Ebullated bed or mixed ebullated bed hydroconversion of feedstocks comprising plastic pyrolysis oil and / or solid recovered fuel fractions

By hydrogenating the fossil-based heavy hydrocarbon raw materials in boiling beds or mixed boiling-entrained beds, adding plastic pyrolytic oil and solid recovery of fuel pyrolytic oil fractions, the catalyst deactivation and blockage problems are solved, and efficient Improve quality of fuel base materials and chemical products.

CN118891343APending Publication Date: 2024-11-01IFP ENERGIES NOUVELLES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380028342.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art faces catalyst deactivation and blockage problems when dealing with plastic pyrolytic oil containing high impurities and solid recovery fuel pyrolytic oil, and it is difficult to effectively improve quality, affecting the production of fuel base materials and chemical products.

Method used

The fossil-based heavy hydrocarbon raw materials are hydrogenated in boiling beds or mixed boiling-entrained beds, and a small amount of plastic pyrolysis oil and solid recovery fuel pyrolysis oil fractions are added, and the hydrogenation conversion is carried out using porous supported catalysts, fractionation and Rehydrogenation is rehydrogenated to produce high-quality fuel bases and other enhanced hydrocarbons.

Benefits of technology

Effectively remove impurities in pyrolytic oil, prolong the circulation time of the hydrogenation conversion unit, improve the yield of fuel base and chemical products, maintain the stability of the fraction, and reduce the risk of catalyst deactivation and blockage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891343A_ABST
    Figure CN118891343A_ABST
Patent Text Reader

Abstract

The invention relates to a process for the hydroconversion of a feedstock comprising less than 50% by weight of a plastic and / or SRF pyrolysis oil fraction (102) and a heavy hydrocarbon fraction (101) comprising at least 50% by weight of a fraction having a boiling point of at least 300 DEG C, and comprising sulfur and nitrogen. The hydroconversion uses one or more ebullated beds or mixed ebullated-entrained bed reactors (20), and preferably two consecutive hydroconversion steps. According to the process of the present invention, materials of higher quality, lower boiling point can be produced, for example, for the production of fuels or compounds for the petrochemical industry, and the yield of certain fractions is increased while promoting the treatment of hydroconversion products in downstream steps, such as fixed bed hydrotreatment, and maintaining good stability of the unconverted fractions.
Need to check novelty before this filing date? Find Prior Art

Description

Prior art

[0003] Over the past few years, several approaches have emerged in the fuel and chemical industries in which products other than traditional petroleum products, such as renewable source products (such as vegetable and animal oils) or oils from waste materials (such as plastics or waste oils) are introduced as a supplement or replacement for fossil source products.

[0004] In particular, plastics from the collection and sorting industry can be subjected to a pyrolysis step to obtain, among other things, pyrolysis oils. These plastic pyrolysis oils are usually incinerated to generate electricity and / or used as fuel for industrial boilers or city heating boilers.

[0005] Solid recovered fuel (SRF), also known as refuse derived fuel (RDF), is solid non-hazardous waste prepared for energy recovery, whether they come from household and similar waste, from economic activity waste or from demolition waste. SRF is usually a mixture of any combustible waste, such as old tires, food by-products (fat, animal meat meal, etc.), viscose and wood waste, light fractions from shredders (e.g. from old vehicles, electrical and electronic equipment (WEEE)), household and commercial waste, residues from the recycling of various types of waste, including some municipal waste, plastic waste, textiles or wood, etc. SRF usually contains plastic waste. Nowadays, SRF is mainly used as energy upgrading. They can be used directly as a fossil fuel substitute in co-incineration facilities (coal and lignite power stations, cement plants, lime kilns) or household waste incineration units, or indirectly in pyrolysis units dedicated to energy upgrading: SRF pyrolysis oil is therefore usually burned to generate electricity, or even used as a fuel in industrial boilers or city heating boilers.

[0006] Plastic pyrolysis oil and SRF pyrolysis oil can also be upgraded through refining processes to produce fuels such as gasoline or diesel and / or chemicals such as olefins for the production of various polymers in the chemical industry.

[0007] However, this other approach to upgrading plastic pyrolysis oils and SRF pyrolysis oils faces problems arising from the specific composition of these oils, in particular the impurities they contain, which composition itself is related to the diversity of the components of the plastic waste or SRF.

[0008] Specifically, plastic waste or SRF is usually a mixture of several polymers, such as a mixture of polyethylene, polypropylene, polyethylene terephthalate, polyvinyl chloride and polystyrene. In addition, depending on the use, plastics may contain other compounds in addition to polymers, such as plasticizers, pigments, dyes or polymerization catalyst residues, as well as other very diverse organic and inorganic impurities from the separation operation of the sorting centers, which may not be completely selective.

[0009] Therefore, the oil obtained from plastic pyrolysis or SRF pyrolysis usually contains a large amount of dienes and impurities, in particular metals, silicon or halogenated compounds, especially chlorine-based compounds, heteroelements (such as sulfur, oxygen and nitrogen), insolubles, whose content is usually high and may be incompatible with certain refining units, such as fixed-bed hydroprocessing units.

[0010] The handling of these oils can cause operability problems, in particular problems of corrosion, coking or catalyst deactivation, or incompatibility problems in the use of the target polymer. The presence of dienes, for example, often causes instability problems of the pyrolysis oils, which instability is characterized by the formation of gums. Gums and insolubles that may be present in pyrolysis oils can cause plugging problems in equipment items.

[0011] For example, patent application WO2018 / 055555 proposes an overall process for recycling plastic waste, which is very versatile and relatively complex, comprising a step of actual pyrolysis of the plastic waste, and a step of steam cracking, which can produce products that can be highly upgraded in the petrochemical field, such as olefins and aromatics. The process notably comprises a step of hydrocracking of the liquid phase directly produced by the pyrolysis, preferably in a fixed bed.

[0012] Patent applications FR3107530, FR3113060 and FR3113061 describe methods for treating plastic pyrolysis oils, which in particular comprise a selective hydrogenation step of the plastic pyrolysis oils and a fixed-bed hydrotreatment of the hydrogenation effluent. The naphtha fraction produced after a specific separation of the hydrotreated effluent with water and a fractionation of the separated hydrocarbon stream can be conveyed to a steam cracker or used as a fuel base. According to patent applications FR3113060 and FR3113061, the method incorporates, after the hydrotreatment step, one or two hydrocracking steps in a fixed bed in order to convert the heavy fraction at least partially into a naphtha fraction by hydrocracking, thereby minimizing the yield of the heavy fraction and maximizing the yield of naphtha, which is the fraction that is usually favorable to the steam cracking unit.

[0013] Due to the impurity content in plastic pyrolysis oils, especially when their impurity content is high, catalyst deactivation can be observed in hydroprocessing units operating as fixed beds, which shortens the cycle time. In fact, the main limiting factor of fixed bed units is the fact that the unit must be shut down for catalyst replacement. In addition, plastic pyrolysis oils, especially those containing large amounts of dienes and impurities, can cause plugging problems, especially in preheating furnaces, feed / effluent heat exchangers or at the top of the bed in fixed bed catalytic reactors.

[0014] Unpublished patent application FR20 / 09750 describes a method for treating plastic pyrolysis oil and / or SRF pyrolysis oil, which comprises in particular subjecting a feedstock, optionally prehydrogenated, to ebullated-bed, entrained-bed and / or moving-bed hydroconversion. The feedstock contains at least 50% by weight of plastic pyrolysis oil and / or SRF pyrolysis oil, preferably consisting of plastic pyrolysis oil and / or SRF pyrolysis oil. After successive steps of separation with water, fractionation of a separated hydrocarbon-based stream, hydrotreatment of a 385°C fraction and fractionation of the hydrotreated stream, a liquid effluent suitable for a steam cracking unit is obtained. The use of an ebullated-bed, entrained-bed and / or moving-bed hydroconversion step allows the cycle time of the hydroconversion unit to be extended, since in such units a system is generally used to add fresh catalyst and remove spent catalyst without stopping the unit. This compensates for possible catalyst deactivation due to feedstock impurities, unlike fixed-bed reactors, where clogging of the catalyst bed is a problem. Furthermore, this hydroconversion step upstream of the hydroprocessing allows the hydroprocessing unit cycle time to be extended by partially conducting the hydroprocessing reactions upstream of the hydroconversion unit, and the hydroprocessing is also made simpler since at least a portion of the heavy compounds are converted to lighter compounds during the hydroconversion process.

[0015] Unpublished patent application FR21 / 04873 describes a process for treating plastic pyrolysis oil and / or SRF pyrolysis oil similar to the process of patent application FR20 / 09750, wherein in particular there is no separation step between the hydroconversion step and the hydrotreatment step.

[0016] Unpublished patent application FR21 / 04874 describes a method for simultaneously treating plastic pyrolysis oil and raw materials from renewable resources (e.g. vegetable oils), which is similar to the method of patent application 21 / 04873, wherein the plastic pyrolysis oil (optionally pre-hydrogenated) is sent to a hydrodemetallization step and the demetallized effluent is then sent to a hydrotreatment step. The hydrodemetallization step and the hydrotreatment step can be carried out in an ebullating bed. The raw materials from renewable resources are fed to the hydrogenation step and / or the hydrodemetallization step and / or the hydrotreatment step.

[0017] Subject Matter and Summary of the Invention

[0018] The present invention is in the field of upgrading heavy feedstocks that are difficult to upgrade, such as petroleum residues, which usually contain high levels of impurities, such as metals, sulfur, nitrogen, Conradson carbon and asphaltenes, with the aim of converting them into lighter products that can be upgraded to fuels, such as for the production of gasoline or gas oil, or feedstocks for the petrochemical industry.

[0019] The inventors have demonstrated in a surprising manner that small amounts of impure plastic pyrolysis oil and / or SRF pyrolysis oil fractions can be added to fossil-based heavy hydrocarbon feedstocks (usually vacuum residues) that are conventionally processed in an ebullating bed or mixed ebullating-entrained bed hydroconversion process, thereby increasing the yield of fuel bases and / or other upgradable hydrocarbons, while at the same time scavenging impurities, such as silicon, originally present in the pyrolysis oil in the supported catalyst of the hydroconversion step, thereby making the product in downstream steps (such as fixed bed hydroprocessing) easier to handle, while maintaining good stability of the unconverted fraction.

[0020] Therefore, the present invention proposes a method for hydroconversion of fossil-based heavy hydrocarbon feedstocks (especially vacuum residue type feedstocks) in an ebullating bed or a mixed ebullating-entrained bed, wherein the feedstock contains a small amount of plastic pyrolysis oil and / or SRF pyrolysis oil fractions, so that fuel base materials and other upgradable hydrocarbons can be produced, thereby achieving the upgrading of the fractions.

[0021] Therefore, in order to overcome the problems existing in the above-mentioned prior art and achieve at least one of the above-mentioned objectives, according to a first aspect, the present invention proposes a method for hydrogenating and converting a feedstock, wherein the feedstock comprises a plastic pyrolysis oil and / or a solid recovered fuel pyrolysis oil fraction and a fossil-based heavy hydrocarbon fraction containing at least 50% by weight of a portion having a boiling point of at least 300° C., and contains sulfur and nitrogen, wherein the pyrolysis oil fraction accounts for less than 50% by weight of the feedstock, and the method comprises:

[0022] (a) conditioning the feedstock and introducing it into a first hydroconversion stage, the first hydroconversion stage comprising at least a first ebullated bed or mixed ebullated-entrained bed hydroconversion reactor, the reactor containing a first porous supported hydroconversion catalyst;

[0023] (b) a first step of hydroconverting the feedstock in the presence of hydrogen in the first hydroconversion section to obtain a first hydroconversion effluent;

[0024] (c) optionally, a step of separating a portion or all of said first effluent produced by step (b) to form at least one heavy fraction boiling primarily at a temperature greater than or equal to 350° C.;

[0025] (d) optionally, a second hydroconversion step of part or all of the first effluent produced by step (b) or optionally the heavy fraction produced by step (c) in a second hydroconversion section comprising at least a second ebullated bed or mixed ebullated-entrained bed hydroconversion reactor, the second hydroconversion reactor comprising a second porous supported catalyst and operated in the presence of hydrogen, to produce a second hydroconversion effluent;

[0026] Step (b) and optional step (d) are carried out at an absolute pressure of 2 MPa to 38 MPa, at a temperature of 300° C. to 550° C., at a temperature of 0.05 h -1 Until 10h -1 At the hourly space velocity and at 50Nm 3 / m 3 Up to 5000Nm 3 / m 3 The hydrogen amount is 2.

[0027] (e) a step of fractionating a portion or all of the first hydroconversion effluent from step (b) or a portion or all of the second hydroconversion effluent from step (d) in a fractionation section to produce at least one heavy liquid product boiling primarily at a temperature greater than or equal to 350° C., the heavy liquid product containing a residual oil fraction having a boiling point greater than or equal to 540° C.

[0028] According to one or more embodiments of the present invention, in step (a), the pyrolysis oil fraction and the heavy hydrocarbon fraction of the feedstock are premixed before being introduced into the at least one first hydroconversion reactor of the first hydroconversion stage.

[0029] According to one or more embodiments of the present invention, in step (a), the pyrolysis oil fraction and the heavy hydrocarbon fraction of the feedstock are separately introduced into the at least one first hydroconversion reactor of the first hydroconversion stage.

[0030] According to one or more embodiments of the present invention, step (a) comprises a step of preheating the heavy hydrocarbon fraction, preferably to a temperature of 280°C to 450°C, and optionally a step of preheating the pyrolysis oil fraction, before introducing the feedstock into the first hydroconversion reactor of the first hydroconversion stage.

[0031] According to one or more embodiments of the present invention, the pyrolysis oil fraction accounts for 1 wt% to 45 wt% of the feedstock, preferably 2 wt% to 30 wt% of the feedstock, more preferably 2 wt% to 25 wt% of the feedstock, and even more preferably 3 wt% to 20 wt% of the feedstock.

[0032] According to one or more embodiments of the present invention, the feedstock is composed of the pyrolysis oil fraction and the heavy hydrocarbon fraction, the pyrolysis oil fraction accounts for 1 weight % to 45 weight % of the feedstock, preferably 2 weight % to 30 weight %, and the heavy hydrocarbon fraction accounts for 55 weight % to 99 weight % of the feedstock, preferably 70 weight % to 98 weight %.

[0033] According to one or more embodiments of the present invention, the pyrolysis oil fraction is plastic pyrolysis oil.

[0034] According to one or more embodiments of the present invention, the heavy hydrocarbon fraction is selected from crude oil, topped crude oil, atmospheric residue or vacuum residue produced by atmospheric distillation and / or vacuum distillation of crude oil or an effluent produced from a thermal conversion unit, a hydrotreating unit, a hydrocracking unit or a hydroconversion unit, an aromatic fraction extracted from a lubricant production unit, a deasphalted oil produced from a deasphalting unit, an asphalt produced from a deasphalting unit, a residue fraction produced from direct liquefaction of coal, a vacuum distillate produced from direct liquefaction of coal, or a mixture thereof.

[0035] According to one or more embodiments of the present invention, the heavy hydrocarbon fraction is a vacuum residue, preferably a vacuum residue resulting from primary fractionation of crude oil.

[0036] According to one or more embodiments of the present invention, the method includes a separation step (c) of separating a part or all of the first hydroconversion effluent from step (b) to produce at least a heavy fraction boiling mainly at a temperature greater than or equal to 350°C, and also includes a second hydroconversion step (d) of the heavy fraction.

[0037] According to one or more embodiments of the present invention, the first hydroconversion section in step (b) and the one or more hydroconversion reactors in the optional hydroconversion step (d) are mixed boiling-entrained bed reactors, and the method also includes a step of introducing a catalyst precursor into the feedstock in a manner that forms a colloidal or molecular catalyst when the feedstock reacts with sulfur before injecting the feedstock into the at least one first mixed boiling-entrained bed reactor of the first hydroconversion section, the catalyst precursor preferably comprising molybdenum 2-ethylhexanoate, and the colloidal or molecular catalyst preferably comprising molybdenum disulfide.

[0038] According to one or more embodiments of the present invention, the first hydroconversion catalyst and the optional second hydroconversion catalyst comprise at least one Group VIII non-noble metal selected from nickel and cobalt, preferably nickel, and at least one Group VIB metal selected from molybdenum and tungsten, preferably molybdenum, and comprise an amorphous support, preferably alumina.

[0039] According to one or more embodiments of the present invention, step (b) and optional step (d) are carried out at a temperature of 405°C to 450°C.

[0040] According to one or more embodiments of the present invention, the optional intermediate separation step (c) is carried out in a separation section, and wherein the separation section and / or the fractionation section in step (e) comprises means for washing at least one separated fraction by contact with an aqueous solution.

[0041] According to one or more embodiments of the present invention, the method further includes a step (f) of further treating the heavy liquid product and / or other one or more products from the fractionation step (e), wherein the step (f) includes at least one step selected from: hydrotreating, steam cracking, fluid catalytic cracking, hydrocracking, deasphalting, lubricating oil extraction, and preferably a fixed bed hydrotreating step (f2) in a hydrotreating section, wherein the hydrotreating section preferably includes at least one fixed bed reactor, wherein the reactor includes n catalytic beds, n is an integer greater than or equal to 1, each catalytic bed contains at least one hydrotreating catalyst, and the hydrotreating section is fed with at least a portion of the liquid product from step e) and a gaseous stream containing hydrogen to obtain a hydrotreating effluent.

[0042] According to a second aspect, the present invention relates to a product obtained by the process according to the present invention.

[0043] According to one or more embodiments, the product is a hydroconversion effluent obtained at the end of the first hydroconversion step (b) or the second hydroconversion step (d) and comprises a liquid fraction having a silicon content less than or equal to 5 weight ppm and / or a chlorine content less than or equal to 10 weight ppm relative to the total weight of said liquid fraction of said effluent.

[0044] Other objects and advantages of the invention will become apparent on reading the following description of a specific exemplary embodiment of the invention, given as a non-limiting example and described with reference to the accompanying drawings listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 One embodiment of the hydroconversion process according to the present invention is schematically illustrated.

[0046] Figure 2 Another embodiment of the hydroconversion process according to the present invention is schematically illustrated.

[0047] In the drawings, the same reference numerals denote the same or similar elements.

[0048] Description of the implementation plan

[0049] Embodiments of the method according to the present invention will now be described in detail. In the detailed description hereinafter, many specific details are disclosed to deepen the understanding of the inventive method. However, it is apparent to those skilled in the art that the inventive method can be implemented without these specific details. In other cases, well-known characteristics are no longer described in detail to avoid unnecessarily complicating the description.

[0050] Some definitions are given below to facilitate a better understanding of the present invention.

[0051] In this specification, the term "include" is synonymous with "include" and "contain", and is inclusive or open, and does not exclude other unmentioned elements. It is understood that the term "include" includes the exclusive closed term "consisting of...".

[0052] In the present specification, the expression “... to ..." means that the limits of the interval are included in the described value range unless otherwise specified.

[0053] In the present invention, different ranges of values ​​for a given parameter can be used alone or in combination. For example, a preferred range of pressure values ​​can be combined with a more preferred range of temperature values, or a preferred range of values ​​for a compound or element can be combined with a more preferred range of values ​​for another compound or element.

[0054] The term "hydroconversion" refers to a process whose primary purpose is to reduce the boiling range of a feedstock and in which a significant portion of the feedstock is converted to a product having a boiling range below that of the starting feedstock, the feedstock containing at least 50% of a heavy hydrocarbon fraction having a boiling point of at least 300°C, or at least 450°C. Hydroconversion generally involves splitting larger hydrocarbon molecules to obtain smaller molecular fragments having a lower number of carbon atoms and a higher hydrogen / carbon ratio. The reactions carried out during hydroconversion can reduce the size of hydrocarbon molecules, primarily by breaking carbon-carbon bonds in the presence of hydrogen, thereby saturating the broken bonds and aromatic rings. The mechanism by which hydroconversion occurs generally involves the formation of hydrocarbon free radicals during the splitting process, primarily by thermal cracking, followed by the termination of the free radicals or fragments with hydrogen in the presence of active catalyst sites. Of course, during hydroconversion, other reactions typically associated with hydroprocessing may occur, for example, removal of sulfur or nitrogen from the feedstock, or saturation of olefins, and these reactions will be more broadly defined below.

[0055] The term "hydrotreating" (commonly referred to as "HDT") refers to a milder operation whose main purpose is to remove impurities such as sulfur, nitrogen, oxygen, halides and trace metals from the feedstock, and to saturate olefins and / or stabilize hydrocarbon free radicals by reacting them with hydrogen rather than reacting them with themselves. The main purpose is not to change the boiling range of the feedstock. Therefore, hydrotreating mainly includes hydrodesulfurization (commonly known as "HDS") reactions, hydrodenitrogenation (commonly known as "HDN") reactions, and hydrodemetallization (commonly known as "HDM") reactions, accompanied by hydrogenation, hydrodeoxygenation (commonly known as "HDO"), hydrodearomatization, hydroisomerization, hydrodealkylation, hydrocracking or hydrodeasphalting reactions and the reduction of Conradson carbon residue. Hydrotreating is usually carried out using a fixed bed reactor, but other reactors can also be used for hydrotreating, such as an ebullating bed hydrotreating reactor.

[0056] The term "hydroconversion reactor" refers to any vessel whose primary purpose is the hydroconversion of a feedstock, such as cracking (i.e., reducing the boiling range) of the feedstock in the presence of hydrogen and a hydroconversion catalyst. Hydroconversion reactors typically include at least one input port through which the feedstock and hydrogen can be introduced, and at least one output port through which the upgraded material can be removed. In particular, hydroconversion reactors are also characterized in that they have sufficient thermal energy to split larger hydrocarbon molecules into smaller molecules by thermal decomposition. Examples of hydroconversion reactors include (but are not limited to) entrained bed reactors, also known as slurry reactors (reactors with three phases of liquid, gas, and solid, in which the solid and liquid phases can appear homogeneous), ebullating bed reactors (fluidized reactors with three phases), moving bed reactors (reactors with three phases in which a solid catalyst moves downward and liquid and gas flow upward or downward) and fixed bed reactors (reactors with three phases in which a liquid feedstock trickles down over a fixed bed of supported catalyst and hydrogen usually flows in the same direction as the liquid, but in some cases can flow in countercurrent).

[0057] For a hydroconversion reactor, the terms "mixed bed", "mixed ebullating bed" and "mixed ebullating-entrained bed" refer to an ebullating bed hydroconversion reactor which, in addition to the porous supported catalyst held in the ebullating bed reactor, also contains an entrained catalyst. Similarly, for a hydroconversion process, these terms thus refer to a process comprising a mixed operation of an ebullating bed and an entrained bed in at least the same hydroconversion reactor. A mixed bed is a mixed bed of two types of catalysts, necessarily different in particle size and / or density, wherein one type of catalyst - the "porous supported catalyst" is held in the reactor, while the other type of catalyst - the "entrained catalyst", also commonly referred to as the "slurry catalyst" is entrained out of the reactor with the effluent (upgraded feedstock). In the present invention, an entrained catalyst is a colloidal catalyst or a molecular catalyst as defined below.

[0058] The terms "colloidal catalyst" and "colloidally dispersed catalyst" refer to catalyst particles having a colloidal particle size, such as a size (diameter) less than 1 μm, preferably a size less than 500 nm, more preferably a size less than 250 nm, or a size less than 100 nm, or a size less than 50 nm, or a size less than 25 nm, or a size less than 10 nm, or a size less than 5 nm. The term "colloidal catalyst" includes, but is not limited to, molecular or molecularly dispersed catalyst compounds.

[0059] The terms "molecular catalyst" and "molecularly dispersed catalyst" refer to catalyst compounds that are substantially "dissolved" or completely dissociated from other catalyst compounds or molecules in the feed, non-volatile liquid fraction, bottoms fraction, resid, or other feed or product in which the catalyst is present. They also refer to very small catalyst particles or flakes containing a few catalyst molecules linked together (e.g., 15 molecules or less).

[0060] The terms "porous supported catalyst", "solid supported catalyst" and "supported catalyst" refer to catalysts commonly used in conventional ebullating bed and fixed bed hydroconversion systems, including catalysts designed primarily for hydrocracking or hydrodemetallization and catalysts designed primarily for hydrotreating. Such catalysts typically comprise: (i) a catalyst support having a large surface area and many interconnected channels or pores; (ii) fine particles of active catalyst, such as sulfides of cobalt, nickel, tungsten or molybdenum, or mixed sulfides of these elements (e.g., NiMo, CoMo, etc.), dispersed in the pores. Supported catalysts are typically produced in the form of cylindrical extrudates (pellets) or spherical solids, but other forms may also be used.

[0061] In the following, unless otherwise specified, the term "pyrolysis oil" refers to oil obtained from pyrolysis of plastics and / or SRF. In addition, for simplicity, unless otherwise specified, the term "heavy hydrocarbon fraction" of the feedstock refers to a fossil-based heavy hydrocarbon fraction.

[0062] The method according to the invention and its implementation will be described in more detail below, with particular reference to Figure 1 and Figure 2 , Figure 1 and Figure 2 are illustrations of exemplary embodiments of the method according to the invention for a better understanding of the invention, but the invention is not limited to these examples.

[0063] The object of the present invention is to propose a process for the hydroconversion of a feedstock comprising a plastic and / or SRF pyrolysis oil fraction 102 and a fossil-based heavy hydrocarbon fraction 101 containing at least 50% by weight of a fraction having a boiling point of at least 300° C., and containing sulfur and nitrogen, the pyrolysis oil fraction representing less than 50% by weight of the feedstock, the process comprising the following steps:

[0064] (a) conditioning the feedstock and introducing it into a first hydroconversion zone 20, the first hydroconversion zone comprising at least a first ebullated bed or mixed ebullated-entrained bed hydroconversion reactor containing a first porous supported hydroconversion catalyst;

[0065] (b) a first step of hydroconverting the feedstock in the presence of hydrogen in the first hydroconversion section to obtain a first hydroconversion effluent;

[0066] (c) optionally, a step of separating a portion or all of said first effluent produced by step (b) to form at least one heavy fraction boiling primarily at a temperature greater than or equal to 350° C.;

[0067] (d) optionally, a second hydroconversion step of part or all of the first effluent produced by step (b) or optionally part or all of the heavy fraction produced by step (c) in a second hydroconversion section comprising at least a second ebullated bed or mixed ebullated-entrained bed hydroconversion reactor, the second hydroconversion reactor comprising a second porous supported catalyst and operated in the presence of hydrogen, to produce a second hydroconversion effluent;

[0068] Step (b) and optional step (d) are carried out at an absolute pressure of 2 MPa to 38 MPa, at a temperature of 300° C. to 550° C., at a temperature of 0.05 h -1 Until 10h -1 At the hourly space velocity and at 50Nm 3 / m 3 Up to 5000Nm 3 / m 3 The hydrogen amount is 2.

[0069] (e) a step of fractionating a portion or all of the first hydroconversion effluent from step (b) or a portion or all of the second hydroconversion effluent from step (d) in a fractionation section 30 to produce at least one heavy liquid product boiling primarily at a temperature greater than or equal to 350° C., the heavy liquid product containing a residual oil fraction having a boiling point greater than or equal to 540° C.

[0070] raw material

[0071] According to a basic aspect of the present invention, the feedstock mainly comprises fossil-based heavy hydrocarbon fractions and a small amount of plastic pyrolysis oil and / or SRF pyrolysis oil fractions.

[0072] According to a preferred embodiment of the present invention, the feedstock consists of the small amount of plastic pyrolysis oil and / or SRF pyrolysis oil fraction and a fossil-based heavy hydrocarbon fraction.

[0073] The process according to the invention is therefore particularly useful for the hydroconversion of mixtures of low-content plastic pyrolysis oils and / or SRF pyrolysis oils with fossil-based heavy hydrocarbon fractions.

[0074] The plastic pyrolysis oil and / or SRF pyrolysis oil fraction accounts for less than 50% by weight of the feedstock (the total weight of the feedstock), preferably 1% to 45% by weight of the feedstock, more preferably 2% to 30% by weight of the feedstock, more preferably 2% to 25% by weight of the feedstock, more preferably 3% to 20% by weight of the feedstock, more preferably 5% to 20% by weight of the feedstock, and even 5% to 15% by weight of the feedstock.

[0075] The feedstock may consist of only these two fractions: a pyrolysis oil fraction and a heavy hydrocarbon fraction, the sum of which forms 100 wt % of the feedstock. When the feedstock consists of the heavy hydrocarbon fraction and the pyrolysis oil fraction, the heavy hydrocarbon fraction may preferably account for 55 wt % to 99 wt % of the feedstock, preferably 70 wt % to 98 wt % of the feedstock, more preferably 75 wt % to 98 wt % of the feedstock, even more preferably 80 wt % to 97 wt % of the feedstock, even more preferably 80 wt % to 95 wt % of the feedstock, even more preferably 85 wt % to 95 wt % of the feedstock.

[0076] According to the invention, "plastic pyrolysis oil or SRF pyrolysis oil" is an oil, advantageously in liquid form at room temperature, obtained from the pyrolysis of plastics, preferably from the pyrolysis of plastic waste, especially from collection and sorting channels, or from the pyrolysis of SRF. It contains in particular a mixture of hydrocarbon compounds, in particular paraffins, olefins, cycloalkanes and aromatics. At least 80% by weight of these hydrocarbon compounds preferably have a boiling point below 700° C., and preferably below 550° C. In particular, depending on the source of the pyrolysis oil, the oil may contain up to 70% by weight of paraffins, up to 90% by weight of olefins and up to 90% by weight of aromatics, it being understood that the sum of paraffins, olefins and aromatics is 100% by weight of hydrocarbon compounds.

[0077] The density of pyrolysis oil measured at 15°C according to ASTM D4052 is typically 0.75 g / cm 3 Up to 0.99g / cm 3 , preferably 0.75 g / cm 3 Up to 0.95g / cm 3 .

[0078] Pyrolysis oil may contain and usually does contain impurities, such as metals, especially iron, silicon, or halides, especially chlorides. These impurities may be present in the pyrolysis oil in high levels, such as up to 500 wt ppm or even 1000 wt ppm or even 5000 wt ppm of halogen elements (such as chlorine) provided by halides (such as chlorides), up to 2500 wt ppm or even 10000 wt ppm of metal or semi-metal elements. Alkali metals, alkaline earth metals, transition metals, post-transition metals and metalloids may be classified in the same category as metallic pollutants, referred to as metals or metallic elements or semi-metal elements. Pyrolysis oil may contain up to 200 wt ppm or even 1000 wt ppm of silicon, and up to 15 wt ppm or even 100 wt ppm of iron. The pyrolysis oil may also contain other impurities, such as foreign elements, in particular foreign elements provided by sulfides, oxides and / or nitrides, the content of which is generally less than 20,000 ppm by weight of foreign elements, preferably less than 10,000 ppm by weight of foreign elements.

[0079] The method according to the invention is particularly suitable for treating a pyrolysis oil containing impurities in combination with a heavy hydrocarbon feedstock as defined in more detail below. The term "containing impurities" means that the pyrolysis oil has the following characteristics:

[0080] - the content of aromatic compounds is from 0 to 90% by weight, typically from 20 to 90% by weight, possibly from 50 to 90% by weight;

[0081] - the halide content is from 2 to 5000 ppm by weight, typically from 200 to 5000 ppm by weight, and may be from 500 to 5000 ppm by weight;

[0082] - the content of metal elements is from 10 wt ppm to 10000 wt ppm, usually from 2000 wt ppm to 10000 wt ppm, and may be from 2250 wt ppm to 5000 wt ppm;

[0083] - the content of iron is 0 wt ppm to 100 wt ppm, typically 10 wt ppm to 100 wt ppm, and may be 15 wt ppm to 100 wt ppm;

[0084] The silicon content is 0 wt ppm to 1000 wt ppm, typically 50 wt ppm to 1000 wt ppm, even 80 wt ppm or 100 wt ppm to 1000 wt ppm, possibly 200 wt ppm to 1000 wt ppm.

[0085] The method according to the invention is particularly suitable for treating a pyrolysis oil containing a large amount of impurities in combination with a heavy hydrocarbon feedstock as defined in more detail below. The term "containing a large amount of impurities" means that the pyrolysis oil has the following characteristics:

[0086] - an aromatics content of 35% to 70% by weight;

[0087] - a halide content of 500 to 5000 ppm by weight;

[0088] - The content of metal elements is 300 ppm to 5000 ppm by weight;

[0089] - The iron content is 15 ppm to 100 ppm by weight;

[0090] - The silicon content is 200 ppm to 1000 ppm by weight.

[0091] SRF pyrolysis oil and / or plastic pyrolysis oil may be obtained from a thermal pyrolysis process or a catalytic pyrolysis process or may be prepared by hydropyrolysis (pyrolysis in the presence of a catalyst and hydrogen).

[0092] The fossil based heavy hydrocarbon fraction in the feedstock of the process according to the invention is a heavy hydrocarbon fraction comprising at least 50 wt. %, preferably at least 80 wt. % of a fraction having a boiling point of at least 300°C, preferably at least 350°C, even more preferably at least 375°C.

[0093] This heavy hydrocarbon fraction in the feedstock may be crude oil, or may result from the refining of crude oil in a refinery or from the processing of other fossil hydrocarbon sources.

[0094] The heavy hydrocarbon fraction in the feedstock may be crude oil, topped crude oil, or may contain or consist of atmospheric residue or vacuum residue produced by atmospheric distillation and / or vacuum distillation of crude oil.

[0095] The heavy hydrocarbon fraction in the feedstock may also consist of an atmospheric residue or a vacuum residue produced by atmospheric and / or vacuum distillation of effluents originating from thermal conversion, hydrotreatment, hydrocracking and / or hydroconversion units.

[0096] Preferably, the heavy hydrocarbon fraction in the feedstock is a heavy hydrocarbon fraction containing at least 50 wt%, even at least 80 wt% of a portion having a boiling point of at least 450°C, preferably at least 500°C, more preferably at least 540°C, such as vacuum residue.

[0097] Advantageously, the heavy hydrocarbon fraction in the feedstock consists of one or more vacuum residues. The vacuum residue may come directly from crude oil, or from other refining units, such as hydrotreating of residue, hydrocracking of residue or visbreaking of residue, etc. Preferably, the vacuum residue is a vacuum residue from a vacuum distillation column of a primary (straight run (SR)) fractionation of crude oil.

[0098] The heavy hydrocarbon fraction in the feedstock may also consist of an aromatic fraction extracted from a lubricant production unit, deasphalted oil (also called DAO, deasphalting unit raffinate) produced from a deasphalting unit, asphalt produced from a deasphalting unit (deasphalting unit residue).

[0099] The heavy hydrocarbon fraction in the feedstock may also consist of settling oil or recycle oil (usually boiling in the range of 360°C to 550°C), such as FCC fluid catalytic cracking effluent, such as heavy cycle oil (HCO) or slurry oil (SLO).

[0100] The heavy hydrocarbon fraction in the feedstock may also be a residual oil fraction from direct coal liquefaction (e.g. atmospheric and / or vacuum residues from processes), or from direct coal liquefaction (e.g. process) under reduced pressure distillate.

[0101] All these fractions of fossil origin can be used individually or as a mixture to constitute the heavy hydrocarbon fraction of the feedstock treated according to the invention.

[0102] According to one or more embodiments, the heavy hydrocarbon fraction comprises and may consist of at least one of the following feedstocks (alone or as a mixture): crude oil, topped crude oil, atmospheric residue or vacuum residue from atmospheric distillation and / or vacuum distillation of crude oil (preferably from primary fractionation of crude oil), atmospheric residue or vacuum residue from atmospheric distillation or vacuum distillation obtained by a direct coal liquefaction process, preferably vacuum residue from vacuum distillation of crude oil (preferably from primary fractionation of crude oil).

[0103] The heavy hydrocarbon fraction of the feedstock treated according to the present invention contains impurities such as sulfur and nitrogen. It may also contain impurities such as metals, Conradson carbon and asphaltenes, particularly C7 asphaltenes which are insoluble in heptane.

[0104] The metal content may be greater than or equal to 20 ppm by weight, preferably greater than or equal to 100 ppm by weight.

[0105] The sulfur content may be greater than or equal to 0.1% by weight, or even greater than or equal to 0.5% by weight or 1% by weight, or greater than or equal to 2% by weight.

[0106] The nitrogen content is typically from 1 wt ppm to 8000 wt ppm, more typically from 200 wt ppm to 8000 wt ppm, for example from 2000 wt ppm to 8000 wt ppm.

[0107] The content of C7 asphaltenes (compounds insoluble in heptane according to the ASTM D6560 standard, also equivalent to the NFT60-115 standard) may be at least 1% by weight and generally greater than or equal to 3% by weight (except for heavy hydrocarbon fractions mainly containing DAO). C7 asphaltenes are known to be compounds that inhibit the conversion of residual oil fractions because of their ability to form heavy hydrocarbon residues (commonly known as coke) and their tendency to produce deposits that severely limit the operability of hydrotreatment and hydroconversion units.

[0108] The Conradson char content may be greater than or equal to 3% by weight, or even at least 5% by weight. The Conradson char content is defined according to the ASTM D482 standard and represents a well-known estimate for those skilled in the art of the carbon residue produced after pyrolysis under standard temperature and pressure conditions.

[0109] The contents of metals, sulfur, nitrogen, asphaltenes and Conradson carbon in the heavy hydrocarbon fraction are expressed in weight % relative to the total weight of the heavy hydrocarbon fraction of the feedstock.

[0110] According to one or more embodiments, the feedstock for the process according to the invention may also contain low amounts (typically 1 to 20 wt. %, or even 1 to 10 wt. % or 5 wt. % of the feedstock) of vegetable oils and / or animal oils or fat fractions, and / or hydrocarbon fractions resulting from thermal and / or catalytic conversion processes of lignin biomass, such as oils produced from lignin biomass according to various liquefaction processes (e.g. hydrothermal liquefaction or pyrolysis), which are then co-processed with plastic pyrolysis oils and / or SRF pyrolysis oils and fossil-based heavy hydrocarbon fractions.

[0111] The oil / fat of plant and / or animal origin contains triglyceride and / or free fatty acid and / or ester.Vegetable oil can advantageously be rough, or refined wholly or in part, and can be produced from following plant: rape, sunflower, soybean, palm, palm kernel, olive, coconut, jatropha (French jatropha), castor, cotton, groundnut, flax or sea kale, and this list is non-restrictive.Algae oil or fish oil are also applicable.The oil / fat of plant and / or animal origin can be waste oil / waste fat, for example waste cooking oil.Animal fat can be selected from lard or the fat consisting of the residue produced by food industry or catering industry.

[0112] The term "lignin biomass" refers to compounds derived from plants or their by-products, including components selected from cellulose, hemicellulose (carbohydrate polymers) and / or lignin (aromatic polymers).

[0113] According to one or more embodiments, the feedstock for the process according to the invention does not contain vegetable oils and / or animal oil or fat fractions, or hydrocarbon fractions resulting from thermal and / or catalytic conversion processes of lignin biomass (eg biomass pyrolysis oils).

[0114] (a) Step of conditioning the feedstock and injecting it into the first hydroconversion reactor

[0115] The process according to the invention comprises a step (a) of conditioning the feedstock and introducing it into a first hydroconversion stage 20 comprising at least a first ebullated-bed or mixed-bed reactor containing a first porous supported hydroconversion catalyst.

[0116] The term "conditioning the feedstock" means placing the feedstock in a state suitable for the hydroconversion step b), in particular placing it under temperature and pressure conditions suitable for hydroconversion in the first hydroconversion reactor, optionally mixing the plastic pyrolysis oil and / or SRF pyrolysis oil fraction with a heavy hydrocarbon fraction before introducing the feedstock into the reactor, and possibly removing solid particles from the plastic pyrolysis oil and / or SRF pyrolysis oil fraction (by filtration, centrifugation, electrostatic separation, washing with an aqueous solution, adsorption, etc.).

[0117] Specifically, the plastic pyrolysis oil and / or SRF pyrolysis oil fraction 102 can be pre-mixed with the heavy hydrocarbon fraction 101 in the feedstock before entering the first hydroconversion reactor in the first hydroconversion step (b). In this case, the two fractions can be pre-heated by any heating device known to those skilled in the art to ensure that they are in a liquid state before mixing. Alternatively, only the heavy hydrocarbon fraction 101 can be heated, especially if the pyrolysis oil fraction is liquid and pumpable at room temperature. Such mixing can be carried out in Figure 1 The mixing can be carried out in the dedicated container 10 shown, and for this mixing, it can be optionally active mixing (such as a pump with a rotor stirrer or an impeller), or it can be directly mixed by connecting two conduits for conveying products. In the latter case, the homogeneity of the mixture can be ensured by installing an online static mixer, which technology is also well known to those skilled in the art.

[0118] By mixing the fractions, a more uniform feedstock 114 is introduced into the first hydroconversion reactor, which is, for example, conducive to good fluidization of the catalyst and good overall fluid dynamics of the reactor. Conventional equipment, such as ovens, feedstock distributors, mixers for mixing hydrogen with the feedstock, such as T-type mixers, can also be used, which can help reduce investment costs.

[0119] Figure 2Another possibility shown is that in the first hydroconversion step (b), the plastic pyrolysis oil and / or SRF pyrolysis oil fraction 102 and the heavy hydrocarbon fraction 101 are separately injected into the first hydroconversion reactor. This injection method may be preferred in order to prevent any problems related to chemical incompatibility between the two fractions (such as the risk of phase separation or asphaltene precipitation), or to prevent possible accelerated fouling of the preheating furnace (the high content of diolefins and olefins in the plastic pyrolysis oil and / or SRF pyrolysis oil can lead to the formation of gums).

[0120] According to these two alternative embodiments, i.e., mixing or not mixing the fractions before introducing them into the first hydroconversion reactor, the feedstock, in particular the heavy hydrocarbon fraction 101 of the feedstock, is heated to a temperature suitable for hydroconversion in the first hydroconversion reactor, that is, so as to advantageously reach a target temperature in the first hydroconversion reactor. This is referred to in this specification as a preheating step. It should be noted that the target temperature in the hydroconversion reactor, i.e., the temperature during the hydroconversion step, is generally not the preheating temperature, which is generally lower than the target temperature in the hydroconversion reactor.

[0121] Preheating of the heavy hydrocarbon fraction is preferably carried out at a temperature of 280 to 450°C, even more preferably of 300 to 400°C, even more preferably of 320 to 365°C.

[0122] Such preheating may also include heating the pyrolysis oil fraction 102, in particular if said fraction is injected into the first hydroconversion reactor separately from the fraction 101; however, it is preferably heated at a lower temperature than the heavy hydrocarbon fraction 101. Advantageously, when the pyrolysis oil fraction 102 is injected into the first reactor separately from the heavy hydrocarbon fraction 101, the pyrolysis oil fraction 102 may be heated to a temperature of from room temperature (e.g. 15°C) to 350°C, preferably from 100°C to 350°C, more preferably from 100°C to 250°C, even more preferably from 100°C to less than 230°C, or even from 150°C to less than 200°C.

[0123] In case of mixing of two fractions, preheating can be performed after, before or during mixing.

[0124] According to one embodiment, in which fraction 101 and fraction 102 are preheated separately and then mixed, the plastic pyrolysis oil and / or SRF pyrolysis oil fraction 102 is preheated to a lower temperature than the heavy hydrocarbon fraction 101 to limit gum formation and / or coking of preheating equipment (e.g., furnace and / or heat exchanger) due to the presence of olefins and diolefins in the pyrolysis oil fraction 102. According to this embodiment, the preheating temperature of the plastic pyrolysis oil and / or SRF pyrolysis oil fraction 102 is preferably lower than 230°C, preferably lower than 200°C, more preferably lower than or equal to 175°C, and very preferably lower than or equal to 100°C. According to this embodiment, the heavy fraction 101 may be preheated to a temperature of 280°C to 450°C, even more preferably 300°C to 400°C, even more preferably 320°C to 365°C before mixing with the pyrolysis oil fraction 102.

[0125] According to another embodiment, in which the heavy hydrocarbon fraction 101 and the pyrolysis oil fraction 102 are mixed, the pyrolysis oil fraction 102 is indirectly heated by mixing with the heavy hydrocarbon fraction 101 (i.e., heat exchange is carried out between the two fractions having different temperatures by contacting them), the heavy hydrocarbon fraction 101 has been preheated to preferably 280°C to 450°C, even more preferably 300°C to 400°C, even more preferably 320°C to 365°C, thereby making it possible to reach the target hydroconversion temperature in the first hydroconversion reactor.

[0126] According to another embodiment, the mixture of the heavy hydrocarbon fraction 101 and the pyrolysis oil fraction 102 is preheated, advantageously using a heating device (e.g., a furnace, a heat exchanger, etc.) as described below, preferably to 280° C. to 450° C., even more preferably to 300° C. to 400° C., even more preferably to 320° C. to 365° C., thereby making it possible to reach the target hydroconversion temperature in the first hydroconversion reactor.

[0127] According to one embodiment, the preheating may also include heat exchange between the feedstock and a stream comprising preheated hydrogen (not shown in the figure), the temperature of the preheated hydrogen being generally between 350°C and 560°C, for example, about 500°C or 540°C, so that the target hydroconversion temperature can be reached in the first hydroconversion reactor.

[0128] Any device known to those skilled in the art capable of preheating the feedstock may be used. At least one oven, usually called a preheating furnace, may be used, which includes, for example, at least one heating chamber, and / or a pipe in which the feedstock flows, a mixer for mixing the feedstock with H2, any suitable type of heat exchanger, such as a tubular or spiral heat exchanger in which the feedstock flows, etc.

[0129] Before the feedstock is introduced into the first hydroconversion reactor, the feedstock is subjected to a pressurization step to adapt to the pressure in the first hydroconversion reactor, for example by a suitable pump. The pressurization step is preferably carried out before the preheating step.

[0130] According to one or more embodiments, the plastic pyrolysis oil and / or SRF pyrolysis oil fraction 102 may first be subjected to a filtration step and / or a centrifugation step and / or an electrostatic separation step and / or a washing step with an aqueous solution and / or an adsorption step to remove impurities that may naturally exist in the plastic pyrolysis oil and / or SRF pyrolysis oil, in particular to remove solid particles.

[0131] Before the feedstock is introduced into the first hydroconversion reactor, the feedstock may be mixed with the entrained catalyst precursor 104. For example, the heavy hydrocarbon fraction 101 may be mixed with the entrained catalyst precursor 104. Figure 1 and Figure 2 As shown, when the entrained catalyst is formed, particularly by reaction with sulfur, the entrained catalyst will comprise a colloidal or molecular catalyst dispersed in the feedstock.

[0132] Before the pyrolysis oil fraction 102 is mixed with the heavy hydrocarbon fraction 101, the entrained catalyst precursor 104 may be mixed with the pyrolysis oil fraction 102 ( Figure 1 ), or may be mixed with the raw material 114 formed by mixing the fraction 101 and the fraction 102 ( Figure 2 The mixing method is the same as the mixing method of the heavy hydrocarbon fraction 101 and the entrained catalyst precursor 104 described below, except that the mixing temperature of the catalyst precursor and the pyrolysis oil fraction 102 is preferably lower than 230°C, or even lower than 200°C (in any case preferably lower than the temperature at which most of the catalyst precursor begins to decompose).

[0133] It should be noted that, for the purpose of the present invention, the catalyst precursor (optionally diluted) does not constitute part of the feedstock comprising plastic pyrolysis oil and / or SRF pyrolysis oil fraction and heavy hydrocarbon fraction as defined above.

[0134] The entrained catalyst precursor can be selected from any metal catalyst precursor known to those skilled in the art, which is capable of forming a colloidal or molecularly dispersed catalyst (i.e., an entrained catalyst) in the presence of hydrogen and / or H2S and / or any other sulfur source and is capable of hydroconverting the feedstock after being injected into the first hydroconversion reactor.

[0135] The catalyst precursor is advantageously an oil-soluble catalyst precursor containing at least one transition metal.

[0136] The catalyst precursor preferably comprises an oil-soluble organometallic compound or complex.

[0137] The catalyst precursor may comprise an oil-soluble organometallic or bimetallic compound or complex comprising one or two of the following metals: Mo, Ni, V, Fe, Co or W, or a mixture of these compounds / complexes.

[0138] The oil-soluble catalyst precursor preferably has a decomposition temperature (the catalyst precursor is chemically stable at temperatures below which it is) of 100°C to 350°C, more preferably 150°C to 300°C, most preferably 175°C to 250°C.

[0139] The oil-soluble organometallic compound or complex is preferably selected from molybdenum 2-ethylhexanoate, molybdenum naphthenate, vanadium naphthenate, vanadium octoate, molybdenum hexacarbonyl, vanadium hexacarbonyl and iron pentacarbonyl. These compounds are non-limiting examples of oil-soluble catalyst precursors.

[0140] More preferably, the catalyst precursor comprises Mo, for example comprising a compound selected from molybdenum 2-ethylhexanoate, molybdenum naphthenate and molybdenum hexacarbonyl.

[0141] The currently preferred catalyst precursor comprises or consists of molybdenum 2-ethylhexanoate (also commonly referred to as molybdenum octoate). Typically, molybdenum 2-ethylhexanoate comprises 15% by weight of molybdenum and has a sufficiently high decomposition temperature or decomposition temperature range to avoid significant thermal decomposition when mixed with heavy hydrocarbon fractions at temperatures below 250°C.

[0142] One skilled in the art can select a mixing temperature profile that allows mixing of selected precursors without significant thermal decomposition prior to forming a colloidal or molecular catalyst.

[0143] As described in US2005 / 0241991, US10822553 or US10941353 and reviewed below, the catalyst precursor 104 (preferably an oil soluble catalyst precursor) may be premixed with a hydrocarbon diluent stream to form a diluted precursor mixture.

[0144] The catalyst precursor 104 may be premixed with a diluent to form a diluted precursor mixture, and the premixing is preferably carried out at a temperature lower than the temperature at which most of the catalyst precursor begins to decompose, preferably at a temperature of from ambient temperature (e.g., 15°C) to 300°C, more preferably from 15°C to 200°C, even more preferably from 50°C to 200°C, even more preferably from 75°C to 150°C, even more preferably from 75°C to 100°C, and advantageously for a time of from 1 second to 30 minutes.

[0145] Typically, the catalyst precursor diluent may be a hydrocarbon-based oil consisting of at least 50% by weight of hydrocarbons having a boiling point of 180° C. to 540° C. relative to the total weight of the hydrocarbon-based oil. Examples of hydrocarbon-based diluents suitable for precursor dilution include, but are not limited to, vacuum gas oils known as "VGO" (which typically have a boiling range of 360° C. to 524° C.), decant oils or recycle oils (which typically have a boiling range of 360° C. to 550° C.), such as FCC fluidized bed catalytic cracking effluents, such as heavy cycle oil (HCO) or light cycle oil (LCO), pyrolysis oils from hydrocrackers, light gas oils (which typically have a boiling range of 200° C. to 360° C.), atmospheric residue, vacuum residue (which typically have a boiling range equal to or greater than 524° C.), deasphalted oils and resins. The catalyst precursor diluent is preferably atmospheric residue, vacuum residue or VGO.

[0146] Then, the diluted precursor can be mixed with the heavy hydrocarbon fraction 101, preferably at a temperature of from ambient temperature (e.g., 15° C.) to 300° C., and advantageously for a time of from 1 second to 30 minutes, preferably from 1 second to 10 minutes, and even more preferably from 2 seconds to 3 minutes. In this specification, a mixing time (or mixing residence time) of 1 second means instantaneous mixing.

[0147] The mass ratio of catalyst precursor 104 to hydrocarbon oil diluent is preferably about 1:500 to about 1:1, more preferably about 1:150 to about 1:2, and even more preferably about 1:100 to about 1:5 (e.g., 1:100, 1:50, 1:30 or 1:10).

[0148] In the absence of mixing with a diluent, it is preferred to ensure that the components are mixed for a sufficient time to completely / intimately mix the catalyst precursor into the heavy hydrocarbon fraction before forming the entrained catalyst. However, long mixing times, such as 24 hours, can be cost-prohibitive for certain industrial operations.

[0149] Premixing the catalyst precursor 104 with the hydrocarbon-based diluent greatly facilitates thorough and intimate mixing of the precursor into the heavy hydrocarbon fraction, especially within the relatively short time required for economically viable large-scale commercial operations.

[0150] The diluted precursor is preferably combined with the heavy hydrocarbon fraction and mixed for a sufficient time and in a manner that disperses the catalyst precursor throughout the heavy fraction, so that the catalyst precursor is completely / intimately mixed with the heavy hydrocarbon fraction. In order to obtain sufficient mixing before forming a colloidal or molecular catalyst, it is more preferred to mix the diluted precursor and the heavy fraction for a time of 1 second to 10 minutes, and even more preferably for a time of 2 seconds to 3 minutes. Increasing the intensity and / or shear energy of the mixing process generally reduces the time required to achieve complete / intimate mixing. Examples of mixing equipment that can be used to perform complete / intimate mixing of the catalyst precursor 104 and the heavy hydrocarbon fraction 101 include, but are not limited to, high shear mixing, such as mixing produced in a pump with a rotor agitator or impeller; multiple static inline mixers; a combination of multiple static inline mixers and high shear inline mixers; a combination of multiple static inline mixers and high shear inline mixers; a combination of multiple static inline mixers and high shear inline mixers, followed by recirculation pumping in a storage tank; a combination of the above equipment, followed by one or more multi-stage centrifugal pumps.

[0151] The heavy hydrocarbon fraction 101 and the diluted precursor are preferably mixed and conditioned at a temperature of 50 to 200° C., more preferably 75 to 175° C. Preferably, the gauge pressure is 0 to 25 MPa, more preferably 0.01 to 5 MPa.

[0152] Under the operating conditions of the hydroconversion reactor in the hydroconversion step (b), the catalyst precursor 104 is completely decomposed and the precursor metal has combined with sulfur (e.g., dissolved HS present in the feedstock, or HS contained in hydrogen recycled to the hydroconversion reactor, or sulfur from organic sulfur molecules present in the feedstock, or possibly previously introduced into the feedstock), thereby obtaining a colloidal or molecular catalyst.

[0153] The metal concentration of the catalyst (preferably Mo) in the feedstock is preferably 5 to 500 ppm by weight of the feedstock, more preferably 10 to 300 ppm by weight, more preferably 10 to 175 ppm by weight, even more preferably 10 to 75 ppm by weight, even more preferably 10 to 50 ppm by weight.

[0154] Preferably, the colloidal or molecular catalyst comprises or consists of molybdenum disulfide.

[0155] As described above, the pyrolysis oil fraction 102 (mixed or not mixed with the heavy hydrocarbon fraction 101) is introduced into the first hydroconversion reactor of the first hydroconversion stage 20. However, the first hydroconversion step may include several hydroconversion reactors in series, and the pyrolysis oil fraction 102 may be placed in a hydroconversion reactor downstream of the first hydroconversion reactor of the first hydroconversion stage 20 without departing from the context of the present invention.

[0156] (b) First Hydroconversion Step

[0157] The feedstock, whether the fractions constituting it are separated (101 and 102) or mixed (114) according to step (a), is introduced together with hydrogen (stream not shown) into the first hydroconversion reactor of the first hydroconversion stage 20. The first reactor contains a first porous supported hydroconversion catalyst.

[0158] The first hydroconversion step (b) is carried out under conditions that produce a first hydroconversion effluent 105. The first hydroconversion effluent 105 contains conversion products; notably, the first effluent has a reduced content of hydrocarbons having a boiling point of at least 300°C, or at least 350°C, 375°C, 450°C, 500°C, or even 540°C (depending on the nature of the feedstock) (relative to the feedstock). The sulfur content and / or metal content and / or silicon content and / or halide (e.g., chlorine) content and / or nitrogen content and / or Conradson carbon content and / or asphaltene content in the first hydroconversion effluent 105 (depending on the reactions carried out in the first hydroconversion reactor and the composition of the feedstock) will also be reduced (relative to the feedstock). In particular, advantageously, the content of sulfur, metals, silicon, halides (e.g., chlorine), nitrogen, Conradson carbon and asphaltene in the first hydroconversion effluent 105 will be reduced (relative to the feedstock).

[0159] Advantageously, the content of silicon and / or halides (e.g. chlorine) in the first hydroconversion effluent 105 obtained at the end of step b) is reduced relative to the content of the same impurities (i.e. silicon and / or halides, e.g. chlorine) in the feedstock. Preferably, the first hydroconversion effluent 105 comprises a liquid fraction (PI+ fraction) having:

[0160] - a silicon content less than or equal to 5 ppm by weight, preferably less than or equal to 2 ppm by weight, even less than or equal to 1 ppm by weight, relative to the total weight of the liquid portion of the first hydroconversion effluent 105, and / or

[0161] - The chlorine content is less than or equal to 10 ppm by weight, preferably less than or equal to 5 ppm by weight, even less than or equal to 2 ppm by weight, or even 1 ppm by weight, relative to the total weight of the liquid portion of the first hydroconversion effluent 105.

[0162] Step (b) is preferably carried out at an absolute pressure of 2 MPa to 38 MPa, more preferably 5 MPa to 25 MPa, more preferably 6 MPa to 20 MPa, at a temperature of 300°C to 550°C, more preferably 350°C to 500°C, preferably 370°C to 450°C, even more preferably 405°C to 450°C, even 410°C to 450°C.

[0163] The hourly space velocity (HSV) (HSV per reactor volume) is preferably 0.05 h -1 Until 10h -1 The hourly space velocity (HSV), also called the liquid hourly space velocity (LHSV), is defined herein as the ratio between the hourly volume flow rate of the liquid feedstock (sent to the hydroconversion step) and the volume of each hydroconversion reactor. According to a preferred embodiment, the HSV is 0.1 h -1 Until 10h -1 , more preferably 0.1h -1 Until 5h -1 , even more preferably 0.15h -1 Up to 2h -1 , even more preferably 0.15h -1 Up to 1h -1 .

[0164] According to another embodiment, the overall HSV is 0.05h -1 To 0.09h -1 , i.e. if several hydroconversion reactors are used in step b), the overall HSV is the ratio of the liquid feed flow rate to step b) relative to the volume of all reactors.

[0165] The amount of hydrogen mixed with the raw material is preferably 50 to 5000 Nm3. 3 ) / cubic meter (m 3 ) Liquid raw material, preferably 100Nm 3 / m 3 Up to 2000Nm 3 / m 3 , 200Nm is very preferred 3 / m 3 Up to 1000Nm 3 / m 3 .

[0166] The first hydroconversion section 20 comprises one or more ebullated bed or mixed bed reactors containing at least one first supported hydroconversion catalyst, which reactors may be arranged in series and / or in parallel. Therefore, in this step, at least one first supported hydroconversion catalyst is maintained in one or more reactors. According to one or more embodiments of the present invention, the first hydroconversion section 20 comprises one or more hydroconversion reactors, which reactors may be arranged in series and / or in parallel as an ebullated bed, for example The invention relates to a method for producing a porous supported solid catalyst in a reactor, for example, as described in patents US4521295 or US4495060 or US4457831 or US4354852, in the paper Aiche, March 19-23, 1995, Houston, Texas, paper number 46d, "Second generation ebullated bed technology", or in the book "Catalysis by Transition Metal Sulphides" published by Technip in 2013, chapter 3.5 "Hydroprocessing and Hydroconversion of Residue Fractions". According to this or these embodiments, each reactor is operated as a fluidized bed (i.e., a so-called ebullated bed). Each reactor advantageously comprises a recirculation pump, which can keep the porous supported solid catalyst as an ebullated bed by such continuous recirculation that at least a portion of the liquid fraction is taken out from the upper part of the reactor and reinjected into the lower part of the reactor.

[0167] The ebullated bed reactor preferably includes at least one input port located at or near the lower part of the reactor, through which the feedstock and hydrogen are introduced together, especially in the case where the pyrolysis oil fraction 102 and the heavy hydrocarbon fraction 101 in the feedstock are introduced separately, two input ports are included, and the ebullated bed reactor also includes an output port located at or near the upper part of the reactor, through which the first hydroconversion effluent 105 is taken out. The reactor also preferably includes an inlet and an outlet for a supported catalyst, as described above in the device for injecting and taking out the supported catalyst. The ebullated bed reactor also includes an expanded catalyst zone containing a porous supported catalyst. The ebullated bed reactor also includes a lower unloaded catalyst zone located below the expanded catalyst zone, and an upper unloaded catalyst zone located above the expanded catalyst zone. The feedstock in the ebullated bed reactor is continuously recycled from the upper unloaded catalyst zone to the lower unloaded catalyst zone through a recirculation pipe connected to a boiling pump. Preferably, a funnel-shaped recirculation cup is installed in the upper part of the recirculation pipe, through which the feed is sucked out from the upper unsupported catalyst zone. The internal recirculation feed is mixed with "fresh" feed and additional hydrogen.

[0168] The first supported hydroconversion catalyst used in the first hydroconversion step (b) may comprise one or more elements from Group 4 to Group 12 of the Periodic Table of the Elements, deposited or not deposited on a support. The catalysts that can be used advantageously comprise an amorphous support, for example silica, alumina, silica-alumina, titania or a combination of these structures, very preferably alumina.

[0169] The first supported catalyst may comprise at least one Group VIII non-noble metal selected from nickel and cobalt, preferably nickel, the Group VIII element preferably being used in combination with at least one Group VIB metal selected from molybdenum and tungsten; preferably, the Group VIB metal is molybdenum.

[0170] In this specification, the group of chemical elements is given according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, edited by DRLide, 81st edition, 2000-2001). For example, group VIII according to the CAS classification corresponds to the metals of columns 8, 9 and 10 according to the new IUPAC classification.

[0171] Advantageously, the first supported hydroconversion catalyst used in the first hydroconversion step (b) comprises an alumina support and at least one Group VIII metal selected from nickel and cobalt, preferably nickel, and at least one Group VIB metal selected from molybdenum and tungsten, preferably molybdenum. The first supported hydroconversion catalyst preferably comprises nickel as Group VIII element and molybdenum as Group VIB element.

[0172] The content of non-noble metals of group VIII, in particular nickel, expressed as the weight of the metal oxide (in particular NiO), is advantageously between 0.5% and 10% by weight, preferably between 1% and 6% by weight, and the content of metals of group VIB, in particular molybdenum, expressed as the weight of the metal oxide (in particular molybdenum trioxide MoO3), is advantageously between 1% and 30% by weight, preferably between 4% and 20% by weight. The content of metal is expressed as a weight percentage of the metal oxide relative to the weight of the catalyst.

[0173] The first supported catalyst is advantageously used in the form of extrudate or beads. The beads have a diameter of, for example, 0.4mm to 4.0mm. The extrudate has a cylindrical shape with a diameter of, for example, 0.5mm to 4.0mm and a length of 1mm to 5mm. The extrudate can also be an object of different shapes, such as regular or irregular trilobal, quadrilobal or other multilobal shapes. Other forms of porous supported catalysts can also be used. The size of these different forms of porous supported catalysts can be characterized by equivalent diameter. Equivalent diameter is defined as the ratio of particle volume to particle surface area multiplied by six. Therefore, the porous supported catalyst used in extrudate, beads or other forms has an equivalent diameter of 0.4mm to 4.4mm. These catalysts are well known to those skilled in the art.

[0174] According to one or more embodiments of the present invention, the first hydroconversion section 20 comprises one or more mixed bed reactors (i.e., mixed boiling-entrained beds), and comprises at least one first supported hydroconversion catalyst maintained in the reactor and at least one entrained catalyst, which enters the reactor with the feedstock and is entrained out of the reactor with the effluent. In this case, as described above with respect to step (a), before the feedstock is injected into the first hydroconversion reactor, an entrained catalyst precursor has been introduced, and a colloidal or molecular catalyst, also referred to as a dispersed catalyst, an entrained catalyst, or a slurry catalyst, may have been formed upstream or in situ of the mixed bed hydroconversion reactor. These entrained catalysts are well known to those skilled in the art.

[0175] The mixed bed reactor comprises a solid phase comprising a porous supported catalyst in the form of an expanded bed; a liquid hydrocarbon-based phase comprising a feedstock containing a colloidal or molecular catalyst dispersed in the feedstock; and a gas phase comprising hydrogen.

[0176] The mixed bed reactor is an ebullated bed hydroconversion reactor as described above, but contains a molecular or colloidal catalyst that is entrained out of the reactor with the hydroconversion liquid effluent 105, in addition to a porous supported catalyst held in the reactor in an expanded bed.

[0177] According to one or more embodiments, the implementation of the mixed bed hydroconversion reactor is based on the implementation of the ebullated bed reactor described above, and further involves a colloidal or molecular catalyst dispersed throughout the feedstock in the mixed bed reactor (including an expanded catalyst zone and an unsupported catalyst zone), thereby being used to promote the upgrading reaction, which constitutes the catalyst-free zone in a traditional ebullated bed reactor.

[0178] The presence of colloid or molecular catalyst in mixed bed reactor provides additional catalytic hydrogenation activity in expanded catalyst zone, recycle pipe and lower unloaded catalyst zone and upper unloaded catalyst zone. The end-capping of free radicals outside porous supported catalyst minimizes the formation of sediment and coke precursor, which is usually the cause of deactivation of supported catalyst. This can reduce the amount of porous supported catalyst required for the required hydroconversion reaction. This can also reduce the rate of needing to take out and replenish porous supported catalyst. Using colloid or molecular catalyst in mixed bed reactor can also make hydroconversion at a temperature higher than that when using ebullating bed reactor (containing only one or more supported catalysts, without entrained catalyst), while remaining within the temperature range given for step (b) above.

[0179] In one embodiment of the process according to the invention, a different first supported hydroconversion catalyst may be used in each reactor of the first hydroconversion stage, the supported catalyst dedicated to each reactor being suitable for the feedstock fed to the reactor. In one embodiment of the process according to the invention, several types of first supported catalysts are used in each reactor.

[0180] As is well known and described, for example, in patent FR3033797, when the first supported hydroconversion catalyst is spent, it can be partially replaced by fresh supported catalyst and / or spent supported catalyst having a higher catalytic activity than the spent supported catalyst to be replaced and / or regenerated supported catalyst and / or reconverted supported catalyst (catalyst from a reconversion zone in which the majority of the deposited metals are removed, and then the spent and reconverted catalyst is sent to a regeneration zone in which the carbon and sulphur contained in the catalyst are removed, thereby increasing the activity of the catalyst) by removing the spent supported catalyst preferably at the bottom of the reactor and introducing the replacement supported catalyst at the top or bottom of the reactor. This replacement of the spent supported catalyst is preferably carried out at regular intervals, preferably batchwise or substantially continuously. The removal and replacement are carried out using removal and injection means that advantageously make this hydroconversion step continuous.

[0181] This supported catalyst withdrawal / injection mode of operation eliminates the need to shut down the unit to replace spent catalyst, nor does it require increasing reaction temperatures along the cycle to compensate for deactivation. In addition, working under constant operating conditions allows for stable product yields and qualities along the cycle.

[0182] Furthermore, since the supported catalyst is kept stirred by significant liquid recirculation, the pressure drop across the reactor remains low and constant and the exothermic heat of reaction is rapidly and evenly distributed over the catalyst bed, the catalyst bed is virtually isothermal without the need for, for example, injection of cooling streams (quenching).

[0183] An important aspect of the present invention is the ability of an ebullated bed or mixed ebullated-entrained bed reactor to continuously convert pyrolysis oil into lighter products by this combination of high temperature and the presence of a catalyst capable of hydrogenating unsaturated molecules (olefins or aromatics). Thus, pyrolysis oil co-treatment can increase the yield of certain fractions obtained in the hydroconversion effluent, in particular the gasoline fraction.

[0184] Another advantage of the present invention is the removal of impurities, such as silicon or metals, by the supported catalyst, which is associated with the co-treatment of the pyrolysis oil using a hydroconversion reactor operating in an ebullating bed or a hybrid ebullating-entrained bed. This allows a product low in impurities to be obtained, which can be more easily processed in downstream processes, such as fixed bed hydroprocessing processes. An ebullating bed or a hybrid ebullating-entrained bed has the advantage that the supported catalyst is continuously replaced and, if necessary, especially in the case of a large amount of impurities in the pyrolysis oil, it is easy to compensate for more severe deactivation by increasing the catalyst replacement.

[0185] According to one or more embodiments, when step (b) is carried out in one or more mixed bed reactors, the feedstock or the entrained catalyst precursor may be premixed with an organic additive before the feedstock is introduced into the first hydroconversion reactor of the first hydroconversion stage 20, thereby minimizing the fouling of the equipment, in particular, before the hydroconversion is carried out in the one or more mixed bed reactors. Without being limited to any theory, the organic additive, as a mixture with the feedstock, can increase the solubility of the catalyst precursor entrained in the feedstock, avoid or reduce fouling caused by metal deposition in the equipment upstream of the hydroconversion reactor (e.g., heating equipment), thereby improving the dispersibility of the entrained catalyst, thereby increasing the utilization of the metal active sites, promoting the hydrogenation of free radicals as precursors of coke and sediments, and significantly reducing the fouling of the equipment. The organic additive is neither a catalyst nor a catalyst precursor (e.g., it does not contain metal), and has at least one carboxylic acid functional group and / or at least one ester functional group and / or at least one anhydride functional group. It preferably contains at least 6 or even at least 8 carbon atoms, more preferably at least 8 carbon atoms. According to one embodiment, it contains 8 carbon atoms. For example, the organic additive can be 2-ethylhexanoic acid, cyclohexane acid, octanoic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, ethyl octanoate, ethyl 2-ethylhexanoate, 2-ethylhexyl 2-ethylhexanoate, benzyl 2-ethylhexanoate, diethyl adipate, dimethyl adipate, di(2-ethylhexyl) adipate, dimethyl pimelate, dimethyl suberate, monomethyl suberate, caproic anhydride, caprylic anhydride, and mixtures thereof. The organic additive is preferably added during the mixing step so that the molar ratio of the organic additive to the one or more active metals (e.g., Mo) in the catalyst precursor composition is from 0.1:1 to 20:1, more preferably from 0.75:1 to 7:1, and even more preferably from 1:1 to 5:1.

[0186] (c) Optional intermediate separation steps

[0187] According to one or more preferred embodiments, the method according to the present invention further comprises a separation step (c) of separating a part or all of the first hydroconversion effluent 105 to produce at least two fractions, one of which is a heavy fraction boiling mainly at a temperature greater than or equal to 350°C.

[0188] The other fraction or fractions are one or more light fractions and middle fractions. The light fraction thus separated contains mainly gases (H2, HCl, H2S, NH3 and C1-C4), naphtha (or gasoline, fractions with a boiling point below 150°C), kerosene (or gas oil, fractions with a boiling range of 150°C to 250°C) and at least some diesel (fractions with a boiling range of 250°C to 375°C). The light fraction can then be at least partially sent to a fractionation unit (not shown in the figure) in which light gases are extracted from the light fraction, for example by passing through an expansion vessel. The fractionation unit can be the fractionation unit of the fractionation step (e), in particular in the case where the second hydroconversion step (d) is carried out therein, the hydrogen thus recovered, which has been sent to the purification and compression equipment, can be advantageously recycled to the first hydroconversion step (b) and / or the second hydroconversion step (d) (if carried out). The recovered hydrogen can also be used in other refinery equipment.

[0189] The optional separation step (c) is carried out in a separation section (not shown) which comprises any separation device known to the person skilled in the art. The separation section may comprise one or more expansion vessels arranged in series and / or one or more steam stripping and / or hydrogen stripping columns and / or atmospheric distillation columns and / or vacuum distillation columns, preferably consisting of a single expansion vessel, usually called a "hot separator". The separation section may also comprise a device for washing the light fraction, which mainly contains gases, by contact with an aqueous solution.

[0190] According to a preferred embodiment, the optional separation step (c) comprises a hot separator, the operating temperature of which is greater than or equal to 300° C., or even greater than or equal to 350° C., in order to avoid the formation of ammonium chloride salts in the liquid phase; the gas phase in the hot separator or at least one phase resulting from the subsequent separation of the gas phase from the hot separator is advantageously contacted with water or an alkaline aqueous solution (e.g. sodium hydroxide solution, one or more amine solutions) in order to at least partially remove hydrogen chloride (HCl) and / or at least partially dissolve the ammonium chloride salts. The separation device or separation vessel may comprise a zone at the bottom for separately settling the hydrocarbon fraction and the aqueous fraction comprising the chloride salts, or may comprise a tower for scrubbing the gas by contact with water or an alkaline aqueous solution.

[0191] (d) Optional Second Hydroconversion Step

[0192] According to one or more preferred embodiments (not shown in the figures), the method further comprises a second hydroconversion step, in the presence of hydrogen, in at least one second ebullating bed or mixed bed reactor comprising a second porous supported catalyst, a part or all of the first effluent 105 produced by step (b), or optionally a heavy fraction from step (c) is subjected to a second hydroconversion. The second hydroconversion step is carried out to produce a second hydroconversion effluent. The second hydroconversion effluent advantageously contains a greater amount of conversion products than the first hydroconversion effluent 105, and in particular even lower content of hydrocarbons having a boiling point of at least 300°C, or at least 350°C, 375°C, 450°C, 500°C or 540°C (depending on the nature of the feedstock). Relative to the first hydroconversion effluent 105, the second hydroconversion effluent may have a further reduced Conradson carbon residue, and optionally a further reduced sulfur and / or nitrogen and / or metal and / or silicon and / or halide (e.g., chlorine) and / or asphaltene content.

[0193] In particular, the second hydroconversion effluent can advantageously have reduced sulfur, metals, silicon, halides (eg, chlorine), nitrogen, Conradson carbon, and asphaltenes content relative to the first hydroconversion effluent 105 and / or relative to the feedstock.

[0194] The content of silicon and / or halides (for example chlorine) in the second hydroconversion effluent obtained at the end of step d) is advantageously reduced relative to the content of the same impurities (ie silicon and / or halides (for example chlorine) contained in the first hydroconversion effluent 105 and / or in the feedstock.

[0195] Preferably, the second hydroconversion effluent comprises a liquid fraction (PI+ fraction) having:

[0196] a silicon content less than or equal to 5 ppm by weight, preferably less than or equal to 2 ppm by weight, even less than or equal to 1 ppm by weight, relative to the total weight of the liquid portion of the second hydroconversion effluent, and / or

[0197] the chlorine content of the element is less than or equal to 10 ppm by weight, preferably less than or equal to 5 ppm by weight, or even less than or equal to 2 ppm by weight, or even 1 ppm by weight, relative to the total weight of the liquid portion of the second hydroconversion effluent.

[0198] The second hydroconversion step is carried out in a similar manner to the first hydroconversion step (b) and will not be described in detail here. This applies in particular to the operating conditions, the equipment used and the porous supported hydroconversion catalyst used, except for the details mentioned below.

[0199] As with the first hydroconversion step (b), the second hydroconversion step is carried out in at least a second ebullated bed or mixed bed reactor. If the first hydroconversion step is also carried out in one or more ebullated bed reactors, the second hydroconversion step is preferably carried out in one or more ebullated bed reactors; if the first hydroconversion step is carried out in one or more mixed bed reactors, the second hydroconversion step is preferably carried out in one or more mixed bed reactors.

[0200] In the second hydroconversion step, the operating conditions may be similar to or different from the operating conditions in the hydroconversion step (d), the temperature is maintained at 405°C to 550°C, preferably 405°C to 500°C, more preferably 405°C to 450°C, the amount of hydrogen introduced into the reactor is maintained at 50 Nm 3 / m 3 Up to 5000Nm 3 / m 3 Liquid raw material, preferably 100Nm 3 / m 3 Up to 3000Nm 3 / m 3 , more preferably 200Nm 3 / m 3 Up to 2000Nm 3 / m 3 The ranges of other pressure and HSV parameters are the same as those described for the hydroconversion step (d).

[0201] The operating temperature of the second hydroconversion step (d) may be higher than the operating temperature of the first hydroconversion step (b). This allows for a more complete conversion of the unconverted feedstock. Hydroconversion of the liquid product from the first hydroconversion step and feedstock conversion are improved, as are hydrotreating reactions such as hydrodesulfurization and hydrodenitrogenation. Operating conditions are selected to minimize the formation of solids such as coke.

[0202] The second porous supported hydroconversion catalyst used in the second hydroconversion reactor may be the same catalyst used in the one or more first hydroconversion reactors of the first hydroconversion stage 20, or may be another porous supported catalyst also suitable for hydroconversion of the treated feedstock, as defined for the first supported catalyst used in the first hydroconversion step (b).

[0203] As described in step (a), the pyrolysis oil fraction 102 (mixed or not mixed with the heavy hydrocarbon fraction 101) in the feedstock is introduced into the first hydroconversion reactor of the first hydroconversion stage 20. However, the pyrolysis oil fraction 102 may be placed in the hydroconversion reactor of the second hydroconversion stage 20 without departing from the context of the present invention.

[0204] (e) Fractionation step

[0205] The first hydroconversion effluent 105 from the hydroconversion step (b) or the hydroconversion effluent from the second hydroconversion step (d) if this step is performed is subsequently at least partially subjected to a fractionation step (e) in a fractionation section 30 .

[0206] The fractionation step (e) separates part or all of the hydroconversion effluent into several fractions, including at least one heavy liquid product 106b, which boils mainly at a temperature above 350° C., preferably above 500° C., and more preferably above 540° C. The heavy liquid product 106b contains a portion boiling at a temperature above 540° C., which is called the residual oil fraction (or vacuum residue), i.e., the unconverted portion. The heavy liquid product 106b may include a gas oil fraction portion with a boiling range of 250° C. to 375° C. and a portion with a boiling range of 375° C. to 540° C. (also called vacuum distillate).

[0207] Thus, the fractionation step produces at least two products including the heavy liquid product 106b described above, and the additional product or products 106a being one or more light fractions and middle fractions.

[0208] Fractionation section 30 comprises any separation device known to those skilled in the art.

[0209] Thus, the fractionation section 30 may include one or more of the following separation devices: one or more flash vessels arranged in series, preferably a group of at least two flash vessels in series, one or more steam and / or hydrogen stripping columns, atmospheric distillation columns, vacuum distillation columns.

[0210] According to one or more embodiments, the fractionation step (e) is performed by a set of at least two flash vessels connected in series.

[0211] According to one or more other embodiments, the fractionation step (e) is performed by one or more steam and / or hydrogen stripping columns.

[0212] According to one or more preferred embodiments, the fractionation step (e) is performed by an atmospheric distillation column, more preferably by an atmospheric distillation column and a vacuum column receiving the atmospheric residue.

[0213] According to one or more most preferred embodiments, the fractionation step (e) is carried out by one or more flash vessels, an atmospheric distillation column and a vacuum column receiving atmospheric residue. This configuration can reduce the size of any downstream deasphalter, thereby minimizing investment and operating costs.

[0214] In addition to part or all of the hydroconversion liquid effluent, the fractionation section 30 may also receive one or more additional effluents, such as one or more hydrocarbon feedstocks from outside the process (e.g. atmospheric and / or vacuum distillates, atmospheric and / or vacuum residues), a portion of the heavy fraction from separation step (c) (if performed), a portion of one or more middle fractions from fractionation step (e), a portion of DAO or a light or heavy fraction of DAO (if the deasphalting step (f1) is performed). The fractionation section 30 may also include means for washing one or more separation products by contact with an aqueous solution.

[0215] According to a preferred embodiment, the fractionation step (e) comprises a hot separator, the operation temperature of which is higher than or equal to 300° C., even higher than or equal to 350° C., in order to avoid the formation of ammonium chloride salts in the liquid phase; the gas phase of the hot separator or at least one phase resulting from the subsequent separation of the gas phase of the hot separator, and at least part of the liquid phase of the hot separator or at least one phase resulting from the subsequent separation of the liquid phase of the hot separator are advantageously contacted with water or an alkaline aqueous solution (e.g. sodium hydroxide solution, amine solution) in order to at least partially remove hydrogen chloride (HCl) and / or at least partially dissolve the ammonium chloride salts. The separation device or separation vessel may comprise a zone at the bottom for separating the settled hydrocarbon fraction and the aqueous fraction containing the chloride salts, or may comprise a tower for washing the gas by contact with water or an alkaline aqueous solution.

[0216] According to a very preferred embodiment, when separation step c) is carried out, at least part of the separation equipment is shared between step c) and step e).

[0217] (f) one or more subsequent processing steps

[0218] The heavy liquid product 106b and / or other product(s) produced in the fractionation step (e) may be subjected to one or more subsequent processing steps (f).

[0219] Such step (f) may comprise at least one step selected from the group consisting of: hydrotreatment, steam cracking, fluidized bed catalytic cracking, hydrocracking, deasphalting and lubricant oil extraction. These examples of subsequent treatments are not exhaustive.

[0220] Specifically, the various hydrocarbon products that may be produced from the fractionation unit 30 in the fractionation step (e) can be sent to various processes in the refinery, as shown in the figure by the reference numeral 40, and the details of all these post-treatments are not described here because they are generally known to those skilled in the art. For example, the gas fraction, naphtha (gasoline), middle distillates, VGO, DAO can be sent to hydrotreating, steam cracking, fluidized bed catalytic cracking (FCC), hydrocracking, lubricating oil extraction and other processes. The residual oil (atmospheric residue or vacuum residue) can also be post-treated or used for other purposes, such as gasification, production of asphalt, heavy fuel oil, etc. The heavy fraction including the residual oil can also be recycled to the hydroconversion process, for example, recycled to the hydroconversion reactor in step (b) or step (d).

[0221] According to one or more embodiments, the hydroconversion process includes a deasphalting step (f1), which comprises deasphalting a portion or all of the heavy liquid product 106b obtained in the fractionation step (e) using at least one hydrocarbon-based solvent in a deasphalter to produce deasphalted oil DAO and residual asphalt ("SDA" solvent deasphalting step).

[0222] Such a deasphalting step (f1) is carried out under conditions well known to those skilled in the art. du Pétrole" Vol. 49, No. 5, pp. 495 to 507, and the book "Raffinageet conversion des products lourds du pétrole" by JF Le Page, SG Chatila and M. Davidson (Edition Technip, pp. 17-32), or reference patents US4239616, US4354922, US4354928, US4440633, US4536283 and US4715946. Deasphalting can be carried out in one or more mixer-settlers or one or more extraction towers. Therefore, the deasphalter includes at least one mixer-settler or at least one extraction tower. Deasphalting is a liquid-liquid extraction, which is usually carried out at an average temperature of 60°C to 250°C, using at least one low boiling hydrocarbon-based solvent, preferably a paraffin solvent, preferably a solvent higher than propylene. The preferred solvents include propane, butane, isobutane, pentane, isopentane, neopentane, hexane, isohexane, C6 hydrocarbons, heptane, C7 hydrocarbons, light gasolines of relatively strong or weak polarity, and mixtures thereof. Preferably, the solvent is butane, pentane or hexane, and mixtures thereof. The solvent / feedstock (volume / volume) ratio entering the deasphalter is generally 3 / 1 to 16 / 1, preferably 4 / 1 to 8 / 1. Preferably, the deasphalter comprises at least one extraction column, preferably only one extraction column (e.g. in a Solvahl TM The extraction tower used in the process) wherein the solvent / feedstock (volume / volume) ratio entering the deasphalter is preferably low, typically 4 / 1 to 8 / 1, or even 4 / 1 to 6 / 1. The deasphalter produces DAO and residual asphalt, the DAO contains almost no C7 asphaltene, the C7 asphaltene content is preferably less than 2% by weight, more preferably less than 0.5% by weight, even more preferably less than 0.05% by weight, the residual asphalt concentrates most of the impurities in the residue, and the residual asphalt is taken out. The DAO yield is typically 40% to 95% by weight, depending on the operating conditions and the solvent used, as well as the quality of the feedstock sent to the deasphalter, especially the heavy liquid product 106b.

[0223] According to one or more embodiments, the hydroconversion process comprises at least one hydroprocessing step (f2), preferably hydroprocessing one or more liquid products from the fractionation step (e) in a fixed bed in a hydroprocessing section. The hydroprocessing section may comprise at least one fixed bed reactor comprising n catalytic beds, n being an integer greater than or equal to 1, each catalytic bed comprising at least one hydroprocessing catalyst, the hydroprocessing reaction section being fed with at least a portion of the liquid products obtained from step e) and a gaseous stream comprising hydrogen to obtain a hydroprocessing effluent.

[0224] This step involves hydroprocessing reactions well known to those skilled in the art, more particularly hydroprocessing reactions such as hydrogenation of aromatics or olefins, hydrodesulfurization and hydrodenitrogenation.

[0225] The hydroprocessing reaction section is advantageously operated at an average temperature (weighted average bed temperature (WABT)) of 250° C. to 430° C., preferably 300° C. to 400° C., at a hydrogen partial pressure of 1.0 MPa to 20.0 MPa, preferably 3.0 MPa to 15.0 MPa, at a rate of 0.1 h -1 To 10.0h -1 , preferably 0.1h -1 Up to 5.0h -1 , preferably 0.2h -1 Up to 2.0h -1 , preferably 0.2h -1 To 1.0h -1 The catalyst is operated at an hourly space velocity (HSV) per volume of catalyst (one or more). In step f2), the hydrogen coverage is advantageously 50 Nm 3 Up to 2000Nm 3 , preferably 100Nm 3 Up to 1000Nm 3 , more preferably 120Nm 3 Up to 800Nm 3 Hydrogen / m 3 Feedstock to step f2).

[0226] The hydroprocessing section may comprise several reactors, preferably two, which may be operated in series and / or in parallel and / or in PRS (lead and lag) and / or swing mode as is well known to those skilled in the art. Alternatively, the hydroprocessing section may comprise a single fixed bed reactor comprising n catalytic beds, n preferably being from 1 to 10, or even from 2 to 5.

[0227] The device of recovering catalyst fines and / or the catalyst from hydroconversion can be used in the upstream or inlet of the hydroprocessing section, such as one or more filters, even reactor internals, such as filter plate type internals, one of which examples is described in patent FR3051375. The fixed bed hydroprocessing catalyst used in step f2) can be selected from known hydroprocessing catalysts and hydrodemetallization catalysts, which are particularly used for processing petroleum fractions. Known hydroprocessing catalysts are those catalysts described in such as patents EP0113297, EP0113284, US6589908, US4818743 or US6332976. Known hydrodemetallization catalysts are those catalysts described in such as patents EP0113297, EP0113284, US5221656, US5827421, US7119045, US5622616 and US5089463.

[0228] Specifically, the hydroprocessing catalyst includes a carrier (preferably a mineral carrier) and at least one metal element having a hydrodehydrogenation function.

[0229] The metal element with hydrodehydrogenation function advantageously includes at least one element of group VIII (preferably selected from nickel and cobalt) and / or at least one element of group VIB (preferably selected from molybdenum and tungsten). The total content of oxides of metal elements from groups VIB and VIII is preferably 0.1% by weight to 40% by weight, more preferably 5% by weight to 35% by weight, relative to the total weight of the hydroprocessing catalyst. The weight ratio between one or more metals of group VIB and one or more metals of group VIII, expressed as metal oxides, is preferably 1 to 20, more preferably 2 to 10. For example, the hydroprocessing section of step f2) comprises a hydroprocessing catalyst comprising 0.5% by weight to 10% by weight of nickel, preferably 1% by weight to 8% by weight of nickel (expressed as nickel oxide NiO, relative to the total weight of the hydroprocessing catalyst), and 0% by weight to 30% by weight, preferably 3% by weight to 29% by weight of the total weight of molybdenum and / or tungsten (expressed as molybdenum oxide MoO3 or tungsten oxide WO3, relative to the total weight of the hydroprocessing catalyst) on a mineral support.

[0230] The support of the hydroprocessing catalyst is advantageously selected from alumina, silica, silica-alumina, magnesia, clay and mixtures thereof. The support may also contain a dopant compound (for example, selected from oxides of boron, in particular boron trioxide, zirconium oxide, cerium dioxide, titanium oxide, phosphorus pentoxide and mixtures of these oxides).

[0231] Preferably, the hydrotreating catalyst comprises an alumina support, preferably an alumina support doped with phosphorus and optionally boron. For example, the alumina used may be gamma alumina or eta alumina.

[0232] The hydrotreating catalyst is advantageously used in the form of extrudates or beads, typically in the millimeter size, for example in the range of 0.4 mm to 4.4 mm in equivalent diameter.

[0233] Advantageously, the hydrotreating catalyst used in step f2) has a catalyst content greater than or equal to 250 m 2 / g, even greater than or equal to 300m 2 / g and advantageously less than or equal to 800m 2 / g, or even less than or equal to 600m 2 / g, or even less than or equal to 400m 2 The specific surface area of ​​??g was measured by BET nitrogen adsorption according to ASTM D3663.

[0234] When it is necessary to recycle a portion of the heavy residual oil fraction (e.g., a portion of the heavy liquid product 106b and / or a portion of the residual asphalt or a portion of the DAO) to the hydroconversion system (e.g., the first hydroconversion reactor or its upstream), it may be advantageous to leave the entrained catalyst in the residual oil fraction and / or the residual asphalt fraction in the case of a mixed bed reactor operation. The recycle stream may be discharged, usually to prevent certain compounds from accumulating to excessive levels. It should be noted that for the purposes of the present invention, such a recycle stream does not constitute a part of the feedstock comprising the pyrolysis oil fraction 102 and the heavy hydrocarbon fraction 101 as defined above.

[0235] Analytical methods used

[0236] Analytical methods and / or standards for determining the characteristics of various streams, in particular the raw materials to be processed and the effluents produced, are known to those skilled in the art. These methods are specifically listed below for reference. Other methods considered equivalent may also be used, in particular equivalent IP methods, EN methods or ISO methods:

[0237] Table 1

[0238]

[0239] (1) The MAV method described in the following article: CL ó pez-García et al., Near Infrared Monitoring of Low Conjugated Diolefins Content in Hydrotreated FCC Gasoline Streams, Oil & Gas Science and Technology-Rev. IFP, Vol. 62 (2007), No. 1, pp. 57-68. Example

[0240] The following examples are intended to demonstrate certain performance qualities of the method according to the invention.

[0241] These examples illustrate the The possibility of co-processing plastic pyrolysis oils in a type of ebullated-bed hydroconversion process, which converts plastic pyrolysis oils into lighter hydrocarbons that can be used as base materials for the production of fuels, lubricants or any other products resulting from petroleum refining, has also been demonstrated. The supported catalyst present in the process has the ability to remove impurities present in the pyrolysis oil, thus facilitating the post-treatment of these products.

[0242] These embodiments represent The process is carried out in a closed reactor (called a batch reactor) under the operating conditions of the process.

[0243] Example 1 is a comparative example illustrating the performance qualities of the hydroconversion process of a reference feedstock (vacuum residue) containing no plastic pyrolysis oil.

[0244] Example 2 illustrates the use of a feedstock comprising a plastic pyrolysis oil fraction and a reference feedstock (vacuum residue) fraction used in Example 1. Performance qualities of the process. This mixture is used during a preliminary step (optional step) of medium homogenization.

[0245] raw material:

[0246] The heavy fraction (I) of the raw material is a "straight run" vacuum residue (SR-VR) obtained directly from the distillation of petroleum crude oil. The plastic pyrolysis oil fraction (II) of the raw material is a pyrolysis oil produced from a plastic mixture and contains a large amount of impurities.

[0247] The main characteristics of these two fractions of the feedstock are shown in Table 2 below.

[0248] Table 2

[0249]

[0250]

[0251] (*)DL: Detection Limit

[0252] Table 3 below summarizes the operating conditions for these examples.

[0253] Table 3

[0254]

[0255] (**)NC: irrelevant

[0256] The steps of Example 1:

[0257] A predetermined mass of NiMo catalyst supported on alumina and 100% of SR-VR (fraction I of the raw material) was loaded into an intermittent reactor, which was preheated to 100°C to reduce its viscosity. The reactor was closed, purged with nitrogen, purged with hydrogen, and then pressurized with hydrogen to a pressure of about 3 MPa. The reactor was then heated to 100°C. At this temperature, stirring was started at 500 rpm. The temperature was gradually increased from 100°C to the reaction temperature, while stirring was gradually increased from 500 rpm to 1000 rpm. When the reaction temperature was reached, the pressure in the reactor was instantly adjusted to the target value by adding H2. At this point, the reaction time began to count down. After the experimental time was over, the reactor was quickly cooled to stop the reaction, stirring was stopped when the reactor was at room temperature, and liquid effluent and gas were collected for analysis.

[0258] The steps of Example 2:

[0259] First, the batch reactor is loaded with the same mass of NiMo catalyst supported on alumina as in Example 1, and 90% by weight of SR-VR (fraction I of the raw material) is added, which is preheated to 100°C to reduce its viscosity, and then 10% of plastic pyrolysis oil (fraction II of the raw material) is added. The reactor is closed, purged with nitrogen, purged with hydrogen, and then pressurized with hydrogen to a pressure of about 3 MPa. The reactor is then heated to 100°C. At this temperature, stirring is started at 500 rpm. The temperature is gradually increased from 100°C to 200°C, while stirring is gradually increased from 500 rpm to 1000 rpm. At 200°C, the pressure in the reactor is 4 MPa. A one-hour stabilization phase is carried out at this temperature, but this step is optional to ensure good dispersion of the pyrolysis oil (fraction II of the raw material) in the SR-VR (fraction I of the raw material). After this stabilization phase, the batch reactor is heated to the reaction temperature, and the pressure in the reactor is instantly adjusted to the target value by adding H2. At this time, the reaction time starts to count down. After the experimental time was over, the reactor was rapidly cooled to stop the reaction, stirring was stopped when the reactor was at room temperature, and the liquid effluent and gas were collected for analysis.

[0260] Overall results and performance quality:

[0261] Tables 4, 5 and 6 below detail the results related to the overall liquid effluent quality and hydroconversion performance quality of these Examples.

[0262] Table 4

[0263]

[0264] (*)DL: Detection Limit

[0265] (**)NC: irrelevant

[0266] Table 5

[0267]

[0268] Table 6

[0269]

[0270]

[0271] The conversion of the 540°C+ fraction was calculated by the mass difference between the feed and the total liquid effluent as follows:

[0272] Mathematical formula 1

[0273]

[0274] It was observed that the presence of plastic pyrolysis oil did not affect the conversion rate of 540°C+, thus significantly increasing the yield of the PI-180°C fraction while reducing the yield of the heavy fraction.

[0275] It was also shown that, despite the presence of silicon in the plastic pyrolysis oil, the hydroconversion product no longer contained silicon, indicating that silicon had been removed by the supported catalyst. Likewise, chlorine was completely converted. Therefore, the product produced in this step has a low impurity content and can be fed particularly to a fixed bed hydroprocessing process.

[0276] Furthermore, the co-treatment of the plastic pyrolysis oil does not appear to significantly impair the stability of the unconverted product, since the sediment content is only 0.04% by weight, which is a very low and completely tolerable value at the end of the hydroconversion process. The hydroprocessing performance (especially hydrodenitrogenation and hydrodesulfurization) is also maintained or even improved.

Claims

1. A process for the hydroconversion of a feedstock comprising a plastic and / or solid recovered fuel pyrolysis oil fraction (102) and a fossil-based heavy hydrocarbon fraction (101) containing at least 50% by weight of a portion having a boiling point of at least 300° C., and containing sulfur and nitrogen, the pyrolysis oil fraction (102) accounting for less than 50% by weight of the feedstock, the process comprising: (a) conditioning the feedstock and introducing it into a first hydroconversion stage (20), the first hydroconversion stage comprising at least a first ebullated bed or mixed ebullated-entrained bed hydroconversion reactor, the reactor containing a first porous supported hydroconversion catalyst; (b) a first step of hydroconverting the feedstock in the presence of hydrogen in the first hydroconversion section (20) to obtain a first hydroconversion effluent (105); (c) optionally, a step of separating a portion or all of said first effluent produced by step (b) to form at least one heavy fraction boiling primarily at a temperature greater than or equal to 350° C.; (d) optionally, a second hydroconversion step of part or all of the first effluent produced by step (b) or optionally part or all of the heavy fraction produced by step (c) in a second hydroconversion section comprising at least a second ebullated bed or mixed ebullated-entrained bed hydroconversion reactor, the second hydroconversion reactor comprising a second porous supported catalyst and operated in the presence of hydrogen, to produce a second hydroconversion effluent; Step (b) and optional step (d) are carried out at an absolute pressure of 2 MPa to 38 MPa, at a temperature of 300° C. to 550° C., at a temperature of 0.05 h -1 Until 10h -1 At the hourly space velocity and at 50Nm 3 / m 3 Up to 5000Nm 3 / m 3 The hydrogen amount is 2. (e) a step of fractionating a portion or all of the first hydroconversion effluent from step (b) or a portion or all of the second hydroconversion effluent from step (d) in a fractionation section (30) to produce at least one heavy liquid product (106b) boiling primarily at a temperature greater than or equal to 350°C, the heavy liquid product containing a residual oil fraction having a boiling point greater than or equal to 540°C.

2. The method of claim 1, wherein: In step (a), the pyrolysis oil fraction (102) and the heavy hydrocarbon fraction (101) of the feedstock are premixed before being introduced into the at least one first hydroconversion reactor of the first hydroconversion stage (20).

3. The method of claim 1, wherein: In step (a), the pyrolysis oil fraction (102) and the heavy hydrocarbon fraction (101) of the feedstock are introduced into the at least one first hydroconversion reactor of the first hydroconversion section (20) respectively.

4. A process as claimed in any one of the preceding claims, wherein step (a) comprises a step of preheating the heavy hydrocarbon fraction (101), preferably to a temperature of 280°C to 450°C, and optionally a step of preheating the pyrolysis oil fraction (102), before introducing the feed into the first hydroconversion reactor of the first hydroconversion stage (20).

5. A method as described in any of the preceding claims, wherein the pyrolysis oil fraction (102) accounts for 1% to 45% by weight of the feedstock, preferably 2% to 30% by weight of the feedstock, preferably 2% to 25% by weight of the feedstock, and more preferably 3% to 20% by weight of the feedstock.

6. The method as claimed in any one of the preceding claims, wherein the feedstock consists of the pyrolysis oil fraction (102) and the heavy hydrocarbon fraction (101), the pyrolysis oil fraction (102) accounting for 1% to 45% by weight of the feedstock, preferably 2% to 30% by weight, and the heavy hydrocarbon fraction (101) accounting for 55% to 99% by weight of the feedstock, preferably 70% to 98% by weight.

7. The method according to any one of the preceding claims, wherein the pyrolysis oil fraction (102) is plastic pyrolysis oil.

8. The method according to any one of the preceding claims, wherein the heavy hydrocarbon fraction (101) is selected from crude oil, topped crude oil, atmospheric residue or vacuum residue produced by atmospheric distillation and / or vacuum distillation of crude oil or an effluent produced from a thermal conversion unit, a hydrotreating unit, a hydrocracking unit or a hydroconversion unit, an aromatic fraction extracted from a lubricant production unit, a deasphalted oil produced from a deasphalting unit, an asphalt produced from a deasphalting unit, a residue fraction produced from direct coal liquefaction, a vacuum distillate produced from direct coal liquefaction, or a mixture thereof.

9. The method according to claim 8, wherein the heavy hydrocarbon fraction (101) is a vacuum residue, preferably produced from primary fractionation of crude oil.

10. A method as claimed in any one of the preceding claims, comprising a separation step (c) of separating part or all of the first hydroconversion effluent (105) produced by step (b) to produce at least a heavy fraction boiling mainly at a temperature greater than or equal to 350° C., and also comprising a second hydroconversion step (d) of the heavy fraction.

11. A method as claimed in any one of the preceding claims, wherein the first hydroconversion section (20) in step (b) and the one or more hydroconversion reactors in the optional hydroconversion step (d) are mixed boiling-entrained bed reactors, and the method also includes a step of introducing a catalyst precursor (104) into the feedstock in a manner that forms a colloidal or molecular catalyst when the feedstock reacts with sulfur before injecting the feedstock into the at least one first mixed boiling-entrained bed reactor of the first hydroconversion section (20), the catalyst precursor (104) preferably comprising molybdenum 2-ethylhexanoate, and the colloidal or molecular catalyst preferably comprising molybdenum disulfide.

12. The process of any one of the preceding claims, wherein the first hydroconversion catalyst and the optional second hydroconversion catalyst comprise at least one Group VIII non-noble metal selected from nickel and cobalt, preferably nickel, and at least one Group VIB metal selected from molybdenum and tungsten, preferably molybdenum, and comprise an amorphous support, preferably alumina.

13. A process as claimed in any one of the preceding claims, wherein step (b) and optionally step (d) are carried out at a temperature of from 405°C to 450°C.

14. A process as claimed in any one of the preceding claims, wherein the optional intermediate separation step (c) is carried out in a separation section, and wherein the separation section and / or the fractionation section (30) in step (e) comprises means for washing at least one separated fraction by contact with an aqueous solution.

15. A method as described in any of the preceding claims, further comprising a step (f) of further processing the heavy liquid product (106b) and / or one or more other products from the fractionation step (e), wherein step (f) comprises at least one step selected from: hydrotreating, steam cracking, fluidized bed catalytic cracking, hydrocracking, deasphalting, lubricating oil extraction, and preferably a fixed bed hydrotreating step (f2) in a hydrotreating section, wherein the hydrotreating section preferably comprises at least one fixed bed reactor, wherein the reactor comprises n catalytic beds, n being an integer greater than or equal to 1, each catalytic bed comprising at least one hydrotreating catalyst, and wherein the hydrotreating section is fed with at least a portion of the liquid product from step e) and a gaseous stream comprising hydrogen to obtain a hydrotreating effluent.

16. A product obtained by the method according to any one of claims 1 to 15.

17. The hydroconversion effluent according to claim 16, obtained at the end of the first hydroconversion step (b) or the second hydroconversion step (d), and comprising a liquid fraction having a silicon content less than or equal to 5 weight ppm and / or a chlorine content less than or equal to 10 weight ppm, relative to the total weight of said liquid fraction of said effluent.

Citation Information

Cited By

  • Coprocessing circular and renewable feedstocks in an ebullated-bed (EB) reactor platform

    WO2026165280A1