Magnesium-lithium-aluminum alloy, method for producing said magnesium-lithium-aluminum alloy, and method for producing molded article comprising magnesium-lithium-aluminum alloy
By controlling the content ratio of lithium and aluminum in the magnesium alloy and adopting injection molding technology, the problem of the reduction of Young's modulus when the lithium content of magnesium alloy is increased is solved, and a lightweight magnesium alloy with excellent mechanical characteristics is achieved, reducing costs And improves forming stability.
Patent Information
- Application Number
- CN202280090748.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-11
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-01
AI Technical Summary
When existing magnesium alloys increase lithium content to achieve light weight, Young's modulus decreases, resulting in difficult rigid design of metal products and may offset the light weight effect.
The magnesium-lithium-aluminum alloy is used to control the content ratio of lithium and aluminum in the alloy (2-6.0% lithium, 5-10% aluminum), and the injection molding process is used to form a lightweight magnesium alloy with excellent mechanical characteristics. .
It realizes that under industrial stable process conditions, it provides lightweight magnesium alloys with excellent mechanical characteristics, improves plastic processing performance and corrosion resistance, reduces the use of lithium, reduces costs, and improves forming stability.
Smart Images

Figure GDA0005017544680000101 
Figure GDA0005017544680000121 
Figure GDA0005017544680000122
Abstract
Description
Technical Field
[0001] The present invention relates to a magnesium-lithium-aluminum alloy, a method for producing the magnesium-lithium-aluminum alloy, and a method for producing a molded product formed of the magnesium-lithium-aluminum alloy. Background Art
[0002] Magnesium alloy is one of the lightest materials among metals in practical use. In order to further reduce the weight, various studies and developments have been conducted on lithium-containing magnesium alloys to which lithium, which has a light specific gravity, has been added.
[0003] As such lithium-containing magnesium alloys, for example, high-lithium magnesium alloys containing 10.5 mass % or more of lithium, and Mg-Li-Al-Zn alloys containing aluminum and zinc in addition to lithium (for example, see Patent Document 1) are known.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6408037 Summary of the invention
[0007] In such lightweight magnesium-lithium alloys (Mg-Li alloys) and magnesium-lithium-aluminum alloys (Mg-Li-Al alloys), alloys containing a large amount of lithium and crystallizing into body-centered cubic (bcc) crystals have been developed from the viewpoint of achieving low specific gravity by containing a large amount of lithium, which is light in specific gravity, and improving the poor plastic workability of magnesium as a hexagonal close-packed crystal (hcp).
[0008] That is, the Mg-Li alloy presents a simple eutectic phase diagram. If about 5.7% by mass or more of lithium is added to magnesium, the solid solution β phase of lithium and the solid solution α phase of magnesium are crystallized together. If about 8.5% by mass or more of lithium is added, it becomes a single β phase. Since magnesium has an hcp structure, it is generally slightly poor in cold workability. Since lithium has a bcc structure, it can be expected that the plastic working performance will be improved through its crystallization.
[0009] However, as the lithium content increases, the Young's modulus tends to decrease. When designing a metal product for rigidity, if the Young's modulus is low, the wall needs to be thickened accordingly. Even if the specific gravity is reduced by adding lithium, there is a possibility that the lightweight effect of the metal product will be offset by the increase in wall thickness.
[0010] An object of the present invention is to solve the above-mentioned problems of magnesium alloys and to provide a lightweight magnesium alloy having excellent mechanical properties by an industrially stable process.
[0011] A magnesium-lithium-aluminum alloy as one embodiment of the present application contains magnesium, 2 to 6.0 mass % of lithium, and 5 to 10 mass % of aluminum.
[0012] In a method for manufacturing a magnesium-lithium-aluminum alloy which is one embodiment of the present application, a first raw material scrap formed of a magnesium-aluminum alloy and a second raw material scrap formed of a magnesium-lithium alloy containing magnesium and lithium are prepared, wherein the magnesium-aluminum alloy contains magnesium, 5 to 10 mass % of aluminum and 0 to 1 mass % of zinc, and these raw material scraps are mixed to obtain the above-mentioned magnesium-lithium-aluminum alloy.
[0013] In a method for manufacturing a magnesium-lithium-aluminum alloy which is another embodiment of the present application, a third raw material scrap formed of a magnesium-lithium-aluminum alloy and a fourth raw material scrap formed of a magnesium alloy that does not contain lithium are prepared, wherein the magnesium-lithium-aluminum alloy contains magnesium, lithium and aluminum, and the ratio of the lithium content to the aluminum content (Li / Al) is less than 8, and these raw material scraps are mixed to obtain the above-mentioned magnesium-lithium-aluminum alloy.
[0014] In a method for manufacturing a molded product formed of a magnesium-lithium-aluminum alloy as one embodiment of the present application, a first raw material scrap of a magnesium-aluminum alloy containing magnesium, 5 to 10% by mass of aluminum, and 0 to 1% by mass of zinc and a second raw material scrap of a magnesium-lithium alloy containing magnesium and lithium are prepared, and these raw material scraps are mixed to obtain the magnesium-lithium-aluminum alloy. Furthermore, the molded product is obtained by injection molding the obtained magnesium-lithium-aluminum alloy.
[0015] In a method for manufacturing a molded product formed of a magnesium-lithium-aluminum alloy as another embodiment of the present application, a third raw material scrap of a magnesium-lithium-aluminum alloy containing magnesium, lithium and aluminum and a ratio of the content of lithium to the content of aluminum (Li / Al) of less than 8 and a fourth raw material scrap of a magnesium alloy not containing lithium are prepared, and these raw material scraps are mixed to obtain the magnesium-lithium-aluminum alloy. Then, the molded product is obtained by injection molding the obtained magnesium-lithium-aluminum alloy.
[0016] Effects of the Invention
[0017] According to the magnesium-lithium-aluminum-based alloy and the method for producing the same which is one embodiment of the present application, a lightweight magnesium alloy having excellent mechanical properties can be provided.
[0018] In addition, according to the method for producing a molded product made of a magnesium-lithium-aluminum alloy as one embodiment of the present application, a molded product made of a lightweight magnesium alloy having excellent mechanical properties can be provided by an industrially stable process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1This is a graph showing data of tensile strength in Examples and Comparative Examples.
[0020] Figure 2 This is a graph showing data of elongation at break in Examples and Comparative Examples.
[0021] Figure 3 This is a graph showing data of yield strength in Examples and Comparative Examples.
[0022] Figure 4 This is a graph showing data of Young's modulus in Examples and Comparative Examples.
[0023] Figure 5 This is a graph showing the data of corrosion resistance in Examples and Comparative Examples.
[0024] Figure 6 It is a graph showing the diffraction patterns obtained by XRD in Examples and Comparative Examples. DETAILED DESCRIPTION
[0025] Hereinafter, the magnesium-lithium-aluminum alloy of the present invention, a method for producing the magnesium-lithium-aluminum alloy, and a method for producing a molded product made of the magnesium-lithium-aluminum alloy will be described with reference to one embodiment.
[0026] [Magnesium-lithium-aluminum alloy]
[0027] The magnesium-lithium-aluminum alloy as one embodiment of the present invention is a magnesium alloy containing magnesium (Mg) as a main component and further containing predetermined amounts of lithium (Li) and aluminum (Al).
[0028] (lithium)
[0029] As is well known, lithium (Li) is a component that has the effect of achieving lightweight magnesium alloys and improving the plastic workability of the magnesium alloys. In the present embodiment, while ensuring the above-mentioned effects, the formability during injection molding is also taken into consideration, and the lithium content in the magnesium-lithium-aluminum alloy is set to 2 to 6.0% in terms of mass % (hereinafter, also simply expressed as "%". In this specification, "%" means mass % unless otherwise specified). The lithium content preferably has a lower limit of 4.8% or more. In addition, it is preferred to set the upper limit to 5.8% or less.
[0030] It is believed that if the lithium content exceeds 6.0%, it is easy to crystallize the β phase (Li). When the magnesium-lithium-aluminum alloy is subjected to plastic processing such as rolling and extrusion, the β phase is preferably present in order to improve the processability. However, in the equilibrium phase diagram of a simple Mg-Li alloy, if the lithium content exceeds 5.7%, the β phase is crystallized, but because it contains other alloy components such as Al and Zn, the phase diagram may change, and in a casting method with a fast cooling rate such as injection molding, it will not reach a perfect equilibrium state. Therefore, in the composition of the present embodiment, it is difficult to crystallize the β phase even if it exceeds 5.7%, which has been actually confirmed.
[0031] On the other hand, when it is envisaged that the material is applied to a process based on a casting method, the β phase of magnesium-lithium is not only unnecessary during the process, but also may easily adhere to the screw in the case of injection molding, easily adhere to the mold and produce mold residue, which may become a cause of deterioration in productivity.
[0032] If the lithium content is less than 2%, the effect of reducing the weight of the magnesium alloy is hardly obtained. In order to sufficiently reduce the weight, the lithium content is preferably 4% or more.
[0033] (aluminum)
[0034] Aluminum (Al) is a component that is hardly dissolved in the magnesium matrix phase and is concentrated at the solidification front of the magnesium primary crystals, resulting in good fluidity of the alloy material before forming a eutectic compound with magnesium or calcium (Ca).
[0035] The aluminum content is preferably 5-10% in the alloy. Aluminum also has the effect of lowering the melting point of the alloy material, but when it is less than 5%, the melting point will not be sufficiently lowered, so it is necessary to increase the melting temperature of the alloy material during alloy smelting and casting, and there is a concern that the operability will be reduced. In addition, if the aluminum content exceeds 10%, the intermetallic compounds increase, so there is a tendency for the casting crack sensitivity to increase and the corrosion resistance to deteriorate. Therefore, from the perspective of making it difficult to produce adverse conditions during casting and not causing problems with corrosion resistance, it is preferred to contain more than 5% aluminum.
[0036] (Zinc)
[0037] Zinc (Zn) is an optional component that improves strength. Zinc can improve the castability of the alloy, but it reduces creep resistance and increases casting crack sensitivity. The content of zinc in the alloy is set to 1% or less, and zinc may not be contained. When zinc is contained, its content is preferably 0.35 to 1%.
[0038] (manganese)
[0039] Manganese (Mn) is a component that combines with aluminum to form an intermetallic compound, dissolves iron (Fe) as an impurity element, and thereby suppresses the deterioration of corrosion resistance. Manganese is an optional component. When manganese is contained, its content is preferably 0.15 to 0.8%. When it is less than 0.15%, the above-mentioned effect cannot be fully obtained, and when it exceeds 0.8%, the melting yield may be deteriorated.
[0040] (other)
[0041] In the magnesium-lithium-aluminum alloy of the present embodiment, magnesium is the main component, and the remainder other than the components described above is basically magnesium, but other components may be contained within a range that does not hinder the effects of the present invention. As such components, for example, unavoidable impurities that are unavoidably contained during alloy production can be exemplified.
[0042] As such inevitable impurities, specifically, iron, copper, nickel, etc. are listed. Such inevitable impurities are preferably not substantially contained in the magnesium-lithium-aluminum alloy, and "not substantially contained" here means that the contents in the alloy are respectively 0.03% or less for iron, 0.25% or less for copper, and 0.01% or less for nickel.
[0043] (Lithium to aluminum content ratio)
[0044] The magnesium-lithium-aluminum alloy in the present embodiment is characterized in that each blending amount satisfies the above range, but it is preferred that the lithium content and the aluminum content are further adjusted to a predetermined ratio.
[0045] Most of the magnesium-lithium-aluminum alloys known so far are alloys in which the aluminum content is equal to the lithium content or the aluminum content is greater than the lithium content in terms of mass %, but in the present embodiment, it is preferred that the lithium content is reduced so that the β phase derived from lithium is not crystallized, and a required amount of aluminum is contained in order to improve the mechanical properties and corrosion resistance. That is, by setting the lithium content and the aluminum content to a predetermined relationship, an alloy can be realized that achieves lightweight and improved formability, and also ensures mechanical properties and corrosion resistance.
[0046] Specifically, the predetermined ratio is preferably a ratio of the lithium content to the aluminum content (Li / Al) in the range of 0.5 to 0.9, and more preferably in the range of 0.5 to 0.85.
[0047] In addition, since lithium has a small atomic weight, when Li / Al is 0.5 to 0.9 in terms of mass%, Li / Al becomes about 2 in terms of atomic%. For example, an alloy of 4 mass% Li-8 mass% Al-88 mass% Mg becomes 12.83 atomic% Li-6.6 atomic% Al-80.58 atomic% Mg (wherein, for the symbol of the alloy composition, the numerical value before the element represents the content of the element in the alloy, and when the magnesium content is omitted, the remainder other than the recorded element content is magnesium). For materials containing these three components, according to the ternary phase diagram of the known literature, the α phase of magnesium is distributed in the range from 100% magnesium content to the alloy containing more lithium relative to aluminum. That is, by containing more lithium and aluminum in the range where the α phase is distributed and quenching the alloy during injection molding, it is possible to make aluminum and lithium solid-dissolve as much as possible and adjust the alloy composition in the direction of not crystallizing the β phase, which is one of the means to improve mechanical properties and corrosion resistance.
[0048] Specifically, in the embodiment, the metallographic structure in the alloy is formed of α-Mg and Al-Li intermetallic compounds in which Li is solid-dissolved. On the other hand, the β phase (Mg 17 Al 12 ) and β phase (Li) are reduced and substantially free of the metallographic structure. By reducing the β phase in this way, the influence on the required properties (especially, adhesion to the molding die in injection molding) can be eliminated.
[0049] [Method for producing magnesium-lithium-aluminum alloy]
[0050] The method for producing a magnesium-lithium-aluminum alloy of the present embodiment can be carried out by preparing raw materials of magnesium, lithium, aluminum and other components so as to have the above-described formulation and mixing these raw materials by a known method.
[0051] As the raw material used here, powdered raw material crumbs are preferably used. As the raw material crumbs, raw material crumbs of suitable size can be used according to the manufacturing method, and it is preferable that the raw material crumbs can be simply heated, melted and mixed. As the raw material crumbs, for example, raw material crumbs with an average particle size of 0.5 to 2.5 mm are preferred, and raw material crumbs with an average particle size of 1.0 to 2.0 mm are more preferred.
[0052] As an example of a method for manufacturing the alloy, for example, the following method can be listed: (a1) preparing a first raw material scrap formed of a magnesium-aluminum alloy and a second raw material scrap formed of a magnesium-lithium alloy containing magnesium and lithium, wherein the magnesium-aluminum alloy contains magnesium, 5 to 10 mass% of aluminum and 0 to 1 mass% of zinc, and then, (b1) mixing the first raw material scrap and the second raw material scrap to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass% of lithium and 5 to 10 mass% of aluminum.
[0053] In addition, as another example of a method for manufacturing the alloy, for example, the following method can be listed: (a2) preparing a third raw material scrap formed of a magnesium-lithium-aluminum alloy and a fourth raw material scrap formed of a magnesium alloy not containing lithium, wherein the third raw material scrap contains magnesium, lithium and aluminum, and the ratio of the lithium content to the aluminum content (Li / Al) is less than 8, and then, (b2) mixing the third raw material scrap and the fourth raw material scrap to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum.
[0054] The first to fourth raw material crumbs mentioned above may be obtained from commercially available raw material crumbs or may be prepared so as to become specific blending components.
[0055] [Method for producing molded product composed of magnesium-lithium-aluminum alloy]
[0056] The manufacturing method of the molded product is as follows: the alloy material obtained by the manufacturing method of the above-mentioned alloy is made into a molded product by using a casting method and a forming mold. As the casting method performed here, various methods generally known can be used, and high-pressure casting methods such as injection molding, die casting, extrusion casting, and metal injection molding can be listed. The above-mentioned alloy material is a material suitable for high-pressure casting. The conditions of these casting methods are not particularly limited, but since it is a magnesium alloy containing lithium with ignition properties, injection molding without melting the alloy in the atmosphere is more desirable. In injection molding, in addition to molding in a completely molten state, molding in a semi-molten state can also be performed.
[0057] In the high pressure casting method, the molten alloy (including the semi-molten state) has high fluidity, so even when forming a thin product, it can be cast with good fluidity, and a complex shape that cannot be formed by rolling or extrusion can be formed by near net shape, thereby obtaining a high product yield. In addition, the obtained parts can ensure excellent properties.
[0058] Hereinafter, a case where injection molding is used will be described in detail as an example.
[0059] As an example of a method for manufacturing the molded product, for example, the following method can be listed: (a1) preparing a first raw material scrap formed of a magnesium-aluminum alloy and a second raw material scrap formed of a magnesium-lithium alloy containing magnesium and lithium, wherein the magnesium-aluminum alloy contains magnesium, 5 to 10 mass% of aluminum and 0 to 1 mass% of zinc, (b1) mixing the first raw material scrap and the second raw material scrap to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass% of lithium and 5 to 10 mass% of aluminum, and further, (c1) injection molding the magnesium-lithium-aluminum alloy obtained by the above-mentioned (b1) step.
[0060] In addition, as another example of the method for manufacturing the molded product, for example, the following method can be listed: (a2) preparing a third raw material scrap formed by a magnesium-lithium-aluminum alloy and a fourth raw material scrap formed by a magnesium alloy that does not contain lithium, wherein the magnesium-lithium-aluminum alloy contains magnesium, lithium and aluminum, and the ratio of the lithium content to the aluminum content (Li / Al) is less than 8, (b2) mixing the third raw material scrap and the fourth raw material scrap to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum, and (c2) injection molding the magnesium-lithium-aluminum alloy obtained by the above-mentioned (b2) step.
[0061] The manufacturing methods of the molded products illustrated in these examples are respectively obtained by adding the (c1) step and the (c2) step to the manufacturing method of the alloy mentioned above, and the molded products are obtained by injection molding. Here, injection molding can be implemented using a known method. In the manufacturing method of the molded product, it is characterized in that two raw material chips are mixed. In the case of using two kinds of raw material chips, it can be set as follows: the two kinds of raw material chips are pre-sorted according to the target mass ratio and mixed in one container, or two hoppers for inputting raw material chips are prepared according to the raw material chips, and a specified amount of raw material chips is supplied from each hopper in a specified matching manner. In addition, in the case of using one or more hoppers to input two kinds of raw material chips, a feeder for supplying each raw material chip is prepared, and each raw material chip is supplied in a manner to achieve the target mixing mass ratio.
[0062] When a molded product is obtained by injection molding, since a melting furnace such as die casting is not used, the risk of combustion of the easily combustible lithium-containing magnesium alloy can be minimized.
[0063] In addition, for example, magnesium alloys with a high lithium content, such as Mg-14% Li-1% Al (LA141), have a narrow semi-melting temperature range. When molded by injection molding, they may melt rapidly in the middle of being conveyed by a screw, and the molding may be unstable. In contrast, by suppressing the amount of lithium, the semi-melting temperature range becomes wider, and the molding stability can be improved. Moreover, even when Mg-7% Li-7% Al-1% Zn (LAZ771), a lithium-containing magnesium alloy with poor molding stability, is used as a raw material, the molding stability is improved by mixing with the generally used and molding-stable AZ91D (Mg-9% Al-1% Zn) chips for injection molding, and the mixing ratio is easily adjusted, so that a molded product formed of a desired alloy component can be obtained with a simple operation.
[0064] The molded product obtained by the method for manufacturing a molded product of the present embodiment can be used as a lightweight, high-strength, and corrosion-resistant component in various applications. Therefore, it can be expected that the use of the magnesium alloy products will be expanded to automotive parts and various portable devices that require these characteristics. Moreover, compared with plastic products, these magnesium alloy products can be recycled and reused, and can also contribute to the protection of the global environment.
[0065] The magnesium-lithium-aluminum alloy, the method for producing the magnesium-lithium-aluminum alloy, and the method for producing a formed product according to the present embodiment have been described above. The magnesium-lithium-aluminum alloy obtained in this manner also has the following advantages.
[0066] (1) The price of lithium is very high. Compared with the raw materials of magnesium and aluminum, which are about 200 to 300 yen / kg, the price of lithium is more than 10 times that of 6,000 to 10,000 yen / kg. Therefore, the more lithium is contained, the higher the price of the alloy. However, according to the magnesium-lithium-aluminum alloy of the above embodiment, the amount of lithium can be suppressed, and the manufacturing cost can be suppressed.
[0067] (2) Magnesium has a very low natural potential and is inferior to iron and aluminum in corrosion resistance. Lithium has a lower potential than magnesium and is an active metal, so increasing the amount of lithium added further deteriorates the corrosion resistance of the magnesium alloy. According to the magnesium-lithium-aluminum alloy of the above embodiment, the amount of lithium can be suppressed and the corrosion resistance can be improved.
[0068] (3) Since magnesium is an active metal, if it melts in the atmosphere, it will emit a fierce flash and burn. In addition, if the fine powder generated during machining, etc. is not properly handled and ignites in the atmosphere, there is also the possibility of a dust explosion. Lithium is a metal that is more active than magnesium. By adding a large amount of lithium to magnesium, it becomes more flammable and the danger increases. According to the magnesium-lithium-aluminum alloy of the above embodiment, the amount of lithium can be suppressed, and the combustibility of the magnesium-lithium-aluminum alloy can be improved.
[0069] (4) For Mg-Li alloys, the temperature difference between the solidus and liquidus in the phase diagram is very small, and the solid-liquid coexistence temperature range is very narrow. Therefore, if heated, it will melt all at once within a narrow temperature range. Therefore, in injection molding in which the alloy is melted while being transported by a screw, the melting characteristics are not stable, making it difficult to perform injection molding. In addition, magnesium alloy chips containing about 5.7% by mass or more of lithium have a β phase with a bcc structure, so they are easy to flow plastically. If they are transported by a rotating screw, they will stick to the screw and be difficult to form. Since the solid-liquid coexistence temperature range is narrow, solidification cracks are also easy to occur in the casting method. In this regard, according to the above-mentioned embodiment, the solid-liquid coexistence temperature range can be expanded, and the injection molding property can be improved.
[0070] Example
[0071] Hereinafter, the magnesium-lithium-aluminum alloy of the present embodiment, the method for producing the magnesium-lithium-aluminum alloy, and the method for producing a molded product formed of the magnesium-lithium-aluminum alloy will be described in detail using examples and comparative examples.
[0072] (Examples 1 to 5, Comparative Examples 1 to 2)
[0073] As raw material chips, LAZ771 (Mg-7% Li-7% Al-1% Zn; manufactured by Anritsu Materials Technology Co., Ltd. (Taiwan, China)) and AZ91D (Mg-9% Al-0.7% Zn; manufactured by Chuo Industries, Ltd.) were prepared.
[0074] A magnesium alloy injection molding machine manufactured by Nippon Steel Works, Ltd. (trade name: JLM280MGIIe, mold clamping force: 2740 kN, barrel inner diameter: 51 mm) was used. The barrel temperature was set to 723K for the hopper supplying chips and 873K for the molten portion at the tip.
[0075] LAZ771 and AZ91D as raw material chips were supplied to a hopper in a predetermined mixing ratio as shown in Table 1, and injection molding was performed in a mold (mold temperature setting: 473K), and a flat plate with a width of 100 mm, a length of 200 mm, and a thickness of 2 mm formed of a magnesium-lithium-aluminum alloy was obtained as a molded body. The element contents in the alloy of the obtained molded body are shown in Table 1.
[0076] [Table 1]
[0077] Table 1
[0078]
[0079] [characteristic]
[0080] The alloy obtained above was subjected to a tensile test (tensile strength, elongation at break, yield strength, and Young's modulus) and XRD measurement as follows.
[0081] (Tensile test)
[0082] A dumbbell-shaped No. 13B test piece in accordance with JIS was cut out from the plate-shaped molded product obtained in each example to prepare a sample.
[0083] The obtained samples were subjected to a tensile test using an INSTRON 5982 tensile testing machine at a test speed of 10 MPa / s (the test speed after the yield strength was set to 11.4 mm / min). In this test, the values were measured at the three locations of the sample: the operating side, the central part, and the opposite side of the operating side. The values of each measured location and their average values were calculated for tensile strength, elongation at break, yield strength, and Young's modulus. These results are shown in the table and the figure. In addition, the tensile strength is shown in Table 2 and Figure 1 The elongation at break is shown in Table 3 and Figure 2 The yield strengths are shown in Table 4 and Figure 3 The Young's modulus is shown in Table 5 and Figure 4 middle.
[0084] (Corrosion resistance)
[0085] Prepare 5% salt water, spray the 5% salt water onto the sample, and leave it at 35°C for 24 hours. The mass before and after the test was measured, and the mass change ratio (%) was calculated. The test results are shown in Table 6 and Figure 5 In general, the less the weight loss due to corrosion, the better the corrosion resistance. However, in this embodiment, due to safety considerations, the removal of corrosion products using hydrofluoric acid was not implemented. The more corrosion products, that is, the greater the weight gain due to corrosion, the worse the corrosion resistance, and the less the weight gain due to corrosion, the better the corrosion resistance.
[0086] (XRD)
[0087] The crystals contained in the molded products obtained in each example were measured by X-ray diffraction. As an X-ray diffraction device, a multifunctional X-ray diffraction device Empyrean (manufactured by Spectris Co., Ltd., trade name) was used, and the target was Co, the tube voltage was 45 kV, and the tube current was 40 mA. The obtained diffraction pattern is shown in Figure 6 middle.
[0088] In addition, Figure 6 The results of Examples 1 to 5 and Comparative Examples 1 to 2 are shown together. In addition, a symbol is given above the peak to the crystal corresponding to each peak, and the crystal represented by each symbol is shown together at the upper right of the graph.
[0089] [Table 2]
[0090] Table 2
[0091]
[0092] [Table 3]
[0093] Table 3
[0094]
[0095] [Table 4]
[0096] Table 4
[0097]
[0098] [Table 5]
[0099] Table 5
[0100]
[0101] [Table 6]
[0102] Table 6
[0103]
[0104] According to the above results, the magnesium-lithium-aluminum alloy of the present embodiment has a significantly improved strength by using 40% LAZ771 (Mg-2.9% Li-8.1% Al-0.8% Zn) compared to the alloy of AZ91D alone (0% LAZ771), and maintains a strength substantially the same as that of 50% LAZ771, 60% LAZ771, 70% LAZ771, and 80% LAZ771. However, there is a tendency for the strength to be slightly reduced in the case of LAZ771 alone (100% LAZ771), and if the known results of forming by mixing LA141 (Mg-14% Li-1% Al) with a high lithium content and AZ91D are considered, it is known that there is a tendency for the strength to be higher when the lithium content is about 2 to 6%. This tendency also exists in the 0.2% yield strength.
[0105] It is also known that the Young's modulus, which is very important in the case of rigidity design, increases in the alloy with 40% LAZ771 relative to AZ91D alone (0% LAZ771), and gradually increases until 80% LAZ771. In addition, there is a tendency that the Young's modulus does not increase even if the LAZ771 is further increased. Generally, the Young's modulus of a metal does not change much depending on the alloy composition. In order to increase the rigidity, a metal-based composite material having a mixture of inorganic particles, fibers, etc. has to be produced, but the composite material is difficult to produce, the cost is high, and the quality is unstable. On the other hand, it is a new insight that the Young's modulus is increased by adding a specified amount of LAZ771. Based on this insight, the inventors of the present application have discovered that a magnesium-lithium-aluminum alloy having stable rigidity can be obtained using the present embodiment.
[0106] In addition, the XRD analysis results of the molded product show that the molded product of this embodiment contains α phase (Mg) and AlLi as an intermetallic compound phase. Therefore, it is clear that AlLi greatly contributes to the improvement of Young's modulus, and it can also be said that the molded product is characterized by having α phase and AlLi phase.
[0107] In addition, in the case of 100% LAZ771 described in Patent Document 1, in addition to the α phase, the β phase was also detected in the XRD analysis. In an alloy with a small amount of Al and 5.7% or more of lithium added, increasing the amount of lithium results in the formation of β phase (Li) instead of AlLi, and it is believed that the Young's modulus cannot be further improved. Therefore, it is known that the composition adjustment of forming AlLi instead of β phase is important for improving mechanical properties.
[0108] In addition, generally, lithium-containing magnesium alloys have poor corrosion resistance, but after the salt spray test was performed on the obtained molded products, although the corrosion resistance of 100% LAZ771 was still poor, when 60-80% LAZ771 was mixed, the corrosion resistance was better than that of AZ91D (0% LAZ771). Although the reason is still unclear, it is believed that not crystallizing the β phase (Li) but crystallizing the AlLi phase is also effective in improving the corrosion resistance.
[0109] As described above, when lithium is added to the extent of β-phase crystallization, although the specific gravity becomes lighter, the corrosion resistance deteriorates and the improvement of mechanical properties cannot be expected. In contrast, it is clear that the lithium-containing magnesium alloy in which the lithium amount is suppressed to an appropriate amount and the β-phase does not exist and has an AlLi phase instead has a lighter specific gravity and improved mechanical properties and corrosion resistance than the magnesium alloy not containing lithium, and the lithium-containing magnesium alloy is considered to be a material suitable for lightweight parts.
[0110] As mentioned above, the invention completed by the inventors of the present application has been specifically described based on the embodiments and examples, but the present invention is not limited to the above-mentioned embodiments or examples, and it goes without saying that various changes can be made within the scope not departing from the gist thereof.
Claims
1. A magnesium-lithium-aluminum alloy comprising magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum.
2. The magnesium-lithium-aluminum alloy according to claim 1, wherein It also contains 0.35 to 1% by mass of zinc and 0.15 to 0.8% by mass of manganese.
3. The magnesium-lithium-aluminum alloy according to claim 1, wherein: The ratio of the lithium content to the aluminum content (Li / Al) is 0.5 to 0.
9.
4. The magnesium-lithium-aluminum alloy according to claim 2, wherein: The lithium is 4.8 to 6.0 mass % lithium.
5. The magnesium-lithium-aluminum alloy according to claim 1, wherein The metallographic structure of the magnesium-lithium-aluminum alloy is composed of α-Mg and Al-Li intermetallic compounds in which Li is solid-dissolved, and does not have β-phase Mg 17 Al 12 And β phase Li.
6. A method for producing a magnesium-lithium-aluminum alloy, comprising the following steps: (a1) step of preparing a first raw material scrap composed of a magnesium-aluminum alloy and a second raw material scrap composed of a magnesium-lithium alloy containing magnesium and lithium, wherein the magnesium-aluminum alloy contains magnesium, 5 to 10% by mass of aluminum, and 0 to 1% by mass of zinc; and In step (b1), the first raw material chips and the second raw material chips are mixed to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum.
7. A method for producing a magnesium-lithium-aluminum alloy, comprising the following steps: (a2) step of preparing a third raw material scrap formed of a magnesium-lithium-aluminum alloy and a fourth raw material scrap formed of a magnesium alloy not containing lithium, wherein the magnesium-lithium-aluminum alloy contains magnesium, lithium and aluminum, and the ratio of the content of lithium to the content of aluminum, Li / Al, is less than 8; and In step (b2), the third raw material chips and the fourth raw material chips are mixed to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum.
8. A method for producing a molded product formed of a magnesium-lithium-aluminum alloy, comprising the following steps: (a1) step of preparing a first raw material scrap composed of a magnesium-aluminum alloy and a second raw material scrap composed of a magnesium-lithium alloy containing magnesium and lithium, wherein the magnesium-aluminum alloy contains magnesium, 5 to 10% by mass of aluminum, and 0 to 1% by mass of zinc; (b1) step of mixing the first raw material chips and the second raw material chips to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum; as well as (c1) The magnesium-lithium-aluminum alloy obtained in the above-mentioned step (b1) is injection molded.
9. A method for producing a molded product formed of a magnesium-lithium-aluminum alloy, comprising the following steps: (a2) a step of preparing a third raw material scrap formed of a magnesium-lithium-aluminum alloy and a fourth raw material scrap formed of a magnesium alloy not containing lithium, wherein the magnesium-lithium-aluminum alloy contains magnesium, lithium and aluminum, and the ratio of the lithium content to the aluminum content (Li / Al) is less than 8; (b2) step of mixing the third raw material chips and the fourth raw material chips to obtain a magnesium-lithium-aluminum alloy containing magnesium, 2 to 6.0 mass % of lithium and 5 to 10 mass % of aluminum; and (c2) The magnesium-lithium-aluminum alloy obtained in the above-mentioned step (b2) is injection molded.