Substrate for electronic device and method for manufacturing same

By forming a declining oxide film on a single crystal silicon substrate and combining the substrate, the problems of warping, slipping and rupture during epitaxial growth of nitride semiconductors are solved, and the damage strength of the substrate and the pressure resistance of the device are improved.

CN118891405APending Publication Date: 2024-11-01SHIN ETSU HANDOTAI CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380031929.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-27
Filing Date
2023-02-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, when epitaxial growth of nitride semiconductors is used by bonding substrates, it is difficult to completely suppress the occurrence of warping, slipping, and rupture, especially on a single crystal silicon substrate, resulting in insufficient productiveness and strength of the device.

Method used

By forming an oxide film with declination on a single crystal silicon substrate and performing heat treatment, the first single crystal silicon substrate is combined with the second single crystal silicon substrate to form a bonding substrate with an inclined cleavage surface, and nitrogen is grown on the surface thereof. Chemical semiconductor film to improve the damage strength of the substrate.

Benefits of technology

It effectively suppresses the occurrence of warpage, slippage, and rupture, improves the damage strength of the substrate for electronic devices, and is particularly suitable for the manufacturing of large-diameter substrates, and enhances the pressure resistance and processability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891405A_ABST
    Figure CN118891405A_ABST
Patent Text Reader

Abstract

The present invention is a substrate for an electronic device in which a nitride semiconductor film is formed on a single-crystal-silicon bonded substrate in which a first single-crystal-silicon substrate having a crystal plane orientation {111} and a second single-crystal-silicon substrate having a crystal plane orientation {111} are bonded to each other with an oxide film interposed therebetween. The main surface of the second single crystal silicon substrate has an off-angle with respect to the crystal orientation {100}, and the nitride semiconductor film is formed on the surface of the first single crystal silicon substrate of the bonded substrate. As a result, provided are: a substrate for an electronic device in which a nitride semiconductor is formed on a single crystal silicon, said substrate being suppressed in the occurrence of slippage, cracking, and the like, and having high breaking strength; and a method for producing the substrate for an electronic device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate for electronic devices and a method for manufacturing the same, and in particular to a substrate for electronic devices having a nitride semiconductor formed on a silicon substrate and a method for manufacturing the same. Background Art

[0002] Nitride semiconductors such as GaN and AlN can be used to manufacture high electron mobility transistors (HEMTs) and high withstand voltage electronic devices using two-dimensional electron gases.

[0003] It is difficult to produce nitride semiconductor wafers formed by growing these nitride semiconductors on a substrate. In the past, sapphire substrates and SiC substrates were used as growth substrates. However, in order to increase the diameter (larger aperture) of the substrate and reduce the cost of the substrate, epitaxial growth of nitride semiconductors based on vapor phase growth on a single crystal silicon substrate is also performed. For the production of epitaxial growth films of nitride semiconductors based on vapor phase growth on a single crystal silicon substrate, a large diameter substrate can be used compared to a sapphire substrate and a SiC substrate, which is advantageous in terms of high device productivity and easy processing. However, in the vapor phase growth of nitride semiconductors on a single crystal silicon substrate, due to the stress generated by the difference in lattice constants and thermal expansion coefficients, warping increases, slippage, cracks, etc. are prone to occur, and stress reduction based on growth conditions and a relaxation layer is performed.

[0004] In particular, in order to make the epitaxial substrate for power devices have a high withstand voltage, it is necessary to produce GaN on Si (GaN on single crystal silicon) with a thickened GaN epitaxial layer. To thicken the epitaxial layer, it is sufficient to thicken the growth substrate, that is, the single crystal silicon substrate, and perform epitaxial growth. In addition, as a method for thickening the single crystal silicon substrate, a step of bonding two single crystal silicon substrates is performed. Patent document 1 discloses setting the thickness of the bonded substrate to be greater than 2 mm. In addition, in patent document 2, as a combination of two substrates to be bonded, it is disclosed that: the bonded wafer is in the plane orientation {111}, and the base substrate is in the plane orientation {100}, and the resistivity is less than 0.1Ωcm.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-014376

[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-027186 Summary of the invention

[0009] 1. Technical issues to be resolved

[0010] As described above, there are known technologies for using a laminated substrate as a growth substrate, as disclosed in Patent Documents 1 and 2. However, even with these laminated substrates, it is still impossible to completely suppress the increase in warpage and the occurrence of slippage, cracks, etc. In addition, slippage, cracks, etc. mostly occur in the notch portion of the substrate. Generally speaking, in a {111} single crystal silicon substrate, <110> A notch is formed in the {100} single crystal silicon substrate. <110> Direction or <100> direction is formed.

[0011] The present invention has been made to solve the above-mentioned problems, and an object thereof is to provide an electronic device substrate having a nitride semiconductor formed on single crystal silicon, in which occurrence of slip, cracking, etc. is suppressed and which has high destructive strength, and a method for manufacturing the same.

[0012] (II) Technical solution

[0013] In order to solve the above-mentioned problems, the present invention provides a substrate for electronic devices, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, and the substrate is characterized in that:

[0014] The combined substrate is a substrate formed by combining a first single crystal silicon substrate and a second single crystal silicon substrate via an oxide film, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100},

[0015] The nitride semiconductor film is formed on the surface of the first single crystal silicon substrate of the bonding substrate.

[0016] Regarding the crystal plane orientation, it is not a just substrate without an off-angle like the usual second single crystal silicon substrate. By setting it to have an off-angle like the second single crystal silicon substrate of the present invention, the cleavage plane will be non-vertical (the cleavage plane is inclined) relative to the main surface (the bonding surface with the first single crystal silicon substrate). In this way, even if there is only one second single crystal silicon substrate, the cleavage plane will be inclined. Therefore, compared with the case of existing products in which the cleavage plane of the second single crystal silicon substrate is also perpendicular to the bonding surface, it is possible to produce a substrate for electronic devices with high destructive strength, in which the increase of warping and the occurrence of slip and cracking (hereinafter also referred to as cracking, etc.) are suppressed.

[0017] In this case, the second single crystal silicon substrate may be a nitrogen-doped substrate.

[0018] With such a structure, the electronic device substrate has higher fracture strength.

[0019] In addition, it can be,

[0020] The first single crystal silicon substrate is <110> A substrate with a notch is formed in the direction,

[0021] The second single crystal silicon substrate is <110> A substrate with a notch is formed in the direction,

[0022] The bonded substrate is a substrate bonded so that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

[0023] With such a structure, the occurrence of cracks and the like is further suppressed due to the positional relationship between the cleavage planes of the first single crystal silicon substrate and the second single crystal silicon substrate to be bonded together, thereby achieving a substrate for an electronic device with high destructive strength.

[0024] Furthermore, the diameter of the bonding substrate may be greater than or equal to 300 mm.

[0025] As described above, the substrate having high fracture strength of the present invention is particularly effective for a substrate for electronic devices having a large diameter of 300 mm or more.

[0026] In addition, the present invention provides a method for manufacturing a substrate for an electronic device, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, and the method is characterized by comprising the following steps:

[0027] Preparing a first single crystal silicon substrate and a second single crystal silicon substrate, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100};

[0028] Thermally oxidizing at least one of the first single crystal silicon substrate and the second single crystal silicon substrate to form an oxide film on the surface;

[0029] Overlaying the first single crystal silicon substrate and the second single crystal silicon substrate with the oxide film interposed therebetween, and performing heat treatment to thereby combine the first single crystal silicon substrate and the second single crystal silicon substrate to manufacture the combined substrate; and

[0030] The nitride semiconductor film is epitaxially grown on the surface of the first silicon single crystal substrate of the bonding substrate.

[0031] According to the method for manufacturing an electronic device substrate of the present invention, a substrate for an electronic device having a high destructive strength and in which occurrence of cracks is suppressed can be manufactured, including a second single crystal silicon substrate having a cleavage plane inclined with respect to a bonding plane.

[0032] In this case, the prepared second single crystal silicon substrate may be a nitrogen-doped substrate.

[0033] By doing so, it is possible to manufacture a substrate for an electronic device having a higher breaking strength.

[0034] In addition, the first single crystal silicon substrate may be prepared as follows: <110> A substrate with a notch is formed in the direction,

[0035] The prepared second single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction,

[0036] The first single crystal silicon substrate and the second single crystal silicon substrate are overlapped and bonded in such a manner that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

[0037] In this way, it is possible to manufacture a substrate for an electronic device with high destructive strength in which the occurrence of cracks and the like is further suppressed, depending on the positional relationship of the cleavage planes of the first single crystal silicon substrate and the second single crystal silicon substrate to be bonded together.

[0038] Furthermore, the diameters of the prepared first single crystal silicon substrate and the prepared second single crystal silicon substrate may be set to be 300 mm or more.

[0039] The electronic device substrate having high breaking strength produced by the production method of the present invention is particularly effective in producing an electronic device substrate having a large diameter of 300 mm or more.

[0040] (III) Beneficial effects

[0041] According to the electronic device substrate and the method for manufacturing the same of the present invention, a second single crystal silicon substrate having a cleavage plane inclined with respect to a bonding plane and having an off-angle can be provided, thereby providing an electronic device substrate with high destructive strength and in which the occurrence of cracks etc. is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a schematic cross-sectional view showing an example of the electronic device substrate of the present invention.

[0043] Figure 2 It is an explanatory diagram showing an example of the positional relationship between the cleavage plane in the first single crystal silicon substrate and the cleavage plane in the second single crystal silicon substrate.

[0044] Figure 3 FIG. 1 is a schematic diagram showing an example of cleavage surfaces of the first single crystal silicon substrate and the second single crystal silicon substrate as viewed from the main surface side.

[0045] Figure 4 FIG. 1 is a schematic diagram showing another example of the cleavage planes of the first single crystal silicon substrate and the second single crystal silicon substrate as viewed from the main surface side.

[0046] Figure 5 This is a flow chart schematically showing an example of the method for producing the electronic device substrate of the present invention.

[0047] Figure 6These are photographs of a state where a bonded substrate is placed in a wafer BOX after the oxide film is removed in the example and the comparative example.

[0048] Figure 7 It is a schematic diagram showing the conditions of the breaking load and bending strength test. Figure 7 (a) is a diagram viewed from the upper side in the vertical direction. Figure 7 (b) is a view viewed from the side. DETAILED DESCRIPTION

[0049] Hereinafter, the present invention will be described in detail with reference to the drawings, but the present invention is not limited thereto.

[0050] [Substrates for electronic devices]

[0051] like Figure 1 As shown, the electronic device substrate 20 of the present invention has a nitride semiconductor film 21 formed on a single crystal silicon bonding substrate 10. In the description of the present invention, the single crystal silicon bonding substrate 10 may also be referred to as simply a "bonding substrate". In this case, the bonding substrate 10 is a substrate formed by bonding a first single crystal silicon substrate 11 and a second single crystal silicon substrate 12 via an oxide film 13, wherein the crystal plane orientation of the first single crystal silicon substrate 11 is {111}, and the main surface of the second single crystal silicon substrate 12 has an angle relative to the crystal plane orientation {100}. Figure 1 As shown, a nitride semiconductor film 21 is formed on a first single crystal silicon substrate 11 .

[0052] In addition, in this specification, the dash before the number in the usual Miller index notation is replaced by a "-". That is, the notation such as [1-10] is different from Have the same meaning.

[0053] In addition, the notation for the Miller index is as generally indicated. That is, {} means the general term for equivalent crystal plane orientations, and () means each orientation of the crystal plane orientation. In addition, <> represents the general term for equivalent crystal axis directions, and [] means each direction of the crystal axis direction.

[0054] Here, as described above, in order to make the epitaxial substrate for power devices have a high withstand voltage, it is necessary to produce a substrate for electronic devices in which a nitride semiconductor film is formed thickly on a single crystal silicon substrate (for example, GaN on Si in which the thickness of the GaN epitaxial layer is thickened). To thicken the thickness of the epitaxial layer, it is sufficient to thicken the single crystal silicon substrate and perform epitaxial growth. In addition, as a method for thickening the silicon crystal plate, a step of bonding two single crystal silicon substrates is performed, but even using a bonded substrate, it is still impossible to completely suppress the occurrence of cracks, etc.

[0055] However, in the electronic device substrate 20 of the present invention, as described above, a substrate formed by combining the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 is used as a base substrate (seed crystal) (combined substrate 10), and further, in the second single crystal silicon substrate 12, the main surface has an angle relative to the crystal plane orientation {100}, so the cleavage plane is non-vertical relative to the bonding surface with the first single crystal silicon substrate. In this case, compared with existing products using just substrates without an angle, it is possible to produce a substrate for electronic devices with high destructive strength and in which the occurrence of cracks (increase in warping, slippage, cracks) is suppressed.

[0056] Figure 2 1 is an explanatory diagram showing an example of the positional relationship between the cleavage planes in the first single crystal silicon substrate 11 and the cleavage planes in the second single crystal silicon substrate 12. In addition, here, the case where these cleavage planes are located close to each other in the vertical direction of the main surface (that is, when they are located close to each other in a plan view) is described as an example, but the present invention is not limited to such a positional relationship. In addition, Figure 2 In the example, the case where there is an angle in the left and right directions on the paper is cited, but the direction of the angle is not particularly limited in the present invention. That is, in a top view, no matter whether the positions of the cleavage planes of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are close or far from each other, and no matter what direction the angle of the second single crystal silicon substrate 12 is (for example, even in Figure 2 The front and rear direction on the paper surface) can still achieve the above-mentioned effect of preventing cracking, etc.

[0057] On the other hand, if both substrates are just substrates without off angles, cracks and the like are likely to occur.

[0058] The size of the off angle is not particularly limited, and can be, for example, greater than 0° and less than 12°, preferably 2° to 8°, and particularly preferably 4°.

[0059] In addition, in the present invention, the formation positions of the notches of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are not particularly limited.

[0060] In the example described below, the first single crystal silicon substrate 11 is <110> The second single crystal silicon substrate 12 is formed with a notch in the direction <110> Furthermore, the bonding substrate 10 is bonded so that the position of the notch of the first single crystal silicon substrate 11 and the position of the notch of the second single crystal silicon substrate 12 coincide with each other.

[0061] With such a structure, the effect of the above-mentioned off-angle (improvement of fracture strength) can be obtained, and the fracture strength can be further improved by shifting the positions of the cleavage planes of the first single crystal silicon substrate and the second single crystal silicon substrate in a plan view.

[0062] More specifically, with respect to the case where the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are bonded as described above, referring to the diagram as viewed from the main surface (main surface) side of each substrate. Figure 3 Here, the following structure is used as an example for explanation: as the first single crystal silicon substrate 11, the crystal plane orientation is {111}, and the notch is located at <110> As the second single crystal silicon substrate 1, the crystal plane orientation is {100}, and the notch is located at <110> location.

[0063] exist Figure 3 In the figure, the cleavage plane of the first single crystal silicon substrate 11 is schematically indicated by a dotted line, and the cleavage plane of the second single crystal silicon substrate 12 is schematically indicated by a dashed line. Figure 1 As shown, if the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are overlapped, it can be seen that the longitudinal cleavage plane in the figure is offset. The transverse cleavage planes in the figure overlap. However, in the entire combined substrate 10, the substrate strength of the combined substrate 10 is improved due to the effect of the longitudinal cleavage plane offset in the figure. As a result, even if there is a nitride semiconductor film 21 formed on the surface of the first single crystal silicon substrate 11 of the combined substrate 10, it is still possible to produce a substrate 20 for electronic devices with high destructive strength in which the occurrence of cracks, etc. is further suppressed.

[0064] Furthermore, in the electronic device substrate 20 of the present invention, the nitride semiconductor film 21 is formed on the surface of the first single crystal silicon substrate 11 having a crystal plane orientation of {111}, so that a good nitride semiconductor film 21 is formed.

[0065] Figure 4 Other examples of bonding substrates are shown in FIG. Figure 4 In the example, the following structure is used as an example: as the first single crystal silicon substrate, the crystal plane orientation is {111}, and the notch is located at <110> As the second single crystal silicon substrate, the crystal plane orientation is {100}, and the notch is located at <100> At this time, the crystal axis direction of the second single crystal silicon substrate where the notch is formed is aligned with Figure 3 The situation is different, but the others are the same Figure 3 Same. Figure 4 It can be seen that if the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are superimposed, the cleavage planes are all in close position. Figure 4 In the case of, since two single crystal silicon substrates having crystal plane orientations of {111} and {100} are bonded, and the second single crystal silicon substrate 12 has the above-mentioned off-angle, the strength of the bonded substrate and the electronic device substrate becomes higher, but Figure 4 compared to, Figure 3 The intensity of the situation is higher.

[0066] In the electronic device substrate 20 of the present invention, since the substrate strength is high as described above, the diameter of the combined substrate 10 (and the electronic device substrate 20) can be set to a large diameter of 300 mm or more. In the past, for such a large-diameter substrate, the substrate strength was sometimes insufficient, and cracks occurred, but the present invention can produce a substrate for electronic devices with high destructive strength while suppressing these situations. The upper limit of the diameter of the combined substrate 10 (and the electronic device substrate 20) is not limited, and can be set to 450 mm or less, for example.

[0067] When the diameter of the combined substrate 10 (and the electronic device substrate 20) is 300 mm or more, the diameters of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are also 300 mm or more. The thickness of each of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 is not particularly limited, and substrates corresponding to the specifications can be used appropriately. In particular, when the diameter is 300 mm, the thickness can be set to 775 μm. Such a single crystal silicon substrate is used as a substrate for a general device, which is cheap and can be used without any particular problems. As the thickness of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12, for example, 500 μm to 1500 μm can be used.

[0068] In addition, the second single crystal silicon substrate 12 may be a nitrogen-doped substrate. By doping with nitrogen, the strength of the second single crystal silicon substrate 12 is further increased, and the electronic device substrate 20 has a further higher breaking strength. The nitrogen concentration is not particularly limited, and can be, for example, 5×10 13 ~5×10 15 atoms / cm 3 .

[0069] [Method for producing a substrate for electronic devices]

[0070] Below, refer to Figure 5 A method for producing the electronic device substrate 20 of the present invention as described above will be described.

[0071] First, if Figure 5 As shown in step S11, a first single crystal silicon substrate 11 and a second single crystal silicon substrate 12 are prepared (step S11). At this time, the following single crystal silicon substrates are prepared as the first single crystal silicon substrate 11, whose crystal plane orientation is {111}, and <110> In addition, the following single crystal silicon substrate is prepared as the second single crystal silicon substrate 12, whose main surface has an off-angle relative to the crystal plane orientation {100} and <110> There is a gap in the direction.

[0072] In addition, when preparing the second single crystal silicon substrate 12 with a deflection angle, for example, it can be obtained by the following method: <100> An ingot is then cut at the desired deflection angle.

[0073] At this time, the diameters of the prepared first single crystal silicon substrate and the second single crystal silicon substrate can be set to 300 mm or more.

[0074] In addition, the second single crystal silicon substrate can be a nitrogen-doped substrate. The nitrogen doping method is not particularly limited, and a known method can be used. For example, in the process of manufacturing single crystal silicon by the CZ method, a silicon wafer with a nitride film can be used as a raw material to manufacture a nitrogen-doped silicon ingot and cut it. In addition, of course, the first single crystal silicon substrate can also be doped with nitrogen.

[0075] Furthermore, since the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are bonded to produce a single single crystal silicon substrate bonded substrate 20 , the first single crystal silicon substrate 11 can be referred to as a bonded wafer, and the second single crystal silicon substrate 12 can be referred to as a base wafer.

[0076] The thickness of each of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 is not particularly limited, and substrates corresponding to the specifications can be used appropriately. In addition, the resistivity and impurity concentration of each of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 can be appropriately set.

[0077] Then, if Figure 5 As shown in step S12 of FIG. 1 , at least one of the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 is thermally oxidized to form an oxide film on the surface (step S12). The oxide film formed here becomes as shown in step S12 after the two single crystal silicon substrates are combined. Figure 1 The oxide film 13 shown. The means for forming the oxide film is not particularly limited, and for example, an oxidation heat treatment can be performed to form an oxide film with a thickness of about 100 nm on the surface. The thickness of the oxide film is not particularly limited, and for example, it can be set to be greater than 10 nm and less than 1000 nm. The oxide film can be formed on each of the two single crystal silicon substrates, or on any one of the single crystal silicon substrates.

[0078] Then, if Figure 5 As shown in step S13, the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are combined (step S13). At this time, first, it is preferred to overlap the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 in such a way that the position of the notch of the first single crystal silicon substrate 11 coincides with the position of the notch of the second single crystal silicon substrate 12. At this time, the two single crystal silicon substrates are overlapped with each other through the oxide film formed in step S12. By performing heat treatment in this state, the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are combined to form a combined substrate 10 (refer to Figure 1 ).

[0079] The conditions (atmosphere, temperature, time, etc.) of the heat treatment (bonding heat treatment) are not particularly limited as long as the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 can be bonded. The bonding heat treatment temperature can be set to, for example, 400° C. to 1200° C. in a nitrogen atmosphere for 1 to 12 hours.

[0080] Preferably, after the bonding heat treatment, the surface of the bonding substrate 10 is cleaned before the epitaxial growth of the nitride semiconductor film described later. It is particularly preferred to remove the oxide film formed on the surface of the bonding substrate 10 (particularly the surface of the first single crystal silicon substrate 11) by hydrofluoric acid spin cleaning or the like.

[0081] In this way, after the first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 are combined to form a combined substrate 10, as shown in FIG. Figure 5 As shown in S14, a nitride semiconductor film 21 (see Figure 1 ) for epitaxial growth (step S14). In addition, the first single crystal silicon substrate 11 may be double-sided polished before the bonding. Even if double-sided polishing is not performed before the bonding, single-sided polishing may be performed in advance on the main surface to be grown after the bonding and before the epitaxial growth. Of course, double-sided polishing may also be performed on the second single crystal silicon substrate 12.

[0082] As the nitride semiconductor film 21, an AlN layer, a GaN layer, an AlGaN layer, etc. can be formed. The nitride semiconductor film 21 can be formed by a conventional method. In addition, an intermediate layer (buffer layer) can be formed appropriately. In this way, it is possible to manufacture Figure 1 The electronic device substrate 20 is shown.

[0083] Example

[0084] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples; however, the present invention is not limited to the following Examples.

[0085] (Example 1)

[0086] according to Figure 5 The method for manufacturing a substrate for an electronic device of the present invention is as shown in Figure 1 The electronic device substrate 20 is shown.

[0087] First, the following single crystal silicon substrates are prepared (step S11): as the first single crystal silicon substrate 11, it is a double-sided polished, 300 mm in diameter, 775 μm in thickness, {111} in crystal plane orientation, p-type, and 1 kΩcm in resistivity. <110> and, as a second single crystal silicon substrate 12, a double-sided polished diameter of 300mm, a thickness of 775μm, a crystal plane orientation {100}, p-type, a resistivity of 30kΩcm and in <110> A single crystal silicon substrate having a notch formed in the direction is prepared (step S11).

[0088] The first single crystal silicon substrate 11 and the second single crystal silicon substrate 12 have the following Figure 3 The cleavage plane is shown as a conceptual diagram in FIG.

[0089] In addition, regarding the crystal plane orientation, the first single crystal silicon substrate 11 is a just substrate without an off-angle, and the second single crystal silicon substrate 12 is a structure with an off-angle (4°). The direction of the off-angle is set to the direction opposite to the notch ( Figure 3 0 point direction).

[0090] In addition, the first single crystal silicon substrate 11 is a substrate not doped with nitrogen, and the second single crystal silicon substrate 12 is a substrate doped with nitrogen, and the nitrogen concentration is 5×10 13 atoms / cm 3 .

[0091] The two prepared single crystal silicon substrates were subjected to oxidation heat treatment to form an oxide film having a thickness of 100 nm on each substrate (step S12 ).

[0092] Next, the two single crystal silicon substrates are bonded together by aligning the notch positions, and a bonding heat treatment is performed at 500°C in a nitrogen atmosphere to form a bonded substrate 10 (step S13). After that, the bonded substrate 10 is subjected to hydrofluoric acid spin cleaning to remove the oxide film on the surface. Figure 6 This shows the state where the wafer is placed in a wafer BOX after the oxide film is removed.

[0093] Next, on the surface of the first single crystal silicon substrate 11 combined with the substrate 10, the following layers are epitaxially grown with a total film thickness of 1.8 μm to serve as a nitride semiconductor film 21. These layers are: 150 nm AlN layer, 160 nm AlGaN layer, a superlattice structure in which 25 groups of GaN layers and AlN layers are alternately stacked, 1000 nm GaN layer, 20 nm AlGaN layer, and 3 nm GaN layer.

[0094] As a result, GaN can be formed without causing cracks or slips. In this way, the electronic device substrate 20 is manufactured.

[0095] (Comparative Example 1)

[0096] As described below, unlike Example 1, a just substrate having no off angle was used as the second single crystal silicon substrate. The electronic device substrate was manufactured in the same manner as Example 1.

[0097] First, the following single crystal silicon substrates were prepared: as the first single crystal silicon substrate, a double-sided polished substrate with a diameter of 300 mm, a thickness of 775 μm, a crystal plane orientation of {111}, a p-type substrate, a resistivity of 1 kΩcm, and <110> A single crystal silicon substrate having a notch formed in the direction; and, as a second single crystal silicon substrate, a double-sided polished single crystal silicon substrate having a diameter of 300 mm, a thickness of 775 μm, a crystal plane orientation of {100}, a p-type substrate, a resistivity of 30 kΩ cm and <110> A single crystal silicon substrate with a notch formed in the direction.

[0098] The first single crystal silicon substrate and the second single crystal silicon substrate have the following Figure 3 The cleavage plane is shown as a conceptual diagram in FIG.

[0099] In addition, with respect to the crystal plane orientation, both the first single crystal silicon substrate and the second single crystal silicon substrate are just substrates without off-angles.

[0100] In addition, the first single crystal silicon substrate is a substrate not doped with nitrogen, and the second single crystal silicon substrate is a substrate doped with nitrogen, and the nitrogen concentration is 5×10 13 atoms / cm 3 .

[0101] The two prepared single crystal silicon substrates were subjected to oxidation heat treatment to form an oxide film with a thickness of 100 nm on each substrate.

[0102] Next, the notch positions of the two single crystal silicon substrates are aligned and bonded together, and a bonding heat treatment is performed at 500°C in a nitrogen atmosphere to produce a bonded substrate. Figure 6 As shown, the bonding heat treatment process in Example 1 is performed simultaneously. After that, the bonding substrate 10 is subjected to hydrofluoric acid spin cleaning to remove the oxide film on the surface. In addition, after the oxide film is removed, it is placed in the wafer BOX (refer to Figure 6 ).

[0103] Next, a GaN film was epitaxially grown as a nitride semiconductor film on the surface of the first single crystal silicon substrate of the bonding substrate under the same conditions as in Example 1.

[0104] As a result, although slippage and the like did not occur, the breaking strength was inferior to that of Example 1 as described later.

[0105] Hereinafter, Example 1 and Comparative Example 1 were respectively used to prepare bonding substrates before forming a nitride semiconductor film under the same conditions, and then the strength of each bonding substrate was measured.

[0106] In the strength measurement of the bonded substrate, Figure 7 As shown, the breaking load and bending strength were investigated using a precision universal testing machine manufactured by Instron Corporation. Figure 7 (a) is a diagram viewed from the upper side in the vertical direction. Figure 7 (b) is a view viewed from the side.

[0107] like Figure 7 As shown in (a) and (b), three support jigs J are arranged above and below the bonding substrate (the curvature radius R of the press-contact point is 15 mm). In the bonding substrate, the notch position is weak in terms of strength, so the notch position N is set so as to be directly below the central support jig J (refer to Figure 7 (a), (b)). The calculation formula for bending strength is as follows.

[0108] Bending strength = 3PL / 2WT 2 (Calculation formula)

[0109] P: Breaking load

[0110] L = distance between fulcrums (150mm)

[0111] W: Width 300nm

[0112] T: Thickness 1.55mm

[0113] As a result, the breaking load of the notch portion of the bonding substrate 10 in Example 1 was 784N, and the bending strength was 245MPa. On the other hand, the breaking load of the notch portion of the bonding substrate in Comparative Example 1 was 732N, and the bending strength was 228MPa. It can be judged that the breaking strength of the bonding substrate 10 in Example 1 is higher than that in Comparative Example 1.

[0114] (Example 2, Comparative Example 2)

[0115] An electronic device substrate (Example 2) was prepared in the same manner as in Example 1 except that a substrate not doped with nitrogen was used as the second single crystal silicon substrate. As a result, GaN was formed without causing cracks or slip.

[0116] Furthermore, an electronic device substrate (Comparative Example 2) was manufactured in the same manner as in Comparative Example 1 except that a substrate not doped with nitrogen was used as the second single crystal silicon substrate, unlike Comparative Example 1. As a result, although slip and the like did not occur, the fracture strength was inferior to that of Example 2 as described later.

[0117] In addition, Example 2 and Comparative Example 2 respectively prepared bonding substrates before forming a nitride semiconductor film under the same conditions, and then measured the strength of each bonding substrate. The measurement method was the same as that of Example 1 and Comparative Example 1.

[0118] As a result, the fracture load of the notch portion of the bonding substrate 10 in Example 2 was 713N, and the bending strength was 223MPa. On the other hand, the fracture load of the notch portion of the bonding substrate in Comparative Example 2 was 663N, and the bending strength was 207MPa. It can be judged that the fracture strength of the bonding substrate 10 in Example 2 is higher than that in Comparative Example 2.

[0119] The above results of breaking load and bending strength are summarized in Table 1.

[0120] [Table 1]

[0121]

[0122] As described above, it can be seen from Table 1 that in terms of breaking load and bending strength, when nitrogen is doped (Example 1 and Comparative Example 1), Example 1 implementing the present invention shows results superior to Comparative Example 1. In addition, when nitrogen is not doped (Example 2, Comparative Example 2), Example 2 implementing the present invention also shows results superior to Comparative Example 2.

[0123] In addition, although the numerical value of Comparative Example 1 is better than that of Example 2, this is the result of the difference in whether or not nitrogen is doped. From the above results, it can be clearly understood that when the conditions other than the bias angle such as whether or not nitrogen is doped are the same, as long as the second single crystal silicon substrate of the present invention has a bias angle, it is superior in terms of breaking load and bending strength compared to the case without a bias angle, and is extremely effective in suppressing existing problems such as increase in warpage and cracking.

[0124] (Example 3-6)

[0125] An electronic device substrate was manufactured in the same manner as in Example 1 except that a substrate having an off angle of 2° (Example 3) or an off angle of 8° (Example 4) was used as the second single crystal silicon substrate.

[0126] An electronic device substrate was manufactured in the same manner as in Example 2 except that a substrate with an off angle of 2° (Example 5) or an off angle of 8° (Example 6) was used as the second single crystal silicon substrate.

[0127] As a result, GaN can be formed without causing cracks or slip.

[0128] In addition, in Examples 3 to 6, bonding substrates before forming a nitride semiconductor film were prepared under the same conditions, and the strength of each bonding substrate was measured. The measurement method was the same as that in Example 1.

[0129] As a result, the breaking load and bending strength of the notch portion of the bonded substrate 10 in Example 3-6 were as follows: (753 N, 235 MPa), (803 N, 251 MPa), (697 N, 218 MPa), and (731 N, 228 MPa).

[0130] From these results, it can be seen that the fracture strength of the bonded substrates 10 of Examples 3 and 4 is higher than that of Comparative Example 1. In addition, the fracture strength of the bonded substrates 10 of Examples 5 and 6 is higher than that of Comparative Example 2.

[0131] The results of the breaking load and bending strength of Examples 3-6 are summarized in Table 2.

[0132] [Table 2]

[0133]

[0134] As described above, it can be seen from Tables 1 and 2 that in terms of breaking load and bending strength, when nitrogen is doped (Examples 3 and 4 and Comparative Example 1), Examples 3 and 4 implementing the present invention show results superior to Comparative Example 1. In addition, when nitrogen is not doped (Examples 5 and 6, Comparative Example 2), Examples 5 and 6 implementing the present invention show results superior to Comparative Example 2.

[0135] Furthermore, from the comparison between Examples 1, 3, and 4 and the comparison between Examples 2, 5, and 6, it can be seen that the larger the off-angle, the better the breaking strength.

[0136] In addition, although Comparative Example 1 shows a numerical value that is superior to or equal to that of Examples 5 and 6, this is due to the same reason as when Comparative Example 1 is compared with Example 2, and is the result of the difference in whether nitrogen is doped or not. When the conditions other than the off-angle are the same, as long as the second single crystal silicon substrate of the present invention has an off-angle, it has a higher breaking strength than the case without an off-angle, which can help suppress the increase of warpage and the occurrence of cracks.

[0137] This manual contains the following methods.

[0138] [1] A substrate for an electronic device, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, wherein:

[0139] The combined substrate is a substrate formed by combining a first single crystal silicon substrate and a second single crystal silicon substrate via an oxide film, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100},

[0140] The nitride semiconductor film is formed on the surface of the first single crystal silicon substrate of the bonding substrate.

[0141] [2] The electronic device substrate according to [1] above, wherein the second single crystal silicon substrate is a nitrogen-doped substrate.

[0142] [3] The electronic device substrate according to [1] or [2], wherein the first single crystal silicon substrate is <110> A substrate with a notch is formed in the direction,

[0143] The second single crystal silicon substrate is <110> A substrate with a notch is formed in the direction,

[0144] The bonded substrate is a substrate bonded so that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

[0145] [4] The electronic device substrate according to any one of [1] to [3] above, wherein the diameter of the bonded substrate is 300 mm or more.

[0146] [5] A method for manufacturing a substrate for an electronic device, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, the method comprising the following steps:

[0147] Preparing a first single crystal silicon substrate and a second single crystal silicon substrate, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100};

[0148] Thermally oxidizing at least one of the first single crystal silicon substrate and the second single crystal silicon substrate to form an oxide film on the surface;

[0149] Overlaying the first single crystal silicon substrate and the second single crystal silicon substrate with the oxide film interposed therebetween, and performing heat treatment to thereby combine the first single crystal silicon substrate and the second single crystal silicon substrate to manufacture the combined substrate; and

[0150] The nitride semiconductor film is epitaxially grown on the surface of the first silicon single crystal substrate of the bonding substrate.

[0151] [6] The method for manufacturing an electronic device substrate according to [5] above, wherein the prepared second single crystal silicon substrate is a nitrogen-doped substrate.

[0152] [7] The method for manufacturing an electronic device substrate according to [5] or [6] above, wherein the first single crystal silicon substrate is prepared <110> A substrate with a notch is formed in the direction,

[0153] The prepared second single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction,

[0154] The first single crystal silicon substrate and the second single crystal silicon substrate are overlapped and bonded in such a manner that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

[0155] [8] The method for manufacturing a substrate for an electronic device as described in any one of [5] to [7] above, wherein the diameters of the prepared first single crystal silicon substrate and the second single crystal silicon substrate are set to be greater than 300 mm.

[0156] The present invention is not limited to the above-described embodiments. The above-described embodiments are illustrative, and any scheme having substantially the same structure and achieving the same function and effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.

Claims

1. A substrate for electronic devices, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, characterized in that: The combined substrate is a substrate formed by combining a first single crystal silicon substrate and a second single crystal silicon substrate via an oxide film, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100}, The nitride semiconductor film is formed on the surface of the first single crystal silicon substrate of the bonding substrate.

2. The electronic device substrate according to claim 1, wherein: The second single crystal silicon substrate is a nitrogen-doped substrate.

3. The electronic device substrate according to claim 1, wherein: The first single crystal silicon substrate is <110> A substrate with a notch is formed in the direction, The second single crystal silicon substrate is <110> A substrate with a notch is formed in the direction, The bonded substrate is a substrate bonded so that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

4. The electronic device substrate according to claim 2, characterized in that: The first single crystal silicon substrate is <110> A substrate with a notch is formed in the direction, The second single crystal silicon substrate is <110> A substrate with a notch is formed in the direction, The bonded substrate is a substrate bonded so that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

5. The electronic device substrate according to any one of claims 1 to 4, characterized in that: The diameter of the bonding substrate is greater than 300 mm.

6. A method for manufacturing a substrate for an electronic device, wherein a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, characterized in that: It has the following processes: Preparing a first single crystal silicon substrate and a second single crystal silicon substrate, wherein the crystal plane orientation of the first single crystal silicon substrate is {111}, and the main surface of the second single crystal silicon substrate has an off-angle relative to the crystal plane orientation {100}; Thermally oxidizing at least one of the first single crystal silicon substrate and the second single crystal silicon substrate to form an oxide film on the surface; Overlaying the first single crystal silicon substrate and the second single crystal silicon substrate with the oxide film interposed therebetween, and performing heat treatment to thereby combine the first single crystal silicon substrate and the second single crystal silicon substrate to manufacture the combined substrate; and The nitride semiconductor film is epitaxially grown on the surface of the first silicon single crystal substrate of the bonding substrate.

7. The method for manufacturing an electronic device substrate according to claim 6, wherein: The prepared second single crystal silicon substrate is set as a nitrogen-doped substrate.

8. The method for manufacturing an electronic device substrate according to claim 6, wherein: The first single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction, The prepared second single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction, The first single crystal silicon substrate and the second single crystal silicon substrate are overlapped and bonded in such a manner that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

9. The method for manufacturing an electronic device substrate according to claim 7, wherein: The first single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction, The prepared second single crystal silicon substrate is set <110> A substrate with a notch is formed in the direction, The first single crystal silicon substrate and the second single crystal silicon substrate are overlapped and bonded in such a manner that the position of the notch of the first single crystal silicon substrate coincides with the position of the notch of the second single crystal silicon substrate.

10. The method for manufacturing a substrate for an electronic device according to any one of claims 6 to 9, characterized in that: The diameters of the prepared first single crystal silicon substrate and the second single crystal silicon substrate are set to be 300 mm or more.

Citation Information

Patent Citations