percent (wt%), 0.1 to 5wt%, or 0.2 to 2wt%.
[0058] The positive active material of the present disclosure can exhibit one or more advantageous properties. For example, for a half-cell, the positive active material can have a discharge capacity of greater than 200 mAh / g at a discharge rate of C / 3 in 100 cycles. In one aspect, for a full cell, the positive active material can have a discharge capacity of greater than 180 mAh / g at a rate of C / 3 within 100 cycles. These and other advantageous features are further described in the working examples below.
[0059] The positive electrode active material obtained by the method described herein can be particularly useful in the positive electrode of the battery. Therefore, the positive electrode of the battery may include a positive electrode active material manufactured by the method described herein, optionally in combination with an original positive electrode active material (i.e., a positive electrode active material prepared without using recycled raw materials). For example, the positive electrode active material of the present disclosure and the original positive electrode active material can be combined in a weight ratio of 1:99 to 99:1, or 10:90 to 90:10, or 20:80 to 80:20, or 30:70 to 70:30, or 40:60 to 60:40, or 45:55 to 55:45, or 50:50.
[0060] It may further be desirable to provide a purified mixed metal composition, such as a precursor positive active material that has not been contacted with lithium to provide a final positive active material. Thus, methods of preparing a purified mixed metal composition (ie, a precursor positive active material) represent another aspect of the present disclosure.
[0061] The method of preparing a purified mixed-metal composition includes contacting the mixed-metal composition with water to form a first solution. The method also includes adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution, and combining the second solution with an alkaline solution to form a precipitate containing the purified mixed-metal composition. The mixed-metal composition, the first solution, the second solution, the alkaline solution, the precipitate, and the various conditions for performing the contacting, adding, and combining steps can be as described above.
[0062] As described in detail above, the precipitate comprising the purified mixed metal composition can be separated, washed, and dried. In one aspect, the mixed metal composition can include Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 6:2:2, 8:1:1 (1:0.125:0.125), or 9:0.5:0.5. In one aspect, the mixed metal composition can include Ni(OH)2, Co(OH)2, and Al(OH)3. In one aspect, the mixed metal composition can include Ni(OH)2, Co(OH)2, Mn(OH)2, and Al(OH)3. The precipitate can further include compounds containing one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li, or a combination thereof. In one aspect, the precipitate can further include one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li, or a combination thereof. For example, the precipitate can further include 5 to 100 ppm Li, such as 10 to 25 ppm Li, based on the total weight of the precipitated purified mixed-metal composition. The precipitated purified mixed-metal composition can optionally further include one or more of 50 to 300 ppm Cu, 50 to 200 ppm Al, 5 to 100 ppm Fe, and 5 to 100 ppm F, each based on the total weight of the mixed-metal composition.
[0063] The present disclosure is further illustrated by the following examples, which are non-limiting.
[0064] Example
[0065] Comparative Example 1
[0066] A metal sulfate solution (MSO4) was prepared using battery grade starting materials having a concentration of 2 moles per liter (M) and a stoichiometric ratio of Ni:Mn:Co of 8:1:1. The impurities of each raw material are shown in Table 1.
[0067] Table 1
[0068] Sulfate Precursors <![CDATA[NiSO4·6H2O]]> <![CDATA[MnSO4·H2O]]> <![CDATA[CoSO4·7H2O]]> Ca ≤0.005% NA NA Co ≤0.002% NA >20.7% Cu ≤0.005% NA NA Fe ≤0.001% NA <50ppm K ≤0.01% NA NA Mg ≤0.005% NA NA Mn ≤0.002% >31.5% NA Na ≤0.05% NA NA Pb NA <4ppm <50ppm Se NA <0.003% NA Ni >22.2% NA <500ppm
[0069] “NA” means data not available.
[0070] NH3 solution (5M) and NaOH solution (2M) are fed separately as chelating agent and precipitation agent respectively. 0.75M NH3 solution is loaded into 3L continuous stirred tank reactor (CSTR), and metal sulfate solution (MSO4), NH3 and NaOH are added together subsequently. The flow rate of MSO4 and NH3 feed is maintained at 0.108L / h and 0.083L / h respectively, so that the ratio of NH3 / M remains constant at 1.92. The NaOH addition rate is also kept constant at 0.108L / h to promote continuous precipitation. After 48-50 hours, the system reaches a steady state, and all reagent concentrations are constant at this moment. The reactor temperature is maintained at 50 ℃, and the stirring speed is 1085RPM. By adjusting the metal and NH3 / NaOH feed, the solution pH is kept constant at 11.3. The solution is subjected to continuous purging of N2 and covering solution to prevent transition metal oxidation.
[0071] After the reaction reached steady state, the precipitate was filtered and washed with water. To ensure the removal of any remaining sulfate ions or metal impurity ions on the surface of the precipitate, the conductivity of the filtrate solution was monitored until it was significantly below 400 S / cm. The filtered wet cake was then dried at 90°C under a N2 flow. The physical properties (tapped density, particle size distribution, and surface morphology) of the precursor positive active material (pCAM) are shown below.
[0072] A positive electrode active material (CAM) was prepared from the pCAM of Comparative Example 1 by mixing crushed pCAM and lithium hydroxide monohydrate in a molar ratio of 1:1.05, followed by high-temperature calcination under an oxygen flow. The mixing was performed using a LABRAM sonic mixer, and the ramp rate of the furnace temperature was 2°C / min until T1 = 750°C was reached. The residence time was 12 hours. After cooling, the CAM was crushed and sieved using a 350 mesh sieve. The CAM prepared from the pCAM of Comparative Example 1 was analyzed using a scanning electron microscope (SEM), as shown in FIG. Figure 1A and 1B Analysis by ICP-OES is consistent with the 8:1:1 Ni:Co:Mn ratio provided in Table 3.
[0073] Comparative Example 2
[0074] The positive active material was prepared using the same materials and steps as in Comparative Example 1, except that a temperature T1 of 800° C. was used during the CAM synthesis.
[0075] Example 1
[0076] A metal sulfate solution (MSO4) having a 2M concentration and a stoichiometric ratio of Ni:Mn:Co of 8:1:1 was prepared with 30 wt% of recycled mixed metal sulfate and 70 wt% of battery grade starting materials (i.e., NiSO4, CoSO4, and MnSO4). The recycled mixed metal sulfate (MMS) contained 20 wt% Ni and 0.86 wt% Co and trace impurities (e.g., Al, Cu). The composition components of the recycled mixed metal sulfate are shown in Table 2.
[0077] Table 2
[0078]
[0079]
[0080] A precursor positive active material (pCAM) was prepared from the composition of Example 1 using the same method as described in Comparative Example 1, except that 30 wt% of mixed metal sulfate (MMS) was used in the metal feed solution. The positive active material (CAM) was prepared from the pCAM of Example 1 by mixing the crushed pCAM with lithium hydroxide monohydrate in a molar ratio of 1:1.05, followed by high-temperature calcination under an oxygen flow. The mixing was carried out using a LABRAM sonic mixer, and the gradual ramp rate of the furnace temperature was 2°C / min until 750°C was reached. The residence time at 750°C was 12 hours. After cooling, the CAM was crushed and screened using a 350 mesh sieve. The CAM prepared from the pCAM of Example 1 was analyzed using a scanning electron microscope (SEM), as shown. Figure 2A and 2B The analysis by ICP-OES was consistent with the 8:1:1 Ni:Co:Mn ratio provided in Table 3.
[0081] Example 2
[0082] The positive active material was prepared using the same materials and steps as in Example 1, except that a temperature T1 of 800° C. was used during the CAM synthesis.
[0083] Example 3
[0084] A metal sulfate solution (MSO4) having a concentration of 2M and a stoichiometric ratio of Ni:Mn:Co of 8:1:1 was prepared using 60 wt% of recycled mixed metal sulfate and 30 wt% of battery grade feedstock (i.e., NiSO4, MnSO4, CoSO4). pCAM and CAM were made using the same method as in Example 1, except that 60 wt% of mixed metal sulfate (MMS) was used in the metal feed solution. The CAM prepared from the pCAM of Example 3 was analyzed using scanning electron microscopy (SEM), as shown in FIG. Figure 3Aand 3B Analysis by ICP-OES is consistent with the 8:1:1 Ni:Co:Mn ratio provided in Table 3.
[0085] Example 4
[0086] A metal sulfate solution (MSO4) having a 2M concentration and a stoichiometric ratio of Ni:Mn:Co of 8:1:1 was prepared using 90 wt% of recycled mixed metal sulfate and 10 wt% of battery grade starting materials. pCAM and CAM were made using the same method as in Example 1, except that 90 wt% of mixed metal sulfate (MMS) was used in the metal feed solution. The CAM prepared from the pCAM of Example 4 was analyzed using scanning electron microscopy (SEM), as shown in FIG. Figures 4A-4D As shown, it shows comparable pCAM and CAM morphology and size distribution compared to Comparative Example 1.
[0087] The physical properties of pCAM and CAM according to Comparative Example 1 and Examples 1 and 3 and the results of ICP analysis are summarized in Table 3. "CE" is used to designate Comparative Examples, and "E" is used to designate Examples.
[0088] Table 3
[0089] unit CE1 E1 E3 pCAM tap density g / cc 1.93 1.91 1.913 pCAM D10 μm 6.5 8.7 7.85 pCAM D50 μm 14.3 17.1 13.61 pCAM D90 μm 27.6 30.92 20.44 ICP determination (mol%) %Ni:%Mn:%Co 79.7:10:10.3 80:9.9:10.1 78:11:11
[0090] Electrode preparation
[0091] CAM powder was mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a ratio of 84:8:8 by weight. The slurry rheology was adjusted with NMP and the mixture was mixed using a THINKY mixer. The slurry was cast on Al foil using a 254 micron (μm) doctor blade, followed by rapid drying at 75°C to remove the NMP solvent. The cast film was then further dried at 100°C under vacuum to promote PVDF curing and complete NMP removal. Button half cells (CR2025) with Li metal anodes and button full cells with graphite anodes were assembled and tested using a MACCOR tester.
[0092] Rate performance test
[0093] The half-cell was charged using a constant current / constant voltage (CC-CV) scheme at a constant charge current of C / 10 until it reached 4.2 V, followed by a constant voltage charge until the charge current dropped to C / 20. Figure 5 As shown, in cycles 1-15, the battery is discharged at different C rates, where the discharge cut-off voltage is 2.5 V. The C rate is defined using the discharge capacity at the C / 10 rate. The C rate refers to the current that discharges the battery in one hour, for example, the C rate of a battery with a discharge capacity of 1 ampere-hour is 1 ampere.
[0094] A similar charging scheme was used for cycles 16-30, except that a charge cutoff voltage of 4.5 V was used. Figure 5 As shown, the positive electrode active material made from recycled raw materials (e.g., Example 4 providing 215 mAh / g at a C / 10 rate) provides a greater capacity than the material made from battery-grade low-impurity raw materials (e.g., Comparative Example 1 providing 200 mAh / g at a C / 10 rate). Figure 5 The results shown in indicate that positive electrode active materials made from recycled raw materials can provide similar or improved discharge capacities relative to those made from battery-grade low-impurity raw materials.
[0095] It was also observed that the pCAM calcination temperature affected the electrochemical performance. Figure 5 As shown, samples calcined at 800°C (Comparative Example 2 and Example 2) exhibit lower discharge capacity than samples calcined at 750°C (Comparative Example 1 and Example 1, respectively). Without wishing to be bound by theory, it is believed that excessive sintering of primary particles at high temperatures and Li loss may lead to the observed reduced capacity when higher calcination temperatures are used. Surface reconstruction of the CAM surface may also lead to a reduction in capacity.
[0096] Fig. 6A A comparison of the discharge capacity at a C / 3 rate at a charge cutoff voltage of 4.2 V is shown, and Figure 6B A comparison of discharge capacity at C / 3 rate at a charge cutoff voltage of 4.5V is shown. For the positive active material prepared from recycled MMS, higher discharge capacity was observed at a cutoff voltage of 4.2V. When a cutoff voltage of 4.5V was used, greater discharge capacity was observed with increasing amount of recycled MMS. Higher capacity was observed when a cutoff voltage of 4.5V was used, and statistically significant high discharge capacity was observed when high content of MMS (e.g., 90wt%) was used in the preparation of pCAM and CAM materials. These results suggest that using recycled MMS in the metal feed solution to make pCAM and CAM can be advantageous in terms of electrochemical performance (e.g., rate capability and discharge capacity).
[0097] Half battery cycle life
[0098] The cycle life performance of the button cell was evaluated according to the test procedure described in J. Electrochem. Soc., 163 (2016) A2999, the contents of which are incorporated herein by reference in their entirety. To further distinguish the cycle life performance, a three-hour constant voltage charge was added to each cycle to simulate accelerated aging. The half-cell includes Li metal as the anode. Figure 7It is shown that the capacity does not change significantly over the course of 100 cycles at C / 3 rate. This result indicates that the performance of cathode materials made from recycled MMS can be comparable to cathode materials made from virgin battery grade materials.
[0099] Full battery cycle life and hybrid pulse power characteristics (HPPC)
[0100] To better evaluate the performance of the positive electrode, a full coin cell with a graphite negative electrode was fabricated. Figure 8 The full cell cycle life of Comparative Example 1 (circles), Examples 1 (triangles) and 3 (diamonds) is shown, and when charged and discharged at a C / 3 rate, the discharge capacity does not change significantly over 100 or more cycles.
[0101] HPPC testing with charge and discharge cycles was performed after every twenty C / 3 cycles. Low cell impedance is preferred because impedance growth can negatively affect charge and discharge efficiency. FIG. 9 shows that cells made with recycled MMS have low area specific impedance (ASI) over both charge and discharge cycles in the HPPC test. A lower ASI indicates potentially good extended cycle performance.
[0102] The present invention further encompasses the following aspects.
[0103] Aspect 1: A method for manufacturing a positive active material, the method comprising: contacting a mixed metal composition with water to form a first solution, the mixed metal composition comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of a compound based on the total weight of the mixed metal composition, the compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof; adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; combining the second solution and an alkaline solution to form a precipitate; adding a lithium compound to the precipitate to form a mixture; and heat treating the mixture to form a positive active material.
[0104] Aspect 2: The method of aspect 1, wherein the mixed metal composition is obtained by a method comprising: contacting electrode particles comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof, based on the total weight of the mixed metal composition; with a leaching solution, which preferably comprises sulfuric acid; precipitating the mixed metal composition from the leaching solution; and separating the mixed metal composition from the leaching solution.
[0105] Aspect 3: The method of aspect 1 or 2, wherein the mixed metal composition comprises mixed metal sulfates, mixed metal nitrates, mixed metal carbonates, mixed metal halides, mixed metal hydroxides, mixed metal oxalates, or combinations thereof.
[0106] Aspect 4: The method of any of Aspects 1 to 3, wherein the mixed metal composition comprises mixed metal sulfates.
[0107] Aspect 5: The method of any one of Aspects 1 to 4, wherein the mixed metal composition comprises: nickel and cobalt, and greater than 0 to 2 weight percent of Cu, Fe, Mg, F, or a combination thereof based on the total weight of the mixed metal composition.
[0108] Aspect 6: The method of any one of Aspects 1 to 5, wherein the mixed metal composition further comprises lithium, preferably in an amount of 100 to 1000 ppm based on the total weight of the mixed metal composition.
[0109] Aspect 7: The method of any one of Aspects 1 to 6, wherein the mixed metal composition is obtained from a recycled feedstock, preferably a post-industrial recycled feedstock, a post-consumer recycled feedstock, or a combination thereof.
[0110] Aspect 8: The method of any one of Aspects 1 to 7, wherein the mixed metal composition comprises 50 to 300 ppm Cu, 50 to 200 ppm Al, 5 to 100 ppm Fe, and 5 to 100 ppm F, each based on the total weight of the mixed metal composition.
[0111] Aspect 9: The method of any one of Aspects 1 to 8, wherein the first solution has a pH of less than 7 or less than 6.5.
[0112] Aspect 10: The method of any one of Aspects 1 to 9, wherein the salt of nickel, cobalt, manganese, aluminum, or a combination thereof is a sulfate or hydroxide thereof.
[0113] Aspect 11: The method of any of Aspects 1 to 10, wherein the mixed metal composition comprises nickel, cobalt and manganese, and the method comprises adding salts of nickel, cobalt and manganese to the first solution in an amount effective to provide a molar ratio of Ni:Co:Mn of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125.
[0114] Aspect 12: The method of Aspect 11, wherein the salt comprises NiSO4, CoSO4, and MnSO4.
[0115] Aspect 13: The method of any one of Aspects 1 to 12, wherein the second solution has a pH of less than 7 or less than 6.5.
[0116] Aspect 14: The method of any one of Aspects 1 to 13, wherein the second solution comprises 0.0001 to 2 weight percent of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof based on the total weight of the solution.
[0117] Aspect 15: The method of any one of Aspects 1 to 14, wherein the alkaline solution comprises a base, the base comprising an alkali metal hydroxide, ammonia, or a combination thereof, preferably sodium hydroxide and ammonia, more preferably wherein the sodium hydroxide and ammonia are present in a ratio of 1.04:1 to 1:1.04, preferably 1.01:1 to 1:1.01, more preferably 1:1.
[0118] Aspect 16: The method of any one of Aspects 1 to 15, wherein the alkaline solution is combined with the second solution in an amount effective to provide a pH greater than or equal to 10, preferably 10-13, more preferably 11-12.
[0119] Aspect 17: The method of any one of Aspects 1 to 16, wherein no precipitate separates from the second solution at a pH of less than 10.
[0120] Aspect 18: The method of any one of aspects 1 to 17, further comprising adding a chelating agent to the second solution, preferably wherein the chelating agent is present in the second solution in an amount of 0.1 to 10M.
[0121] Aspect 19: The method of any one of Aspects 1 to 18, wherein the precipitate comprises Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125.
[0122] Aspect 20: The method of any one of Aspects 1 to 19, wherein the precipitate comprises 5 ppm to 100 ppm of Li, preferably 10 ppm to 25 ppm of Li, based on the total weight of the precipitate.
[0123] Aspect 21: The method of any one of Aspects 1 to 20, wherein the lithium compound comprises lithium hydroxide, lithium carbonate, lithium oxide, lithium oxalate, or a combination thereof.
[0124] Aspect 22: The method of any one of aspects 1 to 21, wherein the positive electrode active material includes a x MO2 has an amount of Ni, Co, Mn, Al, or a combination thereof, wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0≤x≤1.4.
[0125] Aspect 23: The method of Aspect 22, wherein 0≤x≤1.1.
[0126] Aspect 24: The method of any one of Aspects 1 to 23, wherein the positive electrode active material includes a x Ni y Co z Mn vThe amount of Ni, Co, Mn, Al, or a combination thereof in an amount of O2, wherein 0≤x≤1.4 and 0≤(y+z+v)≤1.1.
[0127] Aspect 25: The method of Aspect 23, wherein 0≤x≤1.1.
[0128] Aspect 26: The method of any one of Aspects 1 to 25, wherein the positive electrode active material comprises LiNi 0.8 Co 0.1 Mn 0.1 .
[0129] Aspect 27: The method of any one of Aspects 1 to 21, wherein the positive electrode active material includes Ni, Co, Mn, Al or a combination thereof in an amount corresponding to Formula 3: mLi2MnO3·(1-m)LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof; and 0<m<1.
[0130] Aspect 28: The method of Aspect 27, wherein 0.2 <m<0.5。
[0131] Aspect 29: The method of any one of Aspects 27 and 28, wherein M is Ni, Co, and Mn.
[0132] Aspect 30: The method of any one of Aspects 27 to 29, wherein the ratio of Ni:Co:Mn is greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 6:2:2.
[0133] Aspect 31: The method of any one of Aspects 27 and 28, wherein M is Ni, Co, and Al.
[0134] Aspect 32: The method of any one of Aspects 27, 28 and 31, wherein the ratio of Ni:Co:Al is greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 90:5:5.
[0135] Aspect 33: The method of aspect 27, wherein the positive electrode active material comprises 0.33Li2MnO3·0.66LiNi 0.6 Co 0.2 Mn 0.2 O2.
[0136] Aspect 34: The method of any one of Aspects 1 to 33, wherein the heat treatment comprises sintering at a temperature of 600 to 1000° C. for 2 to 24 hours.
[0137] Aspect 35: The method of any one of Aspects 1 to 34, further comprising stirring the second solution at a temperature of 25 to 90°C at a speed of 500-1500 RPM.
[0138] Aspect 36: The method of any one of Aspects 1 to 35, further comprising separating the precipitate.
[0139] Aspect 37: The method of any one of Aspects 1 to 36, further comprising combining the positive electrode active material with a raw positive electrode active material.
[0140] Aspect 38: The method of Aspect 37, wherein the positive electrode active material and the original positive electrode active material are combined in a weight ratio of 1:99 to 99:1.
[0141] Aspect 39: A positive electrode active material produced by the method according to any one of Aspects 1 to 38.
[0142] Aspect 40: A positive electrode active material comprising: a first layered Li x MO2 phase; and a second phase; wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0<x<1.4; and the second phase is derived from recycled raw materials.
[0143] Aspect 41: The positive electrode active material of Aspect 40, wherein 0 <x<1.1。
[0144] Aspect 42: The positive electrode active material of Aspect 40 or 41, wherein the second phase comprises one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
[0145] Aspect 43: The positive electrode active material of any one of Aspects 40 to 42, wherein the second phase is derived from recycled raw materials and is present in an amount of 1 wt % to 99 wt % based on the total weight of the positive electrode active material.
[0146] Aspect 44: A positive electrode active material comprising: a first layered phase including Li x MO2, wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0<x<1.4; and wherein the first layered phase further comprises Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
[0147] Aspect 45: The positive electrode active material of Aspect 44, wherein 0 <x<1.1。
[0148] Aspect 46: The positive electrode active material of Aspect 44 or 45, wherein Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof is derived from recycled raw materials.
[0149] Aspect 47: The positive electrode active material of any one of Aspects 40 to 46, wherein the positive electrode active material has a discharge capacity of greater than 200 mAh / g at a discharge rate of C / 3 for a half cell in 100 cycles.
[0150] Aspect 48: The cathode active material of any one of Aspects 40 to 47, wherein the cathode active material has a discharge capacity of greater than 180 mAh / g at a rate of C / 3 for a half cell in 100 cycles.
[0151] Aspect 49: A positive electrode active material comprising: a first phase; and a second phase; wherein the first phase comprises a first phase domain having a formula of Li2MnO3 and a second phase domain having a formula of LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof; and the second phase is derived from recycled raw materials.
[0152] Aspect 50: The positive electrode active material of Aspect 49, wherein the second phase comprises one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
[0153] Aspect 51: The positive electrode active material of Aspect 49, wherein the first phase is derived from recycled raw materials.
[0154] Aspect 52: A method for making a purified mixed-metal composition, the method comprising: contacting a mixed-metal composition comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof based on the total weight of the mixed-metal composition; with water to form a first solution; adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; combining the second solution with an alkaline solution to form a precipitate, the precipitate comprising a purified mixed-metal composition.
[0155] Aspect 53: The method of Aspect 52, wherein the mixed metal composition is obtained by a method comprising: contacting electrode particles comprising nickel, cobalt, manganese, aluminum, or a combination thereof; and greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof based on the total weight of the mixed metal composition; with a leaching solution, the leaching solution preferably comprising sulfuric acid; precipitating the mixed metal composition from the leaching solution; and separating the mixed metal composition from the leaching solution.
[0156] Aspect 54: The method of Aspect 52 or 53, wherein the purified mixed metal composition comprises 5 ppm to 100 ppm Li, preferably 10 ppm to 25 ppm Li, based on the total weight of the precipitate.
[0157] Aspect 55: The method of any one of Aspects 52 to 54, wherein the mixed metal composition comprises a mixed metal sulfate, a mixed metal nitrate, a mixed metal carbonate, a mixed metal halide, a mixed metal hydroxide, a mixed metal oxalate, or a combination thereof, preferably a mixed metal sulfate.
[0158] Aspect 56: The method of any one of Aspects 52 to 55, wherein the mixed metal composition is obtained from a recycled feedstock, preferably a post-industrial recycled feedstock, a post-consumer recycled feedstock, or a combination thereof.
[0159] Aspect 57: The method of any of Aspects 52 to 56, wherein the mixed metal composition comprises 50 to 300 ppm Cu, 50 to 200 ppm Al, 5 to 100 ppm Fe, and 5 to 100 ppm F, each based on the total weight of the mixed metal composition.
[0160] Aspect 58: The method of any one of Aspects 52 to 57, wherein the first solution has a pH of less than 7 or less than 6.5.
[0161] Aspect 59: The method of any one of Aspects 52 to 58, wherein the salt of nickel, cobalt, manganese, aluminum, or a combination thereof is a sulfate or hydroxide thereof.
[0162] Aspect 60: The method of any of Aspects 52 to 59, wherein the mixed metal composition comprises nickel, cobalt, and manganese, and the method comprises adding salts of nickel, cobalt, and manganese to the first solution in an amount effective to provide a molar ratio of Ni:Co:Mn of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125.
[0163] Aspect 61: The method of any one of Aspects 52 to 60, wherein the second solution has a pH of less than 7 or less than 6.5.
[0164] Aspect 62: The method of any one of Aspects 52 to 61, wherein the alkaline solution comprises a base, the base comprising an alkali metal hydroxide, ammonia, or a combination thereof, preferably sodium hydroxide and ammonia, more preferably wherein the sodium hydroxide and ammonia are present in a ratio of 1.04:1 to 1:1.04, preferably 1.01:1 to 1:1.01, more preferably 1:1.
[0165] Aspect 63: The method of any one of Aspects 52 to 62, wherein the alkaline solution is combined with the second solution in an amount effective to provide a pH greater than or equal to 10, preferably 10-13, more preferably 11-12.
[0166] Aspect 64: The method of any one of Aspects 52 to 63, wherein no precipitate separates from the second solution at a pH of less than 10.
[0167] Aspect 65: The method of any one of Aspects 52 to 64, further comprising adding a chelating agent to the second solution, preferably, wherein the chelating agent is present in the second solution in an amount of 0.1 to 10 M.
[0168] Aspect 66: The method of any one of Aspects 52 to 65, wherein the purified mixed metal composition comprises Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125.
[0169] Aspect 67: A purified mixed metal composition prepared by the method of any one of Aspects 52 to 66.
[0170] Aspect 68: A purified mixed metal composition comprising: Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125; and one or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li, or a combination thereof.
[0171] Aspect 69: The purified mixed-metal composition of Aspect 68, comprising 5 to 100 ppm Li, preferably 10 to 25 ppm Li, based on the total weight of the precipitate.
[0172] Alternatively, the compositions and methods may include, consist of, or consist essentially of any suitable material, step, or component disclosed herein. The compositions and methods may additionally or alternatively be formulated to be free of or essentially free of any material (or substance), step, or component that is otherwise unnecessary for achieving the function or purpose of the compositions, methods, and articles.
[0173] All ranges disclosed herein include endpoints, and endpoints can be combined independently of each other. "Combination" includes blends, mixtures, alloys, reaction products, etc. The terms "first", "second", etc. do not represent any order, quantity, or importance, but are used to distinguish one element from another. Unless otherwise indicated in this article or clearly contradictory to the context, the terms "one" and "a kind of" and "the" do not represent the limitation of quantity, but are interpreted as covering the singular and plural. Unless otherwise clearly stated, "or" means "and / or". Throughout the specification, mentioning "an aspect" means that the specific elements described in conjunction with this aspect are included in at least one aspect described herein and may or may not be present in other aspects. The term "their combination" as used in this article includes one or more listed elements, and is open, allowing one or more unnamed similar elements to exist. In addition, it should be understood that the described elements can be combined in any suitable manner in various aspects.
[0174] It should be further understood that when the terms "comprises" and / or "comprising" or "includes" or "including" are used in this specification, they specify the presence of stated features, regions, integers, steps, operations, elements, or parts, but do not exclude the presence or addition of one or more other features, regions, integers, steps, operations, elements, parts, or combinations thereof.
[0175] Various aspects are shown in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the aspects set forth herein. Instead, these aspects are provided so that this disclosure will be thorough and complete and will fully convey the scope of the invention to those skilled in the art. The same reference numerals represent the same elements throughout.
[0176] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and the present disclosure, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.
[0177] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 311,535 filed on February 18, 2022 and U.S. Provisional Patent Application No. 63 / 341,270 filed on May 12, 2022, which are incorporated herein by reference in their entirety for all purposes.
[0178] While certain aspects have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not presently foreseeable or may not be foreseeable may occur to the applicant or others skilled in the art. Accordingly, the appended claims as filed and as they may be amended are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.
Claims
1. A method for manufacturing a positive electrode active material, the method comprising: contacting a mixed metal composition with water to form a first solution, the mixed metal composition comprising: Nickel, cobalt, manganese, aluminum or combinations thereof; as well as greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or combinations thereof, based on the total weight of the mixed-metal composition; adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; combining the second solution and an alkaline solution to form a precipitate; adding a lithium compound to the precipitate to form a mixture; as well as The mixture is heat treated to form the positive electrode active material.
2. The method according to claim 1, wherein: The mixed metal composition is obtained by the following method, the method comprising Contacting electrode particles with a leaching solution, the electrode particles comprising Nickel, cobalt, manganese, aluminum or combinations thereof; and greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or combinations thereof, based on the total weight of the mixed-metal composition; precipitating the mixed metal composition from the leach solution; as well as The mixed metal composition is separated from the leach solution.
3. The method according to claim 1, wherein: The mixed metal composition includes mixed metal sulfates, mixed metal nitrates, mixed metal carbonates, mixed metal halides, mixed metal hydroxides, mixed metal oxalates, or combinations thereof.
4. The method according to claim 1, wherein: The mixed metal composition comprises: Nickel and cobalt, and Greater than 0 to 2 weight percent of Cu, Fe, Mg, F, or a combination thereof based on the total weight of the mixed metal composition.
5. The method according to claim 1, wherein: The mixed metal composition further comprises lithium, 50 to 300 ppm Cu, 50 to 200 ppm Al, 5 to 100 ppm Fe, or 5 to 100 ppm F, each based on the total weight of the mixed metal composition.
6. The method according to claim 1, wherein: At least a portion of the mixed metal composition is obtained from recycled raw materials.
7. The method according to claim 1, wherein: The first solution has a pH of less than 7, or wherein the second solution has a pH of less than 7.
8. The method according to claim 1, wherein: The salt of nickel, cobalt, manganese, aluminum or a combination thereof is sulfate or hydroxide thereof.
9. The method according to claim 1, wherein: The mixed metal composition comprises nickel, cobalt and manganese, and the method comprises adding salts of nickel, cobalt and manganese to the first solution in amounts effective to provide a molar ratio of Ni:Co:Mn of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.
125.
10. The method according to claim 1, wherein: The alkaline solution is combined with the second solution in an amount effective to provide a pH greater than or equal to 10, preferably 10-13, more preferably 11-12.
11. The method according to claim 1, wherein: The precipitate comprises Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.
125.
12. The method according to claim 1, wherein: The precipitate contains 5 ppm to 100 ppm of Li, preferably 10 ppm to 25 ppm of Li, based on the total weight of the precipitate.
13. The method according to claim 1, wherein: The lithium compound includes lithium hydroxide, lithium carbonate, lithium oxide, lithium oxalate, or a combination thereof.
14. The method according to claim 1, wherein: The positive electrode active material comprises a material corresponding to Formula 1: Li x The amount of Ni, Co, Mn, Al, or their combination in MO2: wherein M is Ni, Co, Mn, Al, or a combination thereof, and 0≤x≤1.
4.
15. The method according to claim 1, wherein: The positive electrode active material comprises a material corresponding to Formula 2: Li x Ni y Co z Mn v O2 content of Ni, Co, Mn, Al, or a combination thereof: Among them, 0≤x≤1.4 and 0≤(y+z+v)≤1.
1.
16. The method according to claim 1, wherein: The positive electrode active material comprises Ni, Co, Mn, Al, or a combination thereof in an amount corresponding to Formula 3: mLi2MnO3·(1-m)LiMO2: in, M is Ni, Co, Mn, Al, or a combination thereof; and 0<m<1。 17. The method according to claim 1, wherein: The positive electrode active material includes 0.33Li2MnO3·0.66LiNi 0.6 Co 0.2 Mn 0.2 O2.
18. The method of claim 1, further comprising combining the positive electrode active material with a pristine positive electrode active material.
19. A positive electrode active material produced by the method according to any one of claims 1 to 18.
20. A positive electrode active material comprising: The first layer Li x MO2 phase; and Phase II; in, M is Ni, Co, Mn, Al, or a combination thereof, and 0<x<1.4; and The second phase originates from recycled raw materials.
21. The positive electrode active material according to claim 20, wherein The second phase includes one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
22. A positive electrode active material comprising: Contains Li x The first layered phase of MO2, in, M is Ni, Co, Mn, Al, or a combination thereof, and 0<x<1.4; and Wherein, the first layered phase further comprises Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
23. The positive electrode active material according to claim 21 or 22, wherein Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof is derived from recycled raw materials.
24. A positive electrode active material comprising: Phase 1; and Phase II; in, The first phase comprises a first phase domain of formula Li2MnO3 and a second phase domain of formula LiMO2, wherein M is Ni, Co, Mn, Al, or a combination thereof; and The second phase originates from recycled raw materials.
25. The positive electrode active material according to claim 24, wherein The second phase includes one or more of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or a combination thereof.
26. A method of preparing a purified mixed metal composition, the method comprising: contacting a mixed metal composition with water to form a first solution, the mixed metal composition comprising: Nickel, cobalt, manganese, aluminum or combinations thereof; as well as greater than 0 to 2 weight percent of Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or combinations thereof based on the total weight of the mixed-metal composition; adding a salt of nickel, cobalt, manganese, aluminum, or a combination thereof to the first solution to provide a second solution; The second solution is combined with an alkaline solution to form a precipitate comprising the purified mixed-metal composition.
27. The method according to claim 26, wherein: The mixed metal composition is obtained by the following method, the method comprising Contacting electrode particles with a leaching solution, the electrode particles comprising Nickel, cobalt, manganese, aluminum or combinations thereof; and greater than 0 to 2 weight percent of a compound comprising Cu, Fe, Mg, Na, Ca, Zn, F, Si, Li, or combinations thereof, based on the total weight of the mixed-metal composition; precipitating the mixed metal composition from the leach solution; as well as The mixed metal composition is separated from the leach solution.
28. The method according to claim 26, wherein: The mixed metal composition comprises mixed metal sulfates, mixed metal nitrates, mixed metal carbonates, mixed metal halides, mixed metal hydroxides, mixed metal oxalates, or combinations thereof, preferably mixed metal sulfates.
29. The method according to claim 26, wherein: The mixed metal composition is obtained from a recycled feedstock, preferably a post-industrial recycled feedstock, a post-consumer recycled feedstock, or a combination thereof.
30. The method of claim 26, wherein: The mixed metal composition includes 50 to 300 ppm Cu, 50 to 200 ppm Al, 5 to 100 ppm Fe, or 5 to 100 ppm F, each based on the total weight of the mixed metal composition.
31. The method of claim 26, wherein: The salt of nickel, cobalt, manganese, aluminum or a combination thereof is sulfate or hydroxide thereof.
32. The method of claim 26, wherein: The mixed metal composition comprises nickel, cobalt and manganese, and the method comprises adding salts of nickel, cobalt and manganese to the first solution in amounts effective to provide a molar ratio of Ni:Co:Mn of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.
125.
33. The method of claim 26, wherein: The purified mixed metal composition comprises Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.
125.
34. A purified mixed metal composition produced by the method of any one of claims 26 to 33.
35. A purified mixed-metal composition comprising: Ni(OH)2, Co(OH)2, and Mn(OH)2, preferably in a molar ratio of greater than 0 to 1: greater than 0 to 1: greater than 0 to 1, preferably 1:0.125:0.125; and One or more of Cu, Fe, Mg, Na, Ca, Zn, Al, F, Si, Li or a combination thereof.