Seed substrate for high-characteristic epitaxial growth, method for manufacturing seed substrate for high-characteristic epitaxial growth, semiconductor substrate, and method for manufacturing semiconductor substrate
By using composite ceramic core and Si<111> single crystal layer on the Group III nitride substrate, the problem of insufficient thermal conductivity, strength and warpage of the existing Group III nitride substrate is solved, and high thermal conductivity and high thermal conductivity are achieved The strength and low warping substrate reduces production costs and is suitable for high-frequency and high-output devices.
Patent Information
- Application Number
- CN202380027724.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-02-02
- Publication Date
- 2024-11-01
AI Technical Summary
The existing Group III nitride substrates have shortcomings in high thermal conductivity, high strength, high dimensional accuracy and low warpage, and are costly, making it difficult to meet the needs of high output and fine refinement.
A composite ceramic core formed by a group III nitride polycrystalline ceramic and a group III or group IV nitride or oxide fibrous single crystal are used, and a sealing layer of 0.05 to 1.5 μm and a planarization layer of 0.5 to 3 μm are combined and the A Si<111> single crystal seed layer of 0.04 to 1.5 μm is provided on it to achieve surface smoothness by covering and grinding of the sealing layer and the flat layer, reducing thermal stress and reducing crystallization defects.
It significantly improves thermal conductivity and mechanical strength, reduces warpage and cost, and realizes a high-characteristic and low-priced seed substrate for Group III nitride epitaxial growth, suitable for high-output and high-frequency equipment.
Smart Images

Figure CN118891404A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a seed substrate for epitaxy of group III nitrides having high characteristics such as aluminum nitride (AlN), gallium aluminum nitride (Al x Ga 1-x N (where 0 < x < 1), gallium nitride (GaN), etc., which have high thermal conductivity, high strength, high dimensional accuracy, low warpage, few defects, etc., and a method for manufacturing the same. That is, it relates to a seed substrate for epitaxial growth of AlN, Al x Ga 1-x N (0 < X < 1), GaN-based, etc., group III nitride epitaxial growth seed substrates and manufacturing methods thereof, and semiconductor substrates using the same and manufacturing methods thereof. Background Art
[0002] Crystal substrates of group III nitrides such as AlN-based and GaN-based have a wide bandgap, short-wavelength luminescence, high breakdown voltage, and excellent high-frequency characteristics. Therefore, substrates of group III nitrides are expected to be applied to devices such as light-emitting diodes (LEDs), lasers, Schottky diodes, power devices, and high-frequency devices. For example, AlN-based crystal substrates are used instead of mercury lamps for the purpose of sterilizing ballast water on cruise ships and recently for the purpose of removing the new coronavirus, etc. The demand for AlN and / or Al x Ga 1-x N (0.5 < X < 1) single crystal substrates is increasing day by day.
[0003] However, the current situation is that: regarding these AlN and / or Al x Ga 1-x N (0.5 < X < 1) single crystal substrates, for example, regarding AlN single crystal substrates, as described in Non-Patent Document 1 and Non-Patent Document 2, since AlN does not have a melting point, it is difficult to manufacture from silicon (Si) single crystals, etc. using a general solution method. It uses silicon carbide (SiC) and AlN as seeds and is manufactured by a sublimation method (modified Rayleigh method) at 1700 - 2250 °C in an N2 atmosphere, or, as disclosed in Patent Document 1 and Non-Patent Document 3, is fabricated by a hydride vapor phase growth (HVPE) method on a sapphire substrate or an AlN substrate obtained by the sublimation method. The crystal growth of AlN single crystals by the sublimation method requires high temperature. Therefore, due to device limitations, the current situation is that it is a small-diameter substrate with a maximum diameter of inches, which is extremely expensive. The dislocation density of AlN single crystals obtained by the sublimation method is < 10 5 cm -2On the other hand, there are the following disadvantages: the contamination of carbon and metal impurities from carbon materials such as crucibles and insulation materials causes crystal coloring, low resistivity, and low ultraviolet transmittance. On the other hand, the AlN single crystal made by the hydride vapor phase growth (HVPE) method on a sapphire substrate is relatively cheap and less colored, but due to the difference in lattice constants between AlN and sapphire, AlN crystals produce a large number of defects and have low resistivity. In addition, the dislocation density of the AlN crystal obtained by HVPE film formation on the AlN substrate of the sublimation method is relatively small, and the defect is small, but due to the contamination of the coloring matter of the AlN from the base substrate, the transmittance relative to deep ultraviolet luminescence is low, and the resistivity is low. In addition, since the expensive sublimation method AlN crystal is directly used as the base substrate that also serves as a seed, there is a disadvantage of extremely high cost.
[0004] As described above, AlN has low quality and high price, and even if it is used to manufacture devices for various purposes, the expected characteristics cannot be obtained. In addition, it is difficult to cope with heat dissipation, dimensional accuracy, and warping in response to the recent demands for high output and miniaturization, which hinders the widespread popularization and expansion of the use of these substrates.
[0005] Regarding GaN-based substrates, bulk GaN substrates obtained by growing GaN crystals in liquids such as liquid ammonia or sodium flux have fewer defects and high quality, but require high-temperature and high-pressure equipment, so they are extremely expensive. In addition, since the AlN substrate of the above-mentioned sublimation method is directly used as a base substrate that also serves as a seed, the cost is extremely high. On the other hand, if the MOCVD method or the hydride vapor phase growth method (HVPE method, THVPE method) for crystal growth in the gas phase is used to make GaN crystals grow heteroepitaxially on sapphire substrates, in principle, high-quality and large-scale crystals can be achieved, but in fact, the lattice constant and thermal expansion coefficient of the generated GaN crystals are significantly different from those of the sapphire of the base substrate, so that multiple crystal defects and cracks are generated during manufacturing, and high-quality crystals cannot be obtained.
[0006] On the other hand, with the recent start of 5G communications and the development of electric vehicles, GaN-based crystalline substrates require higher high-frequency characteristics and greater pressure resistance. At the same time, they require increased output power, miniaturization, and further high thermal conductivity, high mechanical strength, high dimensional accuracy, and low warpage associated with electric vehicles, just like AlN-based crystalline substrates. Along with the large-diameter substrates, countermeasures for these are increasingly sought. Therefore, for crystalline substrates of group III nitrides such as AlN and GaN in recent years, on the basis of the long-standing requirements of fewer defects and lower prices, there is an urgent need to improve the above-mentioned high thermal conductivity, high strength, high dimensional accuracy, or low warpage. However, the current situation is that, like AlN, GaN-based crystalline substrates have basically not improved in response to these new requirements.
[0007] As one of the solutions to these problems, Patent Document 2 discloses a so-called QST (trade name) substrate of a pasted substrate, which includes a supporting substrate and a planarizing layer such as SiO2 on the upper surface of the supporting substrate, wherein the supporting substrate has an AlN ceramic core and a sealing layer that uses a multilayer film of SiO2 / P-Si / SiO2 / Si3N4 to seal the AlN ceramic core, and the so-called QST (trade name) substrate of the pasted substrate also includes a seed layer, wherein the seed layer is a thin film transfer Si on the upper surface of the planarizing layer. <111> Obtained as seed crystals.
[0008] However, in the above patents, if the thickness of the multilayer films sealing the core or the sealing layer, planarization layer, and seed layer is not well balanced, a large amount of thermal stress caused by the difference in thermal expansion coefficient will be generated, and cracks and defects will be easily generated between the layers, or the supporting substrate will be easily warped and deformed. <111> This can cause contamination and various deformations caused by the diffusion of impurities in the core of the AlN ceramic. As a result, the epitaxially grown film often exhibits low properties with many crystal defects, or reduces thermal conductivity and dimensional stability, or further causes Si <111> The yield rate when the thin film is transferred to the supporting substrate is reduced. In addition, Si may be derived from a seed crystal of a different type from the above. <111> It is hoped that the defects of the epitaxial growth film itself can be improved together.
[0009] Therefore, the inventors firstly focused on reducing the thermal stress between the layers of the seed Si <111> The relationship between the properties of the epitaxial film and the properties of the epitaxial film was thoroughly investigated and it was found that: while reducing the thermal stress between the layers, the seed Si <111> The number of OSFs (oxidation induced stacking faults) contained in the sample is extremely important. In particular, it was found that the number of OSFs contained in the sample is 10 / cm 2 In the following case, the subsequent epitaxial growth film has very few crystal defects and is good, and related patent applications have been filed first (Japanese Special Application 2021-038731 (filing date: March 10, 2021) and Japanese Special Application 2021-098993 (filing date: June 14, 2021), which were not yet disclosed when the present invention was applied for).
[0010] However, the improvements therein are still insufficient in terms of improving thermal conductivity, dimensional accuracy, strength, or warpage resistance, which are indispensable for the recent advanced new applications, and further improvements / measures are required.
[0011] Polycrystalline ceramics of group III nitrides also have objects with high thermal conductivity depending on their type, but the thermal resistance becomes large at the grain boundaries such as the melting joint surface between the polycrystalline grains of the ceramic raw material or the sintering aid, and it cannot be expected to be above a certain specified value. For example, even AlN polycrystalline ceramics, which are said to have high thermal conductivity, usually have an upper limit of about 170W / mK. In addition, the mechanical strength (fracture toughness) of AlN ceramics is weak, at ~3Mpa·m 1 / 2 Therefore, it is insufficient in terms of thermal conductivity and mechanical strength required for recent high output and EV, and further, the low dimensional accuracy and low warpage caused by the low mechanical strength are also serious problems.
[0012] As a method for achieving high thermal conductivity and high strength, non-patent document 5 discloses adding fibrous or whisker-shaped single crystals to polycrystalline ceramics. However, in the pasting substrate where nanometer-level smoothness is indispensable, no example of using fibrous or whisker-shaped single crystals is seen. This is because: the fibrous or whisker-shaped single crystals added to the polycrystalline ceramic float to the surface and cannot form a smooth surface at the nanometer level. Even if you try to smooth it by grinding, the height difference of the fibers or whiskers will occur frequently, and the surface smoothness of Ra below 0.2nm required for pasting cannot be obtained. Therefore, the general understanding so far is that it is completely inappropriate to introduce fibrous or whisker-shaped single crystals into the pasting substrate.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent No. 6042545
[0016] Patent Document 2: Japanese Patent No. 6626607
[0017] Patent Document 3: Japanese Patent No. 2936916
[0018] Non-patent literature
[0019] Non-patent document 1: Japanese Journal of Applied Physics; Vol.46, No.17, 2007, pp.L389-L391
[0020] Non-patent document 2: SEI Laboratories; No. 177, p88~p91
[0021] Non-patent document 3: Fujikura Technical Report; No. 119, 2010 Vol. 2, p33-p38
[0022] Non-Patent Document 4: LEDs Magazine Japan; December 2016, pp. 30 - 31
[0023] Non-Patent Document 5: Iron and Steel; Vol. 80 (1994) No. 3, pp. N91 - N99 Summary of the Invention
[0024] Problems to be Solved by the Invention
[0025] The present invention has been made in view of the above circumstances, and its object is to obtain AlN, Al x Ga 1-x N (0 < X < 1), GaN, etc. with few crystal defects, high characteristics, high thermal conductivity, high strength, low warpage even for large-diameter substrates, and low cost. A seed substrate for high-characteristic epitaxial growth of group III nitrides and a method for manufacturing the same, and a semiconductor substrate and a method for manufacturing the same.
[0026] Solutions for Solving the Problems
[0027] In order to achieve the above object, the seed substrate for epitaxial growth according to an embodiment of the present invention includes a support substrate, a planarization layer of 0.5 - 3 μm provided on the upper surface of the support substrate, and a seed layer provided on the upper surface of the planarization layer. The support substrate includes: a core of a composite ceramic formed of a polycrystalline ceramic of a group III nitride and fibrous single crystals of at least one nitride or oxide of group III or IV, and a sealing layer of 0.05 - 1.5 μm that seals the core. The seed layer is a layer of Si<111> single crystal of 0.04 - 1.5 μm.
[0028] With this configuration, planarization that enables bonding can be achieved. That is, the fibrous (or whisker-like) single crystals added to the core are covered by two layers, the sealing layer and the planarization layer, which have good fusion properties. Therefore, layer separation does not occur, and separation, cracks, and height differences do not occur even after subsequent polishing, and surface smoothness with a Ra of 0.2 nm or less required for bonding can be achieved. As a result, in an example where single crystal fibers of AlN are introduced into AlN ceramics, for example, the thermal conductivity is significantly increased to ~200 W / mK, and the fracture toughness is significantly increased to ~10 Mpa·m 1 / 2 , and it is possible to manufacture epitaxial growth substrates and devices that are most suitable for recent high-output applications and in-vehicle applications that are significantly affected by shocks. Also, in the bonding of the seed substrate in the process of manufacturing an epitaxial growth substrate, the warpage of the support substrate significantly affects the process yield. Since this warpage is greatly improved, the yield is significantly increased. As a result, the cost of the epitaxial growth substrate can also be reduced.
[0029] In the present invention, in the composite ceramic forming the core, the polycrystalline ceramic of group III nitride may be AlN ceramic, and the fibrous single crystal may be AlN, Si3N4 or Al2O3.
[0030] In the present invention, the sealing layer may include at least a Si3N4 layer.
[0031] In the present invention, the planarization layer may be SiO2, silicon oxynitride (Si x O y N z ) and AlAs, or a multilayer film obtained by any combination of them.
[0032] In the present invention, the Si forming the seed layer <111> The OSF of the single crystal is preferably 10 / cm 2 Next. By <111> The OSF in the seed crystal was set to 10 / cm 2 The number of OSFs (number / cm 2 ) can be measured by the evaluation method of Patent Document 3.
[0033] In the present invention, the Si forming the seed layer <111> The resistivity (room temperature) can be 1 kΩ·cm or more.
[0034] In the present invention, a stress adjustment layer may be further provided on the lowermost surface of the support substrate as necessary.
[0035] In the present invention, after the stress adjustment layer is provided with a flattening layer, it has a thermal expansion coefficient that can be corrected when its warping needs to be further corrected. The stress adjustment layer can be SiO2, Si3N4, amorphous Si, polycrystalline Si, etc. alone or in combination thereof. When considering the response to the electrostatic chuck, the stress adjustment layer is preferably a polycrystalline Si made at least by a method selected from sputtering, plasma CVD and LPCVD on the bottom layer of the supporting substrate. At this time, in order to improve the affinity with the sealing layer, SiO2 and / or silicon oxynitride (Si x O y N z) is interspersed between the sealing layer and the polycrystalline Si layer. In the case of using polycrystalline Si to form a film, it can be polycrystalline Si itself or the aforementioned amorphous Si can be polycrystallized by heating or laser, or it can be polycrystalline Si with improved oxidation resistance by partially nitriding the surface layer. If the polycrystalline Si film is set at the bottom layer, the adsorption force based on the electrostatic chuck can be improved, so it is preferred. This is because: the lower the resistivity of the film and the shorter the distance from the film to the electrostatic chuck electrode, the stronger the electrostatic chuck force.
[0036] In the present invention, the sealing layer can be formed by the LPCVD method.
[0037] In the present invention, the planarization layer can be obtained by forming an AlAs film on one side or the entire surface of the upper surface of the support substrate by any one of a plasma CVD method, a LPCVD method, and a low-pressure MOCVD method.
[0038] In the present invention, the seed layer can be formed by providing an OSF of 10 cells / cm 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After hydrogen and / or helium ions are implanted into the single crystal, the Si <111> The single crystal is attached to the upper surface of the planarized layer, and the Si <111> The surface layer of the single crystal is peeled off and thin film transfer is performed to set it.
[0039] The semiconductor substrate according to the embodiment of the present invention is characterized in that a III-V semiconductor thin film is formed on the upper surface of any of the above-mentioned epitaxial growth seed substrates. The III-V semiconductor thin film may be a nitride semiconductor thin film containing Ga and / or Al.
[0040] The manufacturing method of the seed substrate for epitaxial growth described in the embodiment of the present invention comprises the following steps: a step of preparing a core of a composite ceramic, wherein the core of the composite ceramic is formed of a polycrystalline ceramic of a group III nitride and a fibrous single crystal of at least one type of nitride or oxide of group III or group IV; a step of forming a sealing layer with a thickness of 0.05 μm or more and 1.5 μm or less in a manner of wrapping the core to form a supporting substrate; a step of forming a planarizing layer with a thickness of 0.5 μm or more and 3.0 μm or less on the upper surface of the supporting substrate; and a step of transferring Si thin film on the upper surface of the planarizing layer. <111> The step of providing a seed layer with a thickness of 0.04 to 1.5 μm using a single crystal.
[0041] In the present invention, the sealing layer can be formed by the LPCVD method.
[0042] In the present invention, the planarization layer can be formed by forming SiO2 and / or silicon oxynitride (Si2O3) on one side or the entire surface of the upper surface of the support substrate by any one of plasma CVD, LPCVD, and low-pressure MOCVD. xO y N z ) or AlAs.
[0043] In the step of providing the seed layer, the OSF can be 10 / cm 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After hydrogen and / or helium ions are implanted into the single crystal, the Si <111> The single crystal is attached to the upper surface of the planarized layer, and the Si film is transferred by physical means below 450°C. <111> The surface layer of the single crystal is thus provided with a seed layer.
[0044] In the step of providing the seed layer, the stacking faults can be induced to be 10 / cm by oxidation. 2 The following Si <111> After ion implantation of hydrogen and / or helium into the single crystal, the Si film is transferred by physical means below 450°C. <111> The surface layer of the single crystal is 0.20 to 1.7 μm, and the thickness is adjusted to 0.04 to 1.5 μm to provide a seed layer.
[0045] Alternatively, in the step of providing the seed layer, the stacking faults may be induced to be 10 / cm by oxidation. 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After ion implantation of hydrogen and / or helium into the single crystal, the Si film is transferred by physical means below 450°C. <111> The surface layer of the single crystal is 0.20 to 1.7 μm, and the thickness is adjusted to 0.04 to 1.5 μm to provide a seed layer.
[0046] In the present invention, in the step of setting the seed layer, the Si layer transferred by the thin film can be polished by CMP and / or chemical solution. <111> The single crystal is etched to adjust the thickness of the seed layer to 0.04 to 1.5 μm.
[0047] The present invention may further include a step of further providing a stress adjustment layer on the bottom surface of the support substrate. The stress adjustment layer has a thermal expansion coefficient capable of further correcting the warpage after the flattening layer is provided, and the stress adjustment layer may be formed of at least polycrystalline Si produced by a method selected from sputtering, plasma CVD and LPCVD and / or polycrystalline Si whose surface layer is partially nitrided in a nitrogen atmosphere.
[0048] In addition, the semiconductor substrate manufacturing method described in the embodiment of the present invention comprises the following steps: a step of manufacturing a seed substrate for epitaxial growth by any of the above-mentioned methods for manufacturing a seed substrate for epitaxial growth; and a step of forming a III-V semiconductor thin film on the upper surface of the seed substrate for epitaxial growth.
[0049] Effects of the Invention
[0050] According to the present invention, it is possible to provide a seed substrate for epitaxial growth which is excellent in terms of crystal defects, high thermal conductivity, high strength, low warpage, and low cost, and a semiconductor substrate using the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a diagram showing a cross-sectional structure of the seed substrate 1 .
[0052] Figure 2 It is a diagram showing the steps of manufacturing the seed substrate 1. DETAILED DESCRIPTION
[0053] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these.
[0054] The cross-sectional structure of a seed substrate 1 for epitaxial growth of a group III nitride according to the present embodiment (hereinafter sometimes simply referred to as a "seed substrate") is shown in FIG. Figure 1 . Figure 1 The seed substrate 1 shown in the figure has a planarization layer 4 and a Si layer stacked on a support substrate 3. <111> The structure of the seed layer 2. In addition, as necessary, a stress adjustment layer 5 is provided on the surface (lower surface) of the support substrate 3 opposite to the surface on which the planarization layer 4 is stacked.
[0055] The support substrate 3 includes a core 31 serving as a core material of the support substrate 3 and a sealing layer 32 covering the core 31 .
[0056] The core 31 is a composite ceramic formed of polycrystalline ceramic powder of group III nitride, sintering aid, etc., and at least one fibrous single crystal of group III or group IV nitride or oxide. The composite ceramic is preferably sintered by sintering a polycrystalline ceramic powder raw material (e.g., AlN, Si3N4, GaN, or a mixture thereof), a fibrous single crystal of group III or group IV nitride or oxide (e.g., AlN, Si3N4, or Al2O3, or a mixture thereof), and a sintering aid (e.g., Y2O3, Al2O3, CaO, etc.).
[0057] For a support substrate for epitaxial growth film formation of group III nitride crystals, which is the object of the present invention, AlN composite ceramics with a lattice constant, thermal expansion coefficient similar to those of the epitaxial growth film, the best thermal conductivity, and capable of using relatively inexpensive raw materials are most suitable. Composite ceramics can generally be sintered by directly using a hot press at 1750 - 2000 °C in an N2 atmosphere after mixing polycrystalline AlN powder, fibrous AlN single crystals, Y2O3, etc. Alternatively, the polycrystalline AlN powder, fibrous AlN single crystals, Y2O3, etc. of the above raw materials can be made into a slurry using polymers such as polyvinyl alcohol and carboxymethyl cellulose, plasticizers such as polyethylene glycol, and solvents such as water, formed into a sheet using a doctor blade, etc., degreased using a degreasing furnace, and then sintered in a firing furnace. When characteristics are emphasized, a hot press is usually selected, and when cost is emphasized, a sheet forming / atmospheric pressure sintering method is usually selected.
[0058] If described in further detail, in existing AlN ceramics formed from polycrystalline AlN powder and sintering aids, in order to further improve thermal conductivity, mechanical strength, and warpage, it is only necessary to add fibrous single crystals of nitrides or oxides of group III or IV to the polycrystalline AlN powder to form composite ceramics. The added fibrous single crystals can be selected from fibrous single crystals of AlN, Si3N4, or Al2O3 with high thermal conductivity, high aspect ratio, a thermal expansion rate the same as or close to that of the matrix of the AlN powder, affinity with the AlN powder, and electrical insulation.
[0059] The thermal conductivities of fibrous single crystals of AlN, Si3N4, or Al2O3 are approximately 270 - 300 W / mK, 100 - 140 W / mK, and 20 - 45 W / mK respectively, with relatively high thermal conductivities, but there are obvious differences in their values. In addition, since these fibrous single crystals have a large aspect ratio, adding them can improve mechanical strength while suppressing the thermal expansion rate and warpage of the substrate. The order of their mechanical strength is usually Si3N4 < Al2O3 < AlN, and the price is Al2O3 < Si3N4 < AlN. Therefore, for their introduction, it is only necessary to select considering characteristics and economy suitable for the use, and also considering the single use or combined use of the above three. Examples of single introduction are shown below.
[0060] When extremely high thermal conductivity is required and mechanical strength is not very necessary, fibrous single crystals of AlN can be selected. On the contrary, in the case of in-vehicle applications, etc., where the thermal conductivity is about the same but impact resistance is required, fibrous single crystals of Si3N4 can be selected. In addition, when cost is emphasized and both thermal conductivity and mechanical strength are appropriately high, it is only necessary to select fibrous single crystals of Al2O3.
[0061] It should be noted that the mixing ratio of the fibrous single crystal in the composite ceramic is selected in consideration of cost-effectiveness and can be set in the range of 5 to 50wt%. This is because: if the mixing ratio is less than 5%, the effect of improving the characteristics is small, and if it exceeds 50%, the effect tends to be saturated and the cost-effectiveness is low. The substrate for epitaxial growth of the present invention needs to be placed on a semiconductor production line during subsequent equipment processing. Therefore, it is preferred that: after sintering, after processing into a wafer shape, the sintered body is ground and polished until the substrate thickness is 200 to 1000μm, and then CMP polishing is performed to improve smoothness and mirror finishing is performed.
[0062] The present invention forms a supporting substrate by sealing the core of the composite ceramic with a 0.05-1.5 μm sealing layer of the present invention, especially with a layer containing at least a Si3N4 layer, and further covers it with a 0.5-3 μm flattening layer provided on the upper surface of the aforementioned supporting substrate, so that the fibrous or whisker-shaped single crystal is fused with the AlN powder of the matrix, and after being completely integrated by the stacking effect of the two layers, it is polished to obtain a flatness of Ra=0.2nm or less that can be pasted. That is, by optimizing the composition and thickness of the two layers, which are the essential components of the present invention, not only the synergistic effect of the two layers is exerted, but also the flatness that can be pasted can be obtained. It should be noted that the flattening layer can be a single-layer film of any one of SiO2, silicon oxynitride and AlAs, or a multilayer film obtained by any combination of them (for example, a film formed by stacking SiO2 and silicon oxynitride, or a film formed by stacking SiO2 and AlAs).
[0063] If the above-mentioned adjusted composite ceramic is used directly as the core 31 alone, a large number of crystal defects and coloration will be generated in the target epitaxially grown single crystal due to carbon, oxygen, and other impurities from raw materials such as AlN powder, fibrous single crystals, sintering binders, metal impurities such as Y2O3 powder, and insulating materials, furnace materials, containers, etc. during sintering, causing adverse effects.
[0064] Therefore, a sealing layer 32 is provided to wrap and seal the core 31 of the composite ceramic. Specifically, when the core 31 is sealed by the sealing layer 32, the composition and film thickness of each layer constituting the sealing layer 32 need to be considered so that the thermal stress is as small as possible and the thermal conductivity is as large as possible. In the present invention, from the perspective of characteristics and manufacturing cost, the total film thickness of the sealing layer 32 is preferably optimized within the range of 0.05 to 1.5 μm.
[0065] The composition of the sealing layer 32 can be appropriately selected in consideration of the thermal expansion coefficient and thermal conductivity. In order to further improve its resistance to impurity diffusion, it is preferably sealed by covering the entire layer with a film formed of at least silicon nitride (Si3N4).
[0066] In the sealing layer 32, p-Si can be provided as a layer for the electrostatic chuck, as required, for example, when an electrostatic chuck is to be used. The p-Si layer can be formed between the composite ceramic core and the Si3N4 layer, or can be provided together with the stress adjustment layer 5 described later or provided under it. In this case, when the adhesion between p-Si and Si3N4 is insufficient, SiO2, silicon oxynitride (Si3N4) with high adhesion can be sandwiched in consideration of the affinity and thermal expansion coefficient between the layers. x O y N z ) etc. Furthermore, for the purpose of anti-oxidation of p-Si, partially nitrided polycrystalline Si can be made.
[0067] In order to avoid high-frequency loss in a device made of an epitaxial layer grown using the seed substrate, the Si <111> The resistivity (room temperature) of the seed layer 2 is preferably 1 kΩ·cm or more. This is because: in the case of Si having a resistivity (room temperature) of 1 kΩ·cm or less, <111> In the seed layer 2, high-frequency loss due to millimeter waves used in the gigahertz band becomes large, the device generates heat, and the power consumption is also large, and the required characteristics cannot be obtained.
[0068] In the case of setting a p-Si film for an electrostatic chuck, with respect to its resistance, it is preferred that p-Si with a higher resistance be within the range in which the necessary adsorption force can be obtained, and with respect to its position, it can be formed in the lower layer of the core 31 as far as possible from the seed layer 2 to be stacked by epitaxial growth or in the lower part of the stress adjustment layer 5. Alternatively, multilayer film formation can be performed simultaneously with the stress adjustment layer 5. The high-frequency loss of p-Si with high resistance is small. In addition, if it is arranged at the lower part of the supporting substrate 3, it is close to the electrostatic chuck, so even with high resistance, sufficient electrostatic force will be generated. Therefore, even without doping, the substrate can be fully adsorbed. In order to further reduce the high-frequency loss, it is more preferred to remove the p-Si layer by grinding the back of the substrate at the end of the equipment production. In the case of setting the stress adjustment layer 5, it is preferred to maintain the resistance of p-Si as high as possible, and there is no limitation on the minimum doping of boron (B), phosphorus (P), etc. required to generate the necessary electrostatic force.
[0069] In the sealing layer 32, if each layer is too thick, the stress between the layers caused by the difference in thermal expansion coefficient becomes large, and peeling occurs between the layers. Therefore, when selecting films of various compositions and combining them, the thickness of the sealing layer 32 is not preferably more than 1.5μm. On the other hand, from the perspective of the function of sealing impurities, when the thickness is less than 0.05μm, it is insufficient to prevent the diffusion of impurities. In summary, the thickness of the sealing layer 32 is preferably set in the range of 0.05 to 1.5μm. It should be noted that the film forming method of the sealing layer can be selected from film forming methods such as MOCVD, normal pressure CVD, LPCVD, and sputtering. From the perspective of film quality, film coverage, and resistance to impurity diffusion, the LPCVD method is particularly preferred.
[0070] A planarization layer 4 with a thickness of 0.5 to 3 μm is stacked on the sealing layer 32 on at least the upper surface of the support substrate 3. The planarization layer 4 is selected from SiO2, Al2O3, Si3N4, SiC or silicon oxynitride (Si x O y N z ) and other ceramic film materials, Si, GaAs, AlAs, etc., which are often used as sacrificial layers in etching, etc., are preferably selected from SiO2 and / or silicon nitride oxide (SiO2) which are easy to grind or polish during flattening and easy to separate when obtaining a clean substrate, etc. x O y N z ) or AlAs.
[0071] It should be noted that, from the perspective of cost, the planarization layer 4 is usually stacked only on one side of the sealing layer 32, but when the warping is large, the film can also be formed in a manner that covers the entire sealing layer 32. The thickness of the planarization layer 4 needs to be a thickness that can fully fill the pores, concave-convexities, or height differences caused by the aforementioned fibrous single crystals of the core 31 of the composite ceramic using the sealing layer 32, and can obtain sufficient smoothness for the seed crystal to be transferred. However, even for a core of a composite ceramic with a fibrous single crystal, an overly thick planarization layer 4 cannot fully suppress the thermal stress of the thick planarization layer, which becomes a cause of warping, cracking, etc. of the seed substrate 1, so it is not preferred. Therefore, it is appropriate to set it with a thickness of at least 0.5 to 3 μm on the upper surface. If the thickness is less than 0.5 μm, it is difficult to use the sealing layer 32 and the planarization layer 4 to fill the pores, concave-convexities, or height differences caused by the fibrous single crystals of the core 31 of the composite ceramic. On the other hand, when the thickness is 3 μm or more, warping and cracking are likely to occur in the planarizing layer 4 .
[0072] From the viewpoints of necessary film quality and film-forming efficiency, the film-forming method of the planarization layer 4 is preferably a plasma CVD method, an LPCVD method, a low-pressure MOCVD method, or the like. The stacked planarization layer 4 is subjected to heat treatment for sintering and CMP polishing for smoothing according to the film condition, so as to prepare for the thin film transfer of the seed layer 2 described later.
[0073] The seed layer 2 is formed by thin film transferring seeds onto the surface of the planarization layer 4. The seeds used in the thin film transfer are selected from substrates having a crystal structure similar to that of III-nitride such as AlN, Al x Ga 1-x N(0 < X < 1), GaN, etc. Therefore, AlN, Si<111>, SiC, SCAM, AlN, AlGaN, sapphire, etc. can be considered. From the viewpoints of ease of large diameterization, availability of mass-produced commercial products, low cost, etc., Si<111> is suitable. Among Si<111> crystals, particularly suitable is a Si<111> single crystal with an oxidation-induced stacking fault (OSF) of 10 / cm 2 or less.
[0074] If the OSF of the Si<111> single crystal, which serves as the seed for epitaxial growth film formation in the subsequent process, is 10 / cm 2 or less, the crystal formed by epitaxial growth film formation also has few defects following the seed. Furthermore, the equipment using it also exhibits high characteristics and a good yield, so the cost becomes low. In contrast, if the OSF exceeds 10 / cm 2 , the defects of the crystal formed by epitaxial growth film formation increase sharply, the equipment characteristics deteriorate, and inevitably, the yield deteriorates and the cost becomes high.
[0075] When the resistivity (room temperature) of the Si<111> single crystal is less than 1 kΩ·cm, high-frequency loss occurs due to its resistance, the power consumption increases, or heat is generated, deteriorating the characteristics of the equipment. Therefore, when using the epitaxial growth and scale-free substrate obtained by epitaxial growth film formation on the seed substrate 1 for high-frequency equipment, especially for high frequencies of 5G and later, as the Si<111> single crystal, it is preferable to select an object with a resistivity (room temperature) of 1 kΩ·cm or more.
[0076] Si <111> After the single crystal is implanted with ions of hydrogen and / or helium (He) whose ion species have little influence on the resistance of the single crystal substrate, the Si <111> The ion implanted surface of the single crystal is bonded to the upper surface of the planarized layer 4 and peeled off by physical means such as claws at a temperature below 450°C. <111> The surface layer of the single crystal is separated at the depth of ion implantation, and the thin film is transferred to the planarization layer 4. That is, a seed layer 2 is set on the upper surface of the planarization layer 4. Light elements such as hydrogen and helium are different from heavy elements such as boron (B). Ion implantation of light elements such as hydrogen and helium causes little damage to the seed crystal and does not reduce the resistance. From this point of view, it is suitable for ion implantation into the seed crystal. In addition, by performing the peeling / transfer at a low temperature below 450°C, it is possible to prevent the Si that cannot be avoided in the smart peeling method that performs thermal peeling / transfer at a high temperature above 700°C. <111> Thermal damage of single crystal.
[0077] The final thickness of the seed layer 2 can be set to 0.04 to 1.5 μm. In ion implantation, even if only the damaged layer is caused by ions, there is a thickness of approximately 0.1 μm. If it is set to less than 0.04 μm, a good seed cannot be obtained. In addition, when the transfer thickness is 1.5 μm or more, the ion implanter requires high-output ion energy, and the ion implanter becomes huge in size, requiring huge investment, which is not economical. In order to set the seed layer 2 of appropriate thickness, the thin film transfer Si can be used. <111> The surface layer of the single crystal is 0.20 to 1.7 μm, and then the thickness is adjusted to 0.04 to 1.5 μm. <111> The thickness of the single crystal thin film is determined by the amount of cutting when removing the damaged layer during ion implantation, and the upper limit is determined by the constraints of the ion implantation device (large-scale and high-cost devices based on high acceleration voltage). The range can be set to 0.1 to 2.0 μm, and more preferably 0.20 to 1.7 μm. The thickness can be adjusted by CMP polishing and / or etching in a chemical solution.
[0078] If a more specific implementation method is described, after hydrogen and / or helium are ion-implanted into the seed crystal at a depth of 0.2 to 1.7 μm, the upper surface of the planarization layer 4 is bonded to the ion-implanted surface of the seed crystal. Thereafter, the seed crystal can be peeled off by physical methods such as gas pressure and claws at a temperature below 450°C. By setting the processing temperature to below 450°C, it is possible to suppress impurity diffusion, stress caused by thermal stress, and thermal damage that are easily generated in the seed crystal of the thin film transferred by processing at a high temperature exceeding 450°C.
[0079] Afterwards, the upper surface of the transferred film can be polished by CMP and / or lightly etched by a chemical solution to remove the damaged layer of ion implantation, thereby obtaining a single crystal seed film (seed layer) with a thickness of 0.04 to 1.5 μm. It should be noted that when seeking higher uniformity in ion implantation, SiO2 or the like can be formed into a film on the ion implantation surface of the seed substrate as needed before ion implantation.
[0080] In the present invention, a stress adjustment layer 5 may be added to the bottommost surface of the aforementioned support substrate 3 depending on the situation. The stress adjustment layer 5 corrects the warping of the seed substrate 1 that occurs by forming the planarization layer 4. The stress adjustment layer 5 selects a film material and a thickness that have a thermal expansion coefficient that can correct the warping of the seed substrate 1. As the stress adjustment layer 5, it is suitable to form a film of at least polycrystalline Si (p-Si) in order to cope with the electrostatic chuck. It should be noted that from the viewpoint of correcting the warping and the affinity with the sealing layer 32, SiO2 and / or silicon nitride oxide (Si 2O) may be interspersed between the polycrystalline Si forming the stress adjustment layer 5 and the sealing layer 32. x O y N z ) etc. as a part of the stress relaxation layer. In addition, a part of the polycrystalline Si can be nitrided to impart oxidation resistance.
[0081] Next, refer to Figure 2 , the steps of the method for manufacturing the seed substrate 1 for epitaxial growth of group III nitrides according to the present embodiment are described. It should be noted that if the method suitable for forming each layer has been described together with the structure of each part of the seed substrate 1, the repeated description here will be omitted.
[0082] First, a composite ceramic core 31 ( ) is prepared which is composed of a polycrystalline ceramic of a group III nitride and a fibrous single crystal of at least one type of group III or group IV nitride or oxide. Figure 2 Then, a sealing layer 32 is formed into a film with a thickness of 0.05 μm to 1.5 μm in a manner of wrapping the core 31 to form a supporting substrate 3 ( Figure 2 At this time, the sealing layer 32 can be formed by LPCVD. Next, a planarization layer 4 ( Figure 2 In addition, as required, a stress adjustment layer 5 ( Figure 2After the flattening layer 4 is provided, the stress adjustment layer 5 may be formed of a single film of SiO2, Si3N4, amorphous Si, polycrystalline Si, or a film formed by a combination thereof in order to correct the warping. However, in consideration of the handling of the electrostatic chuck, it is preferred that: polycrystalline Si formed by at least one of the sputtering method, plasma CVD, and LPCVD method is directly formed on the bottom layer of the support substrate 3, or, when the lower part of the support substrate 3 is difficult to bond with the polycrystalline Si, SiO2 and / or silicon oxynitride (Si 2N4) is formed on the lower part of the support substrate 3. x O y N z ) and a polycrystalline Si layer is formed at its lower part. The polycrystalline Si may be polycrystalline Si itself or the aforementioned amorphous Si may be polycrystalline Si by heating or laser. It may be polycrystalline Si whose surface layer is partially nitrided to improve oxidation resistance. Furthermore, in order to improve oxidation resistance, a part may be nitrided, or a Si3N4 film may be further formed after the polycrystalline Si is formed. It should be noted that the planarization layer 4 and the stress adjustment layer 5 may be formed at the same time.
[0083] In addition, a seed crystal, that is, Si, for peeling off the transfer seed crystal layer 2 is prepared separately from S01 to S04. <111> Single crystal substrate 20 ( Figure 2 Next, ion implantation is performed from one surface (ion implantation surface) of the single crystal substrate 20 to form a peeling position (embrittled layer) 21 ( Figure 2 of S12).
[0084] Next, the ion implanted surface of the single crystal substrate 20 is bonded to the planarized layer 4 formed on the support substrate 3 to form a bonded substrate ( Figure 2 S21). If necessary, heating may be performed at 450°C or below to improve the bonding strength. Then, the single crystal substrate 20 is separated at the peeling position 21 of the single crystal substrate 20 in the bonding substrate ( Figure 2 By doing so, a thin film transfer Si is formed on the planarization layer 4 on the support substrate 3. <111> The single crystal film is used as the seed layer 2. The thickness of the transferred seed layer 2 is adjusted by CMP polishing and / or etching in a chemical solution as needed. <111> The remaining portion of the single crystal substrate 20 is polished again to form an ion implantation surface, and can be repeatedly used for thin film transfer to form a seed layer for further manufacturing another group III nitride composite substrate.
[0085] As described above with respect to the structure and manufacturing method of the seed substrate 1 for epitaxial growth, the seed substrate 1 for epitaxial growth described in the present invention is a seed substrate for epitaxial growth having a supporting substrate, a planarization layer of 0.5 to 3 μm arranged on the upper surface of the aforementioned supporting substrate, and a seed layer arranged on the upper surface of the aforementioned planarization layer. The supporting substrate comprises a composite ceramic core and a sealing layer of 0.05 to 1.5 μm that seals the core, wherein the composite ceramic core is formed of a polycrystalline ceramic of a group III nitride and at least one fibrous single crystal of a group III or group IV nitride or oxide. The stacking faults induced by thin film transfer oxidation are 10 / cm 2 The following Si <111> The surface layer of the single crystal is provided with a seed layer of 0.04 to 1.5 μm. According to the present invention, in particular, through the following features 1) to 3), it is possible to achieve high thermal conductivity, high strength, high dimensional accuracy, and low warping based on the additive effect of the fibrous single crystal, and further, as an additional effect, a high-performance, low-cost epitaxial growth film crystalline substrate can be obtained. 1) A core of a composite ceramic formed by a polycrystalline ceramic of a group III nitride and at least one fibrous single crystal of a group III or group IV nitride or oxide is used; 2) The supporting substrate is, of course, used to minimize thermal stress between the planarization layer, the seed layer, and other layers by optimizing their composition and film thickness; 3) The oxidation-induced stacking faults of the seed layer thin film transfer are 10 / cm 2 The following Si <111> The surface of a single crystal.
[0086] These results of the present invention are not only due to a single reason, but also the result of the good performance of the "synergistic effect" of various reasons complementing each other. It should be noted that as other secondary reasons, 4) further achieving low stress by using a stress adjustment layer as needed, and 5) ion implantation of light elements limited to hydrogen and / or helium and performing thin film transfer by peeling at below 450°C using physical means such as claws, etc. also contribute to achieving the effects of the present invention.
[0087] As the use of the substrate of the present invention expands in devices such as light-emitting diodes used in the deep ultraviolet region (UVC; 200-280nm), 5G communications, EV vehicles, etc., it can greatly improve the characteristics of increasingly high-output, high-frequency, and high-voltage devices, and also significantly improve the manufacturing yield of the equipment, which can achieve low cost.
[0088] Example
[0089] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0090] [Example 1]
[0091] (Preparation of Support Substrate)
[0092] The following items were prepared as a support substrate 3 having a structure in which a composite ceramic core 31 composed of a polycrystalline ceramic of a group III nitride and a fibrous single crystal of a group III nitride was covered with a sealing layer 32. Specifically, for the composite ceramic core 31, 80 parts by weight of commercially available AlN powder, 20 parts by weight of commercially available AlN fibrous single crystals, and 5 parts by weight of commercially available Y2O3 as a sintering aid were mixed with an organic binder, a solvent, etc., and a green sheet was prepared and degreased, and then sintered at 1900°C in a N2 atmosphere. The sintered body was hollowed out to form a Inch wafers are then polished on both sides to produce The core of the composite ceramic of the AlN composite ceramic substrate is a 725μm substrate with a thickness of 0.1 μm × t. After the core substrate of the AlN composite ceramic was polished, when the Ra of the surface was measured, a fibrous single crystal height difference portion was observed in a part. The result of measuring the Ra representing the flatness was that the average Ra at 10 locations was 520nm (0.52μm). The core 31 of the AlN composite ceramic was covered as a whole by wrapping it with a 0.1μm thick silicon oxynitride layer based on the LPCVD method, and another LPCVD device was further used thereon to seal the whole with a 0.4μm thick Si3N4 layer, thereby forming a sealing layer 32. The total thickness of the sealing layer 32 is set to 0.5μm. On the Si3N4 layer, for the purpose of further flattening, a 6μm thick SiO2 is stacked only on one side of the upper layer using a plasma CVD method (ICP-CVD device). After sintering at 1000°C, SiO2 was polished to 2 μm thickness by CMP polishing, and the Ra indicating flatness was measured. The average Ra of 10 locations was 0.18 nm. This confirmed that the flatness was sufficient for bonding, and prepared for the thin film transfer of the seed crystal in the subsequent process.
[0093] (Seed Crystal Preparation)
[0094] In the evaluation of Patent Document 3, the oxidation induced stacking fault (OSF) was set to 9 / cm 2 And the resistivity (room temperature) is 1.2kΩ·cm inches, 725μm thick Si <111> The single crystal substrate was used as the seed substrate. At 100 keV, a depth of 0.6 μm, and a doping amount of 8×10 17 cm -2 Under the conditions of , hydrogen ions are implanted into the Si substrate.
[0095] The ion implantation of Si was attempted on the planarized layer 4 (thickness 2 μm) of the support substrate 3 prepared in advance. <111> Thin film transfer of the surface 0.6μm portion of the single crystal. Although the core is a composite ceramic containing AlN fibrous single crystal, the Si of the seed crystal can be smoothly transferred. <111> . For Si during ion implantation and transfer <111> The damaged part of the single crystal is gently polished using CMP to remove the Si <111> The single crystal layer was formed into a 0.3 μm thick seed layer 2. The obtained seed substrate 1 had a balanced film thickness and thermal stress between the sealing layer 32, the sealing layer 32, the planarizing layer 4, and the seed layer 2, resulting in no cracks, film peeling, or warping.
[0096] It should be noted that the remaining Si after the film transfer <111> A single crystal substrate can be repeatedly used as a plurality of seed crystals by repeatedly performing ion implantation multiple times, which is extremely economical.
[0097] The characteristics of the seed substrate 1 as a seed substrate for epitaxial growth of GaN were simply evaluated using the following composition and method.
[0098] The seed substrate 1 is epitaxially grown using an MOCVD device. At this time, the epitaxial layer forms AlN and AlGaN films in sequence from the seed substrate 1 side toward the growth direction, and then GaN is epitaxially grown. In this epitaxial growth film formation, after the AlN layer is formed to 110nm and the AlGaN layer is formed to 140nm, the thickness of the GaN epitaxial layer is set to 5um. During epitaxial growth, TMAl (trimethylaluminum) is used as the Al source, TMGa (trimethylgallium) is used as the Ga source, and NH3 is used as the N source. In addition, it is implemented in the range of 900 (front stage) to 1200℃ (GaN film formation) with carrier gases of N2 and H2.
[0099] The thermal conductivity, fracture toughness as a mechanical strength, and WARP as a warpage evaluation of the epitaxial growth substrate were measured and found to be 230 W / mK and 9 MPa·m 1 / 2 , 22μm. In addition, in order to evaluate the dislocation density, etch pits were generated by molten alkali (KOH) etching method, and the etch pit density (Etch Pit Density, hereinafter referred to as EPD) was measured. In addition, as an evaluation of crystallinity, X-ray rocking curve (XRC) measurement was performed.
[0100] As a result, the EPD was 0.1×10 4 cm -2, showing an extremely low dislocation density. In addition, the half-value width FWHM in the XRC measurement of the (0002) plane of the substrate (hereinafter referred to as "0002XRC FWHM") is 128arcsec, and high-quality GaN single crystals can be obtained. According to these results, the seed substrate 1 described in this embodiment has excellent properties as a seed substrate for epitaxial growth. When an epitaxial growth substrate having an epitaxial layer provided on the seed substrate 1 is used for high-frequency equipment of 30GHz / 20Gbps, the surface temperature of the equipment is 45°C, and no temperature rise due to high-frequency loss, which is particularly problematic, is observed.
[0101] [Comparative Example 1]
[0102] The support substrate of Example 1 was composed of 100 parts by weight of commercially available AlN powder and 5 parts by weight of commercially available Y2O3 as a sintering aid. <111> For single crystal substrate, the OSF is set to 15 / cm 2 , the resistivity (room temperature) is 0.7 kΩ·cm, and the Si <111> The single crystal substrate was subjected to thin film transfer with a seed layer 2 having a thickness of 1.7 μm. Other than this, the same conditions as those of Example 1 were used including the evaluation method.
[0103] The thermal conductivity, fracture toughness as a mechanical strength, and WARP as a warpage evaluation of the epitaxial growth substrate were measured in the same manner as in Example 1. The results were 150 W / mK, 3 MPa·m 1 / 2 , 55μm. In addition, in order to evaluate the dislocation density, the molten alkali (KOH) etching method was used to generate etching pits and the EPD measurement was performed. In addition, as an evaluation of the crystallinity, the XRC measurement was performed. The result was that the EPD was 10×10 4 cm -2 , showing a very large dislocation density. In addition, the FWHM of 0002XRC is 920 arcsec, and a GaN single crystal with poor crystallinity is formed compared with Example 1. In addition, when the epitaxial growth substrate is used for 30GHz / 20Gbps high-frequency equipment, the surface temperature of the equipment reaches 132°C due to high-frequency loss, and water cooling is required for long-term use.
[0104] [Example 2]
[0105] Regarding the supporting substrate of Example 1, 80 parts by weight of commercially available AlN powder and 30 parts by weight of commercially available Si3N4 fibrous single crystals, as well as 5 parts by weight of commercially available Y2O3 and 2 parts of Al2O3 as sintering aids, are used. Other than that, the conditions including the evaluation method are the same as those of Example 1.
[0106] The thermal conductivity, fracture toughness as a mechanical strength, and WARP as a warpage evaluation of the epitaxial growth substrate were measured in the same manner as in Example 1. The results were 175 W / mk and 15 MPa·m 1 / 2 , 7μm, and WARP is extremely small. In addition, in order to evaluate the dislocation density, etch pits were generated by molten alkali (KOH) etching method, and EPD measurement was performed. In addition, XRC measurement was performed as an evaluation of crystallinity. The result was that EPD was 0.6×10 4 cm -2 , showing a small dislocation density. In addition, the FWHM of 0002XRC is 320 arcsec, and the crystallinity is slightly worse than that of Example 1. In addition, when the epitaxial growth substrate is used for 30GHz / 20Gbps high-frequency equipment, the surface temperature of the equipment is 78°C due to high-frequency loss, and it can be used for a long time only by air cooling.
[0107] Description of Reference Numerals
[0108] 1 Seed substrate
[0109] 2 Seed layer
[0110] 3 Support base plate
[0111] 4 Planarization layer
[0112] 5 Stress Adjustment Layer
[0113] 20 Seeded single crystal substrate
[0114] 21 peeling position
Claims
1. A seed substrate for epitaxial growth, It is characterized in that It has: support base plate; A planarization layer with a thickness of 0.5 to 3 μm, which is disposed on the upper surface of the support substrate; and a seed layer disposed on the upper surface of the planarization layer, The support substrate comprises: A composite ceramic core, which is formed of a polycrystalline ceramic of a group III nitride and a fibrous single crystal of at least one or more nitrides or oxides of group III or group IV; and A sealing layer of 0.05 to 1.5 μm, which seals the core, The seed layer is 0.04 to 1.5 μm Si <111> Layers of a single crystal.
2. The epitaxial growth seed substrate according to claim 1, It is characterized in that The polycrystalline ceramic of the group III nitride forming the core is AlN ceramic, and the fibrous single crystal is AlN, Si 3 N 4 or Al 2 O 3 .
3. The seed substrate for epitaxial growth according to claim 1 or 2, It is characterized in that The sealing layer contains at least Si 3 N 4 layer.
4. The seed substrate for epitaxial growth according to any one of claims 1 to 3, It is characterized in that The planarization layer is SiO 2 、Silicon Oxynitride (Si x O y N z ) and AlAs, or a multilayer film obtained by any combination of them.
5. The seed substrate for epitaxial growth according to any one of claims 1 to 4, It is characterized in that The Si forming the seed layer <111> The oxidation-induced stacking faults of the single crystal are 10 / cm 2 the following.
6. The seed substrate for epitaxial growth according to any one of claims 1 to 5, It is characterized in that The Si forming the seed layer <111> The resistivity (room temperature) of the single crystal is 1 kΩ·cm or more.
7. The seed substrate for epitaxial growth according to any one of claims 1 to 6, It is characterized in that The support substrate further includes a stress adjustment layer on the lowermost surface thereof.
8. The epitaxial growth seed substrate according to claim 7, It is characterized in that The stress adjustment layer has a thermal expansion coefficient capable of further correcting the warpage of the planarization layer after the planarization layer is provided, and is formed of polycrystalline Si produced by at least a method selected from a sputtering method, a plasma CVD method, and a LPCVD method.
9. The seed substrate for epitaxial growth according to claim 7 or 8, It is characterized in that The stress adjustment layer is formed by sandwiching SiO 2 and / or silicon oxynitride (Si x O y N z ) and / or the surface layer is formed by locally nitrided polycrystalline Si.
10. The seed substrate for epitaxial growth according to any one of claims 1 to 9, It is characterized in that The sealing layer is formed by LPCVD method.
11. The seed substrate for epitaxial growth according to any one of claims 1 to 10, It is characterized in that The planarization layer is formed by forming a SiO film on one side or the entire surface of the upper surface of the support substrate by any one of a plasma CVD method, a LPCVD method, and a low-pressure MOCVD method. 2 and / or silicon oxynitride (Si x O y N z ) or AlAs.
12. The seed substrate for epitaxial growth according to any one of claims 1 to 11, It is characterized in that The seed layer is set as follows: the oxidation-induced stacking fault is 10 / cm 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After single crystal ion implantation of hydrogen and / or He, Si is peeled off by physical means below 450°C <111> The surface layer of the single crystal is transferred into a thin film and thus set.
13. A semiconductor substrate, It is characterized in that A III-V semiconductor thin film is formed on the upper surface of the epitaxial growth seed substrate according to any one of claims 1 to 12.
14. The semiconductor substrate according to claim 13, It is characterized in that The III-V semiconductor film is a nitride semiconductor film containing Ga and / or Al.
15. A method for manufacturing a seed substrate for epitaxial growth, comprising the following steps: A step of preparing a core formed of a polycrystalline ceramic of a group III nitride and a fibrous single crystal of at least one type of group III or group IV nitride or oxide; A step of forming a sealing layer having a thickness of 0.05 μm or more and 1.5 μm or less so as to wrap the core to prepare a supporting substrate; forming a planarization layer having a thickness of 0.5 μm or more and 3.0 μm or less on the upper surface of the support substrate; and By thin-film transfer Si on the upper surface of the planarization layer <111> The step of providing a seed layer with a thickness of 0.04 to 1.5 μm using a single crystal.
16. The method for producing a seed substrate for epitaxial growth according to claim 15, It is characterized in that The sealing layer is formed by LPCVD method.
17. The method for producing a seed substrate for epitaxial growth according to claim 15 or 16, It is characterized in that The planarization layer is formed by forming a SiO film on one side or the entire surface of the upper surface of the support substrate by any one of a plasma CVD method, a LPCVD method, and a low-pressure MOCVD method. 2 and / or silicon oxynitride (Si x O y N z ) or AlAs.
18. The method for producing a seed substrate for epitaxial growth according to any one of claims 15 to 17, It is characterized in that In the step of providing the seed layer, the oxidation induced stacking fault is 10 / cm 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After single crystal ion implantation of hydrogen and / or He, the Si <111> The single crystal is attached to the upper surface of the planarized layer, and the Si <111> The surface layer of the single crystal is subjected to thin film transfer, thereby providing the seed layer.
19. The method for producing a seed substrate for epitaxial growth according to any one of claims 15 to 18, It is characterized in that In the step of providing the seed layer, the oxidation induced stacking fault is 10 / cm 2 The following Si <111> After single crystal ion implantation of hydrogen and / or He, Si thin film transfer is performed by physical means below 450°C. <111> The surface layer of the single crystal is 0.20 to 1.7 μm, and the thickness is adjusted to 0.04 to 1.5 μm, thereby providing the seed layer.
20. The method for producing a seed substrate for epitaxial growth according to any one of claims 15 to 18, It is characterized in that In the step of providing the seed layer, the oxidation induced stacking fault is 10 / cm 2 Si with a resistivity (room temperature) of 1 kΩ·cm or more <111> After single crystal ion implantation of hydrogen and / or He, Si thin film transfer is performed by physical means below 450°C <111> The surface layer of the single crystal is 0.20 to 1.7 μm, and the thickness is adjusted to 0.04 to 1.5 μm, thereby providing the seed layer.
21. The method for producing a seed substrate for epitaxial growth according to claim 19 or 20, It is characterized in that In the step of providing the seed layer, the Si layer transferred from the thin film is polished by CMP and / or chemical solution. <111> The single crystal is etched to adjust the thickness of the seed layer to 0.04 to 1.5 μm.
22. The method for producing a seed substrate for epitaxial growth according to any one of claims 15 to 21, It is characterized in that The method further comprises the step of providing a stress adjustment layer on the bottom surface of the support substrate.
23. The method for producing a seed substrate for epitaxial growth according to claim 22, It is characterized in that The stress adjustment layer has a thermal expansion coefficient capable of further correcting the warping after the planarization layer is provided, and is formed of at least polycrystalline Si produced by a method selected from sputtering, plasma CVD, and LPCVD and / or polycrystalline Si whose surface layer is locally nitrided in a nitriding atmosphere.
24. A method for manufacturing a semiconductor substrate, comprising the following steps: a step of manufacturing a seed substrate for epitaxial growth by the method for manufacturing a seed substrate for epitaxial growth according to any one of claims 15 to 23; and The step of forming a III-V semiconductor thin film on the upper surface of the epitaxial growth seed substrate.