Plastic optical fiber and medical sensor device

By adding carbon black sunscreen to the first and second claddings of the plastic optical fiber, the light propagation path is optimized, the noise problem caused by the propagation of the cladding light is solved, and the signal-to-noise ratio of the sensor is improved. It is suitable for all type of sensor application.

CN118891553APending Publication Date: 2024-11-01TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028233.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The noise problem caused by cladding light propagation in sensor applications has not been effectively solved, especially when used for short distances, noise can easily become detection errors.

Method used

A plastic optical fiber consisting of a core and a cladding is used, wherein the first cladding contains 100 to 10000 ppm of carbon black sunscreen, and a second cladding is formed on the outside, with a refractive index greater than the first cladding, in which the second cladding is It also contains 100 to 10000ppm carbon black sunscreen to optimize the light propagation path and reduce noise.

Benefits of technology

It effectively suppresses the noise generated by cladding light propagation, improves the signal-to-noise ratio of the sensor, and is suitable for industrial sensors and medical sensors, such as blood oxygen concentration measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005046648610000181
    Figure BDA0005046648610000181
Patent Text Reader

Abstract

Provided is a plastic optical fiber having an excellent noise suppression effect. This plastic optical fiber comprises a core and claddings, and is characterized in that a light-screening agent is contained in a first cladding adjacent to the core, the content of the light-screening agent is within the range of 100-10000 ppm, and it is preferable that a second cladding is further provided on the outside of the first cladding. In addition, the plastic optical fiber can be applied to a medical sensor device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to plastic optical fiber and medical sensor equipment. Background Art

[0002] Plastic optical fibers are superior to glass optical fibers in terms of processability, handling, and manufacturing costs, and are therefore used for short-distance optical signal transmission, light guides, sensors, and the like.

[0003] Plastic optical fiber is usually composed of two layers: the core and the first cladding. The core usually uses a polymer with excellent transparency and good weather resistance, represented by polymethyl methacrylate (hereinafter referred to as PMMA). On the other hand, in order to seal the light inside the core, the cladding needs to have a lower refractive index than the core, and fluorinated polymers are widely used. The condition for causing total reflection of light inside the core is that the propagation angle θ is smaller than the critical angle (total reflection angle) θ0. For the critical angle (total reflection angle) θ0, if the refractive index of the core is set to n1 and the refractive index of the cladding is set to n2, it can be calculated by Sinθ0=n2 / n1. On the other hand, light larger than the critical angle θ0 invades the cladding. The light that invades the cladding is totally reflected when the propagation angle is less than the critical angle (total reflection angle) θ1. The critical angle (total reflection angle) θ1 is calculated by Sinθ1=n3 / n2 from the refractive index n2 of the cladding and the refractive index n3 of the air. Since the refractive index n1 of the core is greater than the refractive index n2 of the cladding, the light that is totally reflected does not have a critical angle and will return to the core again. For the light that returns to the core via the cladding, when the optical fiber is used in a sufficiently long state for communication purposes, the light greater than the critical angle (total reflection angle) θ1 will be emitted into the air layer and gradually attenuated due to the scattering of light in the cladding and the bending of the optical fiber, so it will not become a big problem. However, when the optical fiber is used in a length of less than several meters for sensor purposes, the light propagating through the cladding will not be attenuated and detected, and thus become noise, which becomes a problem. As a plastic optical fiber to reduce this noise, a solution has been proposed in which a second cladding is formed by a resin layer with a refractive index higher than that of the first cladding adjacent to the core (for example, refer to patent document 1).

[0004] In addition, it has been proposed to add a light-shielding agent to the second cladding layer (for example, refer to Patent Document 2).

[0005] Furthermore, it has been proposed that the refractive index of the first cladding layer is larger than that of the second cladding layer, and a light-shielding agent is added to the second cladding layer (for example, Patent Document 3).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-227976

[0009] Patent Document 2: International Publication No. 2022 / 009653

[0010] Patent Document 3: Japanese Patent Application Publication No. 2002-98864 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in the method described in Patent Document 1, since the refractive index of the second cladding is greater than that of the first cladding, the critical angle (total reflection angle) between the first cladding and the second cladding disappears, and the light propagation through the first cladding is reduced. However, since the second cladding is sandwiched between the first cladding and the air layer, which have a lower refractive index than the second cladding, there is a problem of generating a new light propagation path through the second cladding.

[0013] In addition, in the scheme described in Patent Document 2, the refractive index of the second cladding is less than the refractive index of the first cladding. Therefore, there is a critical angle (total reflection angle) at the interface between the second cladding and the first cladding. Light greater than the critical angle invades the second cladding. Since the second cladding contains a sunscreen, the light invading the second cladding gradually decays. A portion of the light smaller than the critical angle is absorbed by the sunscreen on the surface of the second cladding, but most of the light is totally reflected.

[0014] Furthermore, in the scheme described in Patent Document 3, the refractive index of the second cladding is greater than the refractive index of the first cladding, so that the critical angle (total reflection angle) between the first cladding and the second cladding disappears, the light propagation through the first cladding is reduced, and the light intruding into the second cladding gradually attenuates. However, even in this scheme, the noise cannot be eliminated. This means that, usually in the case of forming an optical fiber by melt spinning, there is a compatibility layer of tens to hundreds of nm between each layer, so even if the refractive index of the second cladding is greater than the refractive index of the first cladding, the light will not completely intrude from the first cladding into the second cladding, and there is light reflected between the second cladding and the first cladding.

[0015] Therefore, the present invention provides a plastic optical fiber and a medical sensor device in which the plastic optical fiber is excellent in the effect of suppressing noise generated by light propagating through a cladding.

[0016] Means of solving the problem

[0017] The present invention has the following contents.

[0018] (1) A plastic optical fiber comprising a core and a cladding, wherein a light-shielding agent is contained in a first cladding adjacent to the core, and the content of the light-shielding agent is in the range of 100 to 10000 ppm.

[0019] (2) In the plastic optical fiber according to (1), the light-shielding agent contained in the first cladding is carbon black.

[0020] (3) The plastic optical fiber according to (1) or (2), further comprising a second cladding outside the first cladding.

[0021] (4) In the plastic optical fiber according to (3), the refractive index of the second cladding is greater than the refractive index of the first cladding.

[0022] (5) The plastic optical fiber according to (3) or (4), wherein the second cladding contains a light-shielding agent, and the content of the light-shielding agent is in the range of 100 to 10000 ppm.

[0023] (6) According to the plastic optical fiber described in (5), the transmittance t1 of light with a wavelength of 650 nm at the first cladding film thickness and the transmittance t2 of light with a wavelength of 650 nm at the second cladding film thickness have a relationship of t1>t2.

[0024] (7) In the plastic optical fiber according to (5) or (6), the light-shielding agent contained in the second cladding is carbon black.

[0025] (8) According to the plastic optical fiber described in any one of (5) to (7), the sun-shielding agent contained in the first cladding and the sun-shielding agent contained in the second cladding are made of the same material, and the sun-shielding agent content D1 of the first cladding and the sun-shielding agent content D2 of the second cladding are in the relationship of D1<D2.

[0026] (9) In the plastic optical fiber according to any one of (4) to (8), a film thickness T1 of the first cladding formed on the plastic optical fiber and a film thickness T2 of the second cladding formed on the plastic optical fiber satisfy a relationship of T1<T2.

[0027] (10) The plastic optical fiber according to any one of (1) to (9), wherein the core is made of polymethyl methacrylate, and the numerical aperture NA of the core and the first cladding is 0.65 or less.

[0028] (11) A medical sensor device comprising the plastic optical fiber according to any one of (1) to (10).

[0029] Effects of the Invention

[0030] According to the present invention, a plastic optical fiber having an excellent effect of suppressing noise generated through the cladding can be provided. Moreover, as the noise suppression effect, the excellent effect can also be exerted in plastic optical fibers used for a length of several meters or less, such as for sensors, where light propagating through cracks is not completely attenuated and easily becomes noise.

[0031] Therefore, according to the present invention, it is possible to provide a plastic optical fiber that is suitable for use in industrial sensors such as semiconductor manufacturing equipment and automobile manufacturing equipment, and medical sensors such as blood oxygen concentration measurement. DETAILED DESCRIPTION

[0032] Preferred embodiments of the plastic optical fiber and the plastic optical fiber cord including the same according to the present invention are described in detail below. However, the present invention is not limited to the following embodiments and can be implemented with various modifications according to the purpose and application.

[0033] The plastic optical fiber involved in the embodiment of the present invention has a core and a first cladding adjacent to the core in sequence. The first cladding is adjacent to the core and is arranged in a manner covering its periphery. It is also possible to have a second cladding on the outside of the first cladding, and it is also possible to have a coating on the outside of the first cladding, or on the outside of the second cladding arranged on the outside of the first cladding as required. Considering the centering of the optical axis when connecting the sensor connector, it is preferred that the core layer and the first cladding, as well as the second cladding and the coating arranged as required are substantially concentric.

[0034] In addition, when the plastic optical fiber of the present invention is used as a multi-core optical fiber, it is preferred that the first cladding adjacent to the core has a uniform thickness. Specifically, in the method for measuring the thickness of the first cladding described later, it is preferably the following shape: extract any three points of the first cladding at the interface between the first cladding and the air (or the second cladding, or the coating described later), that is, any three points on the outer circumference of the first cladding (3 points with a central angle of the arc in the range of 120°±10°), and a circle can be drawn by the three points. It should be noted that half of the value obtained by subtracting the core wire diameter from the diameter of the drawn circle is used as the first cladding thickness, and the core wire diameter is measured by the method described later. In the case where there is a second cladding on the outside of the first cladding, in the case of a 3-layer single core, it is preferred that the second cladding also has a uniform thickness. Specifically, it is preferred that a shape such as a circle can be drawn by extracting any three points of the interface between the second cladding and the air (or the coating described later), that is, any three points on the outer circumference of the second cladding (3 points with a central angle of the arc in the range of 120°±10°). Alternatively, a three-layer multi-core may be formed in which the second cladding exists as a sea outside the first cladding. In this case, the thickness of the second cladding is defined as the thickness of the thinnest portion.

[0035] (core)

[0036] The core material of the plastic optical fiber of the present invention is a (co)polymer with methyl methacrylate (hereinafter, sometimes referred to as MMA) as the main component of the copolymer component. Specifically, the copolymer containing polymethyl methacrylate (hereinafter, sometimes referred to as PMMA) or MMA as 70% by weight or more of the copolymer component, for example, can be exemplified by copolymerization of (meth)acrylate, (meth)acrylic acid, (substituted)styrene and (N-substituted)maleimide, or by polymer reaction thereof to obtain modified polymers such as glutaric anhydride and glutarimide. The above-mentioned (co)polymer represents polymers and copolymers. Similarly, (meth)acrylate represents acrylate and methacrylate. As (meth)acrylate, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, phenyl methacrylate, bornyl methacrylate and adamantyl methacrylate can be cited, and as substituted styrene, methyl styrene, α-methyl styrene can be cited. As N-substituted maleimide, N-isopropylmaleimide, N-cyclohexylmaleimide, N-methylmaleimide, N-ethylmaleimide and N-o-methylphenylmaleimide etc. can be listed. These copolymerization components can use multiple, and components other than these can also be used in small amounts. In addition, stabilizers such as antioxidants can also be contained only in an amount that does not adversely affect light transmittance.

[0037] In addition, as a polymer forming the core, for example, cycloolefin polymer (COP), cycloolefin copolymer (COC), polystyrene, polycarbonate, polyester containing fluorene, polymethylpentene, etc., it can also be preferably used in the combination of the core and the first cladding within the range of the optical fiber numerical aperture (hereinafter referred to as NA) not exceeding 0.65. If NA exceeds 0.65, the noise (hereinafter referred to as S / N ratio) of the plastic optical fiber in the present invention tends to become larger. The S / N ratio mentioned here refers to the value obtained by dividing the light intensity distribution emitted from the optical fiber into a region of θm / 10 inward from the one-sided maximum light emission angle θm calculated from the optical fiber numerical aperture (hereinafter referred to as NA) and a region of the maximum emission angle ±θm / 10, and dividing the maximum light intensity (S) of the region of θm / 10 inward from the maximum light emission angle by the maximum light intensity (N) of the region of ±θm / 10 of the maximum emission angle. For example, if the maximum light emission angle is 40°, the value is calculated by dividing the maximum light intensity (S) in the area 4° inward from the maximum light emission angle, that is, the area 0 to 36°, by the maximum light intensity (N) in the area 36 to 44°.

[0038] The core diameter of the plastic optical fiber of the present invention is preferably 100 to 3000 μm. By setting it to 100 μm or more, it is preferred as the plastic optical fiber of the present invention in terms of obtaining a sufficient amount of light. In addition, by setting it to 3000 μm or less, it is preferred in terms of a size suitable for use as a sensor.

[0039] The light quantity mentioned here refers to the transmission loss (dB / km) of the optical fiber calculated by the cutoff method.

[0040] (First cladding)

[0041] The plastic optical fiber of the present invention has a cladding in addition to the core, and the cladding adjacent to the core is called the first cladding. When the core material is PMMA (refractive index 1.48-1.50), the cladding material used in the first cladding is preferably a low-refractive fluororesin from the perspective of NA. As fluororesin, there is no particular restriction, and preferably a copolymer formed by vinylidene fluoride units and trifluoroethylene units (refractive index 1.39-1.41), a fluorinated acrylic acid ester polymer (refractive index 1.35-1.37) having a lower refractive index than the fluorinated acrylic acid ester and having good adhesion to PMMA and excellent processability, polymethacrylate perfluorobutyl ester (refractive index 1.36), polymethacrylate perfluoroisopropyl ester (refractive index 1.37), polymethacrylate hexafluoro 2-propyl ester (refractive index 1.38). In addition, for the purpose of further reducing the refractive index, dopants such as fluorine-based materials such as magnesium fluoride may also be added.

[0042] In addition, as a material for forming the cladding, for example, when a cycloolefin polymer (COP), a cycloolefin copolymer (COC), polystyrene, polycarbonate, a polyester containing fluorene, polymethylpentene, etc. is used as the core, PMMA can also be used as a resin other than a fluororesin for the cladding material as long as the NA in the combination with the cladding is within the range of not more than 0.65. If the core material is PMMA with a refractive index of about 1.49, the refractive index difference between the core and the cladding is preferably in the range of 0.03 to 0.15. In addition, if the core material is a cycloolefin polymer with a refractive index of about 1.54, the refractive index difference between the core and the cladding is preferably in the range of 0.03 to 0.15. In addition, if the core material is a polyester containing fluorene with a refractive index of about 1.64, the refractive index difference between the core and the cladding is preferably in the range of 0.03 to 0.14.

[0043] The first cladding of the plastic optical fiber of the present invention is characterized in that it contains a light-shielding agent. As the light-shielding agent, any of organic pigments and inorganic pigments can be used, for example, carbon black, titanium black, etc. can be used. Among them, carbon black is preferably used. Here, as the light to be shielded, the wavelength of 650 to 1000 nm commonly used as a sensor is assumed, but it is not necessarily limited to this. By containing a light-shielding agent, noise of light propagation through the first cladding can be suppressed.

[0044] In the plastic optical fiber of the present invention, the first cladding adjacent to the core preferably contains carbon black as a light shielding agent. The content of light shielding agents such as carbon black in the cladding material is preferably in the range of 100 to 10000 ppm. By making the content of light shielding agents such as carbon black greater than 100 ppm, noise detection can be suppressed. In addition, by making the content of light shielding agents such as carbon black less than 10000 ppm, it is possible to obtain a sufficient amount of light emitted from the core.

[0045] The carbon black content contained in the cladding of the optical fiber can be identified by SEM observation. When the cross section of the optical fiber is observed by SEM, the resin (cladding material) and carbon black constituting the cladding can be identified, thereby the area ratio of the resin and carbon black constituting the cladding can be calculated. If the area is multiplied by the specific gravity of each material, it can be calculated as a weight ratio. Considering the deviation, it is preferred to prepare SEM samples with different cross sections and calculate them as the average value of the measurements of 10 test objects. In addition, this content identification method can be applied not only to carbon black, but also to other organic pigments and inorganic pigments.

[0046] The first cladding thickness of the plastic optical fiber of the present invention is preferably 5 to 50 μm. By setting it to 5 μm or more, it can fully function as a cladding. In addition, by setting it to 50 μm or less, it will not form an excessive thickness as a cladding, which becomes a preferred size.

[0047] (Second cladding)

[0048] The plastic optical fiber of the present invention may also have a second cladding outside the first cladding. When the second cladding is included, the refractive index of the second cladding is preferably greater than the refractive index of the first cladding. Thus, as the above-mentioned second cladding, in addition to the function of protecting the first cladding, the following functions can also be given: by making the refractive index greater than that of the first cladding, the reflection at the interface between the first cladding and the second cladding is eliminated, and the light in the first cladding escapes to the second cladding, thereby inhibiting the propagation of light through the first cladding. However, as mentioned above, there is a compatibility layer formed by melt spinning of tens of nm to hundreds of nm between the first cladding and the second cladding, so the light intrusion from the first cladding to the second cladding is not 100%. The refractive index of the resin forming the second cladding can be greater than that of the resin forming the first cladding, and there is no special numerical regulation, but in the case where the first cladding is a fluororesin, a fluororesin with a refractive index greater than that of the fluororesin of the first cladding, or a resin such as PMMA can be used. In addition, in the case where the first cladding is a PMMA resin, a resin such as cycloolefin, polycarbonate, etc. with a refractive index greater than that of PMMA can be used.

[0049] The difference in refractive index between the second cladding and the first cladding is not a problem in principle as long as the refractive index of the second cladding is larger, but the difference in refractive index between the second cladding and the first cladding is preferably greater than 0.01. This is because the refractive index of the third digit below has batch variation of raw materials, and the refractive index difference may disappear.

[0050] The second cladding of the plastic optical fiber of the present invention preferably contains a light-shielding agent. As the light-shielding agent, any of organic pigments and inorganic pigments can be used, for example, carbon black, titanium black, etc. Among them, carbon black is preferably used.

[0051] The light that intrudes into the second cladding and is smaller than the critical angle between the second cladding and the air is reflected by the air interface having a lower refractive index than the second cladding. Furthermore, the light that is smaller than the critical angle between the first cladding and the second cladding in the reflected light is again reflected by the first cladding interface having a lower refractive index than the second cladding. In this way, noise caused by the propagation of light through the cladding is sometimes generated in the second cladding. Therefore, it becomes possible for a sunscreen such as carbon black to take on the role of absorbing these lights. As the sunscreen that can be used, the same sunscreen as the sunscreen exemplified as the sunscreen contained in the first cladding can be cited. The amount of sunscreen such as carbon black added is preferably in the range of 100 to 10000 ppm. By being less than 10000 ppm, the dispersibility of sunscreens such as carbon black becomes good, and the line diameter of the plastic optical fiber can be well maintained.

[0052] It is preferred that the light shielding agent contained in the first cladding of the plastic optical fiber of the present invention is composed of the same material as the light shielding agent contained in the second cladding, and the light shielding agent content D1 of the first cladding and the light shielding agent content D2 of the second cladding are in the relationship of D1<D2. This is because if the carbon black content D1 of the first cladding is high, the noise suppression effect becomes better, but due to the absorption of carbon black, a compromise occurs in that the amount of emitted light decreases. Therefore, it is easier to take both the noise suppression effect and the amount of emitted light into account by making the carbon black content D2 of the second cladding higher than D1. In addition, the second cladding also plays the role of blocking external interference light, so the higher the concentration, the better the blocking property against interference light.

[0053] In addition, the thickness T1 of the first cladding of the plastic optical fiber of the present invention formed on the plastic optical fiber and the thickness T2 of the second cladding formed on the plastic optical fiber preferably have a relationship of T1<T2. This is because if the thickness T1 of the first cladding is thick, the loss of light quantity due to light scattering in the first cladding becomes large, so when the second cladding exists, it is more effective to absorb more noise in the second cladding by making the thickness of the first cladding as thin as possible and making the thickness of the second cladding thicker.

[0054] In addition, the transmittance t1 of the light with a wavelength of 650nm under the first cladding film thickness of the plastic optical fiber of the present invention and the transmittance t2 of the light with a wavelength of 650nm under the second cladding film thickness preferably have a relationship of t1>t2. Here, the transmittance under the cladding film thickness refers to the transmittance when a film with the same film thickness as the film thickness of the cladding is made for each material used in the cladding. In practice, it is difficult to make a film with the same thickness as the cladding film thickness, so a 100μm film is formed and the transmittance is measured by a spectrophotometer. The transmittance at the cladding film thickness is calculated from the transmittance at the 100μm film thickness. This is because if the transmittance t1 of the light with a wavelength of 650nm under the first cladding film thickness is low, the noise suppression effect becomes better, but the compromise of a reduction in the amount of emitted light is produced due to the absorption of the light-shielding agent, so it is easier to take both the noise suppression effect and the amount of emitted light into account by making the transmittance t2 of the light with a wavelength of 650nm under the second cladding film thickness lower than t1. In addition, the second cladding layer also plays a role in shielding disturbance light from the outside, so the lower the transmittance, the better the shielding property against disturbance light.

[0055] In order to directly measure the transmittance of the cladding of the optical fiber, for example, the following method can be used. That is, the optical fiber is embedded in epoxy resin to collect a measurement sample. For the measurement sample, the cross section in the direction perpendicular to the longitudinal direction is polished until the length of the optical fiber in the longitudinal direction becomes 100μm, and a light with a wavelength of 650nm is irradiated from the cross section along the longitudinal direction using high-precision microspectroscopy to measure the transmittance of the cladding part. The transmittance of the cladding part with a thickness of 100μm is thus obtained. Based on the transmittance obtained at a thickness of 100μm, the transmittance under the cladding thickness is calculated.

[0056] (core material)

[0057] In addition, the core material of the plastic optical fiber of the present invention is most preferably polymethyl methacrylate, and the numerical aperture NA of the core and the first cladding is most preferably 0.65 or less. This is because the present invention contains a sunscreen in the cladding for the purpose of suppressing noise. On the other hand, the light absorption of the sunscreen may increase the transmission loss. Therefore, polymethyl methacrylate with the highest transmittance is preferred as the core material. In addition, from the perspective of suppressing noise, if the numerical aperture exceeds 0.65, that is, if the expansion of light exceeds ±40.5°, it is judged that the noise area is expanded, so NA is preferably 0.65 or less.

[0058] The type and amount of the light shielding agent and the film thickness of each cladding layer may be adjusted according to the required noise suppression degree, or these means may be combined to perform the adjustment.

[0059] (Manufacturing method of plastic optical fiber)

[0060] As a method for manufacturing plastic optical fiber, for example, the following composite spinning method is preferably used: the raw material for constituting the core material, the raw material for constituting the first cladding material, and the material for constituting the second cladding material as an optional component are fully dried under heating vacuum at 50 to 90° C., and then discharged from a composite die for concentric composite in a heated and molten state at 200 to 300° C. to form a core-sheath structure of two or three layers of core / first cladding / second cladding (optional component). Then, in order to improve mechanical properties such as breaking strength, a stretching treatment of about 1.2 to 3 times is usually performed to form a plastic optical fiber.

[0061] (Wire coating)

[0062] The plastic optical fiber involved in the embodiment of the present invention may have at least one coating layer on the outer layer of the above-mentioned plastic optical fiber. As the material forming the coating layer, for example, polyethylene, polypropylene or their copolymers, blends, olefin polymers containing organic silane groups, ethylene-vinyl acetate, polyvinyl chloride, polyvinylidene fluoride, polyamide resins such as nylon 12, polyester resins, nylon elastomers, polyester elastomers, polyurethane resins, fluororesins, rubbers such as EPM and EPDM, etc. can be listed. The coating layer can be a single layer or multiple layers. In the case of multiple layers, tension members such as "ケブラー" (registered trademark) can be added between the coating layers. In addition to flame retardants, these coating layers can also contain antioxidants, anti-aging agents, UV stabilizers and other stabilizers. It should be noted that the coating layer can be preferably formed by conventional methods such as melt extrusion molding using a crosshead die after first forming the plastic optical fiber by composite melt spinning.

[0063] (Plastic Optical Fiber)

[0064] The plastic optical fiber of the present invention thus obtained has an excellent effect of suppressing noise propagating through the cladding. As described above, even if the plastic optical fiber does not have a sufficient length for attenuating the noise, for example, a length of several meters or less, it has an excellent effect of suppressing noise generated by light propagating through the cladding, and can therefore be suitably used as a plastic optical fiber for industrial sensors such as semiconductor manufacturing equipment and automobile manufacturing equipment, and for medical sensors such as blood oxygen concentration measurement.

[0065] Example

[0066] Hereinafter, the present invention will be described in more detail by way of examples. It should be noted that the evaluations in the examples and comparative examples were performed by the following methods.

[0067] (1) Core diameter / Thickness of first cladding / Thickness of second cladding

[0068] The core diameter / thickness of the first cladding / thickness of the second cladding can be measured by the following method: for 5 randomly selected locations from the plastic optical fiber, cut perpendicularly to the extension direction, grind the cross section in such a way that the interface of the core / first cladding / second cladding can be observed, and then use a digital microscope VHX-7000 (manufactured by Keyence) to observe the enlargement, thereby measuring the core diameter / thickness of the first cladding / thickness of the second cladding. The magnification of the observation is between 10 and 200 times, and the range in which the entire cross section is within the field of view and the interface can be observed is selected. In the cross section, on the boundary circle formed by the interface between the core and the first cladding, 3 points are extracted in such a way that the central angle of each arc is in the range of 120°±10°, and the diameter of the circle drawn by the 3 points is taken as the core diameter. Extract any 3 points on the first cladding at the interface between the first cladding and the air (or second cladding) (3 points such that the central angle of the arc is in the range of 120°±10°), and half of the value obtained by subtracting the core diameter from the diameter of the drawn circle is taken as the first cladding thickness. Three arbitrary points (three points such that the central angle of the arc is in the range of 120°±10°) at the interface between the second cladding and the air are extracted, and half of the value obtained by subtracting the cladding diameter from the diameter of the drawn circle is taken as the second cladding thickness.

[0069] (2) Refractive index

[0070] A test piece of 10 mm×10 mm×3 mm was prepared from the materials used in each example and comparative example by injection molding at 250° C., and the refractive index was measured at room temperature 25° C. using an Abbe refractometer.

[0071] (3) Numerical aperture NA

[0072] The numerical aperture was calculated by the following formula based on the refractive index measured by the above method.

[0073] Numerical aperture of core / first cladding

[0074] =((refractive index of core) 2 -(refractive index of the first cladding) 2 ) 1 / 2 .

[0075] (4) Light transmission loss of plastic optical fiber

[0076] For the wound optical fiber obtained in each example and comparative example, a sample cut into a length of 5 m was used, and halogen parallel light (wavelength 650 nm, incident NA = 0.25) was incident from the end, and the light amount A (dBm) emitted from the other end was measured. Next, the 5 m sample was cut into a length of 2 m, and the same parallel light was incident from the end, and the light amount B (dBm) emitted from the other end was measured, and the light transmission loss C (dB / km) was calculated from (BA) / (5-2).

[0077] (5) Noise S / N ratio

[0078] The wound optical fiber obtained by each embodiment and comparative example was cut into a length of 2 m, and a laser (wavelength 650 nm, incident NA = 0.65) was irradiated from the end. The spot diameter at this time was adjusted to the fiber diameter. Light emitted from one end of an optical fiber was irradiated onto the screen of LaseView-LHB (manufactured by Kohike Co., Ltd.) from a position of 2.5 mm, and the light intensity distribution was measured. With respect to the maximum emission angle θm from the optical fiber NA to the optical fiber NA, the maximum light intensity (S) in the region of 0° to (0.9×θm) was determined. On the other hand, the maximum light intensity (N) in the region of 0.9×θm to 1.1×θm was determined.

[0079] Calculate S / N, if 1×10 3 The above are considered qualified.

[0080] (6) Materials used in Examples and Comparative Examples

[0081] Material A: acrylic polymer (PMMA) (trade name "GH-1000S", manufactured by クラミレ (KK)) The refractive index measured after injection molding was 1.49.

[0082] Material B: Cycloolefin polymer (trade name "K26R", manufactured by Nippon Zeon Co., Ltd.) The refractive index measured after injection molding was 1.54.

[0083] Material C: a copolymer of 74.5 wt% vinylidene fluoride / 25.5 wt% tetrafluoroethylene. The refractive index measured after injection molding was 1.40.

[0084] Material D: A copolymer of 18 wt% vinylidene fluoride / 62 wt% tetrafluoroethylene / 16 wt% hexafluoropropylene / 4 wt% perfluoropropyl vinyl ether. The refractive index measured after injection molding was 1.35.

[0085] (7) Dispersion of carbon black

[0086] Material E: Material A and carbon black were mixed in a ratio of 96:4 (mass ratio) using a twin-screw extruder melt-kneading device.

[0087] Material F: Material C and carbon black were mixed in a ratio of 96:4 (mass ratio) using a twin-screw extruder melt-kneading device.

[0088] Material G: Material C and material F are mixed in a ratio of 39:1 (mass ratio), and the carbon black content is 1000 ppm.

[0089] Material H: Material C and material F are mixed in a ratio of 19:1 (mass ratio), and the carbon black content is 2000 ppm.

[0090] Material I: Material C and material F are mixed in a ratio of 9:1 (mass ratio), and the carbon black content is 4000 ppm.

[0091] Material J: Material C and material F are mixed in a ratio of 1:1 (mass ratio), and the carbon black content is 20000 ppm.

[0092] Material K: Material A and material E are mixed in a ratio of 19:1 (mass ratio), and the carbon black content is 2000 ppm.

[0093] (8) Carbon black content

[0094] In this embodiment, the carbon black content is calculated based on the amount of raw material used. It should be noted that when the carbon black content contained in the cladding is measured using an optical fiber, it is carried out by the above method.

[0095] (9) Transmittance measurement

[0096] After processing each material containing carbon black into a 100μm film using a hot press, the transmittance t100 at 650nm is determined using a spectrophotometer UV3510 (manufactured by Hitachi, Ltd.). Based on the transmittance t100, the absorbance A100 at a film thickness of 100μm is determined by the formula A=-LOG10(t100). The absorbance A can be determined according to the Lambert-Beer law that is proportional to the optical path length. For example, the absorbance A10 at 10μm is determined by A10=A100 / 10 (when the thickness is nμm, it is An=A100 / (100 / n)). Based on the absorbance A10, the transmittance t10 at a film thickness of 10μm can be determined by t10=10 to the power of -A10. It should be noted that the above method can also be used to measure the transmittance of the cladding using an optical fiber.

[0097] [Example 1]

[0098] Material A as the core material and material H as the first cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 1 with a fiber diameter of 260μm (core diameter: 240μm, first cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material H using a hot press is 4.8%. Based on this transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 73.8%. The light transmission loss of the obtained plastic optical fiber is 250dB / km, which is good. The S / N ratio is 1.3×10 4 , is good.

[0099] [Example 2]

[0100] Material A as the core material and material I as the first cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 2 with a fiber diameter of 260μm (core diameter: 240μm, first cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material I using a hot press is 0.2%. Based on this transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 54.5%. The light transmission loss of the obtained plastic optical fiber is 450dB / km, which is good. The S / N ratio is 3.5×10 5 , is good.

[0101] [Example 3]

[0102] Material A as the core material, material H as the first cladding material, and material A as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 3 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material H using a hot press is 4.8%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 73.8%. The transmittance obtained by making a 100μm film of material A using a hot press is 99.3%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 99.9%. The light transmission loss of the obtained plastic optical fiber is 250dB / km, which is good. The S / N ratio is 7.5×10 3 , is good.

[0103] [Example 4]

[0104] Material A as the core material, material H as the first cladding material, and material K as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 4 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material H using a hot press is 4.8%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 73.8%. The transmittance obtained by making a 100μm film of material K using a hot press is 20.0%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 85.1%. The light transmission loss of the obtained plastic optical fiber is 250dB / km, which is good. The S / N ratio is 1.5×10 6 , which is good.

[0105] [Example 5]

[0106] Material B as the core material and material K as the first cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 5 with a fiber diameter of 260μm (core diameter: 240μm, first cladding thickness: 10μm) and a theoretical numerical aperture of 0.3. The transmittance obtained by making a 100μm film of material K using a hot press is 20.0%. Based on this transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 85.1%. The light transmission loss of the obtained plastic optical fiber is 650dB / km, which is good. The S / N ratio is 5.3×10 4 , is good.

[0107] [Example 6]

[0108] Material A as the core material, material G as the first cladding material, and material K as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 4 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material G using a hot press is 21.9%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 85.9%. The transmittance obtained by making a 100μm film of material K using a hot press is 20.0%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 85.1%. The light transmission loss of the obtained plastic optical fiber is optimal at 200dB / km. The S / N ratio is 2.5×10 6 , is good.

[0109] [Example 7]

[0110] Material A as the core material, material H as the first cladding material, and material K as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 4 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 5μm, second cladding thickness: 15μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material H using a hot press is 4.8%. Based on the transmittance, the transmittance when the first cladding thickness is 5μm is calculated to be 85.9%. The transmittance obtained by making a 100μm film of material K using a hot press is 20.0%. Based on the transmittance, the transmittance when the second cladding thickness is 15μm is calculated to be 78.6%. The light transmission loss of the obtained plastic optical fiber is 250dB / km, which is good. The S / N is 7.5×10 6 , for the best.

[0111] [Comparative Example 1]

[0112] Material A as the core material, material C as the first cladding material, and material D as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 6 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material C using a hot press is 98.0%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 99.8%. The transmittance obtained by making a 100μm film of material D using a hot press is 99.1%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 99.9%. The light transmission loss of the obtained plastic optical fiber is 200dB / km, which is good. The S / N ratio is 2.6×10 2 , which is NG.

[0113] [Comparative Example 2]

[0114] Material A as the core material, material C as the first cladding material, and material K as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 7 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. The transmittance obtained by making a 100μm film of material C using a hot press is 98.0%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 99.8%. The transmittance obtained by making a 100μm film of material K using a hot press is 20.0%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 85.1%. The light transmission loss of the obtained plastic optical fiber is 200dB / km, which is good. The S / N ratio is 8.2×10 2 , which is NG.

[0115] [Comparative Example 3]

[0116] Material B as the core material and material D as the first cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 8 with an optical fiber diameter of 260μm (core diameter: 240μm, first cladding thickness: 10μm) and a theoretical numerical aperture of 0.74. The transmittance obtained by making material D into a 100μm film using a hot press is 99.1%. Based on this transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 99.9%. The light transmission loss of the obtained plastic optical fiber is 650dB / km, which is good. The S / N ratio is 3.7×10 1 , which is NG.

[0117] [Comparative Example 4]

[0118] Material B as the core material, material A as the first cladding material, and material H as the second cladding material are supplied to a composite spinning machine, and core-sheath composite melt spinning is performed at a temperature of 250°C to obtain a plastic optical fiber 9 with a fiber diameter of 280μm (core diameter: 240μm, first cladding thickness: 10μm, second cladding thickness: 10μm) and a theoretical numerical aperture of 0.39. The transmittance obtained by making a 100μm film of material A using a hot press is 99.3%. Based on the transmittance, the transmittance when the first cladding thickness is 10μm is calculated to be 99.9%. The transmittance obtained by making a 100μm film of material H using a hot press is 4.8%. Based on the transmittance, the transmittance when the second cladding thickness is 10μm is calculated to be 73.8%. The light transmission loss of the obtained plastic optical fiber is 670dB / km, which is good. The S / N ratio is 5.4×10 2 , which is NG.

[0119] [Comparative Example 5]

[0120] Material A as the core material and material J as the first cladding material were supplied to a composite spinning machine, and core-sheath composite melt spinning was performed at a temperature of 250°C to obtain a plastic optical fiber 10 with a fiber diameter of 260μm (core diameter: 240μm, first cladding thickness: 10μm) and a theoretical numerical aperture of 0.5. Material J was made into a 100μm film using a hot press, and the transmittance was measured, which was the lower limit of the measurement. Therefore, theoretically, the transmittance of material H at 100μm is theoretically the same as the transmittance of material J at 10μm, so the transmittance of material H at 100μm is considered to be 4.8%, and the transmittance when the first cladding thickness is 10μm is considered to be 4.8%. The light transmission loss of the obtained plastic optical fiber is 3000dB / km, which is NG. No S / N ratio was detected.

[0121]

Claims

1. A plastic optical fiber, which is a plastic optical fiber consisting of a core and a cladding, wherein: A light-shielding agent is contained in the first cladding layer adjacent to the core, and the content of the light-shielding agent is in the range of 100 to 10000 ppm. 2 . The plastic optical fiber according to claim 1 , wherein the light-shielding agent contained in the first cladding is carbon black. 3 . The plastic optical fiber according to claim 1 , further comprising a second cladding layer outside the first cladding layer. The plastic optical fiber according to claim 3 , wherein the refractive index of the second cladding is greater than the refractive index of the first cladding.

5. The plastic optical fiber according to claim 3 or 4, wherein the second cladding contains a light-shielding agent, and the content of the light-shielding agent is in the range of 100 to 10000 ppm. 6 . The plastic optical fiber according to claim 5 , wherein a transmittance t1 of light with a wavelength of 650 nm at the first cladding film thickness and a transmittance t2 of light with a wavelength of 650 nm at the second cladding film thickness have a relationship of t1>t2. 7 . The plastic optical fiber according to claim 5 , wherein the light-shielding agent contained in the second cladding is carbon black.

8. The plastic optical fiber according to any one of claims 5 to 7, wherein the sunscreen contained in the first cladding and the sunscreen contained in the second cladding are made of the same material, and a sunscreen content D1 of the first cladding and a sunscreen content D2 of the second cladding are in a relationship of D1<D2. 9 . The plastic optical fiber according to claim 4 , wherein a film thickness T1 of the first cladding formed on the plastic optical fiber and a film thickness T2 of the second cladding formed on the plastic optical fiber have a relationship of T1<T2. 10 . The plastic optical fiber according to claim 1 , wherein the core is made of polymethyl methacrylate, and the numerical aperture NA of the core and the first cladding is 0.65 or less. 11 . A medical sensor comprising the plastic optical fiber according to claim 1 .