Manufacturing method and power semiconductor device

By generating a carbon-depleted layer through low-energy electron radiation and combining thermal annealing treatment, the carbon defect problem at the SiO2/n type 4H-SiC interface is solved, and the on-resistance and flat band voltage of power semiconductor devices is improved, avoiding the existing technology control difficulty and voltage offset.

CN118891735APending Publication Date: 2024-11-01HITACHI ENERGY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380028158.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-01-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The carbon defect concentration at the SiO2/n type 4H-SiC interface in existing power semiconductor devices is high, resulting in a high on-resistance. The existing improved methods such as post-oxidation annealing and pre-oxidation injection have difficulty in controlling and flat band voltage offset The problem.

Method used

Low-energy electron radiation is used to generate a carbon-depleted layer, which acts as a carbon absorber, reduces the carbon defect concentration at the SiO2/4H-SiC interface, and prevents carbon atoms from clustering during oxidation by thermal annealing, forming an improved electrically insulating layer.

Benefits of technology

Improved on-resistance and optimization of flat band voltage are achieved, the defect of impurities injection into oxides is avoided, the occurrence of normally open state is reduced, and the electronic characteristics of the device are improved by monitoring the concentration of carbon atoms in the depth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891735A_ABST
    Figure CN118891735A_ABST
Patent Text Reader

Abstract

In at least one embodiment, the method is used for manufacturing a power semiconductor device (1) and comprises the steps of:-providing a SiC-based semiconductor body (2),-irradiating at least one first portion (21) of a top side (20) of the semiconductor body (2) with low-energy electron radiation (E), and-generating an electrically insulating layer (3) at least in the irradiated at least one first portion (21).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A method for manufacturing a power semiconductor device is provided. Furthermore, a power semiconductor device is provided. Background Art

[0002] Documents US 2019 / 0296146 A1 and US 2002 / 0034852 A1 mention semiconductor devices having regions doped in different ways.

[0003] The problem to be solved is to provide a power semiconductor device with improved electrical performance. Summary of the Invention

[0004] This object is achieved in particular by a method for manufacturing a power semiconductor device as specified in the independent patent claim. Further exemplary embodiments are specified in the dependent patent claims.

[0005] For example, in the method described herein, low energy electron irradiation is used in order to improve the flat band voltage V FB and reducing carbon (C) defects at the oxide-SiC interface (eg, at the SiO2 / SiC interface).

[0006] In at least one embodiment, the method is for manufacturing a power semiconductor device and includes the following steps, for example in the order recited:

[0007] - providing a semiconductor body based on a carbon-containing semiconductor material (e.g. SiC),

[0008] - irradiating at least a first portion of the top side of the semiconductor body with low-energy electron radiation, and

[0009] - generating an electrically insulating layer at least in the at least one first portion that is irradiated. For example, the low-energy electron radiation has a kinetic energy of at least 116 keV and at most 210 keV, by means of which carbon atoms are moved from the top side into the semiconductor body, so that after irradiating the at least one first portion, the semiconductor body has Si 0.5+x C 0.5-x The electrically insulating layer is a layer wherein x is at least 0.001 and at most 0.1, the thickness of the aforementioned layer is at least 10 nm and at most 0.2 μm, and the electrically insulating layer is generated by thermal growth.

[0010] Despite the high bulk mobility of SiC, the inversion-channel mobilities μ in SiC metal oxide semiconductor field effect transistors (MOSFETs) are reported to be low, resulting in on-resistances much higher than expected from bulk SiC properties. This difference is attributed to the interface state density (D it ) is large, which is one to three orders of magnitude higher than that in the case of SiO2 / Si interface. it The nature of this phenomenon is often attributed to the presence of carbon-related defects and intrinsic oxide acceptor defects. The presence of carbon in the SiC epilayer is due to implantation during oxidation. The implanted carbon atoms form clusters that create acceptor levels close to the conduction band. These levels shorten the charge carrier lifetime and act as scattering centers, thereby reducing μ.

[0011] In order to improve the electronic properties of SiC MOSFET, the C defect concentration D at the SiO2 / n-type 4H-SiC interface should be reduced. it .

[0012] In the method described herein, pre-oxidation low-energy electron irradiation is used to achieve defect reduction at the SiO2 / n-type 4H-SiC interface.

[0013] For n-channel MOSFETs, different methods can reduce D it It is possible to perform oxidation annealing (POA) and pre-oxidation implantation (POI) in N2O or POCl3 environment or POI by N, P or Sb donor impurities, which leads to the formation of D in the upper part of SiC band gap. it Reduce (10 for POA 11 cm -2 eV -1 , for POI as low as 10 12 cm -2 eV -1 ) and μ increases (90 cm for POA 2 V -1 s -1 , 20cm for POI 2 V -1 s -1 Up to 100cm 2 V -1 s -1 ). Dit The reasons for the decrease and subsequent increase in μ have been explained in terms of passivation of C clusters by N or P atoms or in terms of counter-doping. Nevertheless, both POA and POI still have some disadvantages: it is difficult to control the concentration of N or P incorporated by POA, and a flat band voltage V may occur due to the introduction of N or P or Sb into SiO2. FB In addition, since P is more easily incorporated into SiC than N, a normally-on device can be obtained.

[0014] One idea of ​​the present method is, among other things, to use low-energy electron irradiation in order to create a C-poor layer, i.e. a layer rich in C voids (also called V C rich layer). This will act as a sink for C, leading to improved V FB and reduce the D at the SiO2 / 4H-SiC interface it .

[0015] To generate V C , using low energy electron irradiation, for example with energy between 116keV and 210keV. This is to generate C atom substitution (i.e., V C ) The minimum energy required. In this way, other defects (complex or Si-related) will hardly form, as would occur after impurity implantation or higher energy electron irradiation.

[0016] After irradiation, [V C ] increases, and by thermal annealing (at, for example, up to 500° C.), the carbon interstitial (C I ) atoms will diffuse deep into the bulk. Although C I Although mobile even at room temperature, heat treatment can prevent the C atoms displaced by irradiation from clustering during oxidation.

[0017] For the Al-implanted n-type 4H-SiC epitaxial layer, [V C ] is 6×10 15 cm -3 After dry oxidation at 1150℃ for 2h, [V C ] becomes 3×10 15 cm -3 , which means that approximately 3×10 15 cm -3 [C I ]. This means that before forming SiO2 with a thickness of, for example, 65 nm, the native n-type epitaxial layer should be irradiated with a certain electron dose so that, for example, [V C ] is at least 3×10 15 cm -3In this way, a C-poor layer is formed and during oxidation, very little C I will cluster to form D it .

[0018] By using the method described in this article, for example, the following benefits can be achieved:

[0019] 1. The electron irradiation dose can be changed to control [V C ] in order to capture the C atoms implanted during oxidation.

[0020] 2. Unlike POA or POI, impurities are not incorporated into the oxide.

[0021] 3. High annealing temperatures, such as about 1300° C., as used for POA are not required.

[0022] 4. Unlike N, P or Sb implants, no unwanted impurity-related complexes or other defects are generated.

[0023] 5. No implanted donor impurities (such as P) close to the surface prevent the normally-on state.

[0024] 6. By monitoring the [V C ] (by deep level transient spectroscopy DLTS or photoluminescence or by performing constant capacitance deep level transient spectroscopy CC-DLTS), it is possible to reverse engineer it into the final product.

[0025] 7. Improved on-resistance R can be achieved ON and lower D it .

[0026] In accordance with at least one embodiment, the electron kinetic energy of the low-energy electron radiation is at least 116 keV. Alternatively or additionally, this energy is at most 210 keV. This means, for example, that at least 90%, at least 99%, or at least 99.9% of the electrons of the low-energy electron radiation have the aforementioned kinetic energy. By having such energies, the C atoms of the SiC lattice can be specifically addressed by the radiation so as to move away from the top side.

[0027] According to at least one embodiment, the dose of the low-energy electron radiation in the first portion is at least 10 10 cm -2 or at least 10 12 cm -2 or at least 10 14 cm -2 Alternatively or additionally, it is possible that the aforementioned dosage is up to 10 17 cm -2 or up to 10 16 cm -2 or up to 1015 cm -2 .

[0028] According to at least one embodiment, the electrically insulating layer comprises oxygen. For example, the electrically insulating layer is an oxide layer, in particular a metal oxide or semiconductor oxide layer. The electrically insulating layer may be formed of a stoichiometric oxide.

[0029] According to at least one embodiment, the electrically insulating layer is formed of SiO2. Otherwise, the electrically insulating layer may be formed of Al2O3, NO x , Y2O3, ZrO2, HfO2, La2O3, Ta2O5 or TiO2.

[0030] According to at least one embodiment, the electrically insulating layer is grown by thermal growth. For example, the components of the electrically insulating layer, such as Si and O in the case of SiO2, are provided in the gas phase. For example, the temperature during the growth of the electrically insulating layer is at least 600°C, at least 800°C, or at least 1000°C. Alternatively or additionally, the temperature is at most 1500°C, at most 1300°C, or at most 1150°C.

[0031] According to at least one embodiment, the generating of the electrically insulating layer comprises annealing previously applied material of the electrically insulating layer. It is possible that all or most of the material of the electrically insulating layer has been applied on the top side of the semiconductor body before the annealing.

[0032] For example, the temperature during annealing of the electrically insulating layer is at least 200° C., or at least 300° C., or at least 400° C. Alternatively or additionally, the temperature is at most 1000° C., or at most 800° C., or at most 600° C. For example, the annealing requires at least 0.5 h, or at least 1 h, and / or the annealing requires at most 12 h, or at most 4 h. It is possible that the temperature during annealing is lower than the temperature during application of the material of the electrically insulating layer.

[0033] Optionally, during annealing and / or during thermal growth, at least one temperature ramp may be applied.

[0034] According to at least one embodiment, the annealing is performed in a nitrogen-containing atmosphere. For example, the annealing is performed in an N2 atmosphere (which may contain no or almost no oxygen), or even in air, or in one of N2O, NO, O2, or O3. The same applies to the thermal growth of the electrically insulating layer.

[0035] According to at least one embodiment, irradiating the at least one first portion is performed in a nitrogen-containing atmosphere, which may contain no or almost no oxygen, or the nitrogen-containing atmosphere may be air or one of N2O, NO, O2 or O3.

[0036] In accordance with at least one embodiment, the top side of the semiconductor body is a planar surface of the semiconductor body. Thus, the power semiconductor device may have a planar design.

[0037] According to at least one embodiment, the method further includes forming one or more trenches into the semiconductor body. For example, at least one trench is formed into the semiconductor body before irradiating the at least one first portion. The at least one trench can be generated by etching. Thus, the resulting power semiconductor device can have a trench design.

[0038] According to at least one embodiment, the at least one first portion comprises sidewalls and a bottom surface of the at least one trench. Possibly, the at least one first region is confined to the sidewalls and / or the bottom surface of the at least one trench.

[0039] According to at least one embodiment, the method includes applying a mask material to the top side before irradiating the at least one first portion. The mask material can be used to define the region of the top side to be irradiated or, for a given material, to adjust the penetration depth of the low-energy electron radiation into the semiconductor body by means of the mask material or by means of a certain thickness of the mask material.

[0040] According to at least one embodiment, during the irradiation of the at least one first portion, the at least one first portion is free of mask material, while the remainder of the top side is partially or completely covered by the mask material. If the penetration depth of the low-energy electron radiation into the semiconductor body is also to be adjusted by means of the mask material in the first portion, it is possible to partially provide the at least one first portion with a mask material, possibly with a reduced thickness compared to other areas of the top side. Even the entire at least one first portion can be covered with a thin layer of mask material.

[0041] It is possible to use not only one mask material but also a plurality of different mask materials.

[0042] According to at least one embodiment, carbon atoms are moved from the top side into the semiconductor body by means of low-energy electron irradiation in at least one first portion. That is, after irradiation of at least one first portion, the semiconductor body can be formed of non-stoichiometric SiC. That is, in this region, the semiconductor body has a thin layer of SiC. 0.5+x C 0.5-x , wherein x may be at least 0.001 or at least 0.01, and / or x is at most 0.1 or at most 0.02. The aforementioned layer may have a thickness of at least 10 nm or at least 100 nm. Alternatively or additionally, the aforementioned thickness is at most 1 μm or at most 0.2 μm.

[0043] Additionally provided is a power semiconductor device, which is manufactured, for example, by means of a method as indicated in conjunction with at least one of the embodiments set out above. Therefore, features of the power semiconductor device are also disclosed with respect to the method, and vice versa.

[0044] In at least one embodiment, a power semiconductor device includes: a semiconductor body based on SiC; and an electrically insulating layer applied in at least a first portion of a top side of the semiconductor body, wherein, adjacent to the electrically insulating layer, the semiconductor body is rich in silicon and therefore, for example, carbon-poor compared to stoichiometric SiC.

[0045] In accordance with at least one embodiment, the power semiconductor device is a metal insulator semiconductor field effect transistor (MISFET) or an insulated gate bipolar transistor (IGBT).

[0046] In accordance with at least one embodiment, the power semiconductor device is configured for an operating voltage of at least 0.6 kV or at least 1.2 kV. Alternatively or additionally, the power semiconductor device is configured for an operating voltage of at most 10 kV or at most 6 kV.

[0047] In accordance with at least one embodiment, the power semiconductor device is configured for an operating current of at least 10 A or at least 0.1 kA or at least 1 kA. Alternatively or additionally, the power semiconductor device is configured for an operating current of at most 20 kA or at most 5 kA.

[0048] According to at least one embodiment, the power semiconductor device is a device selected from the following group: metal oxide semiconductor field effect transistor (MOSFET), insulated gate bipolar transistor (IGBT), gate turn-off thyristor (GTO), gate commutated thyristor (GCT), junction gate field effect transistor (JFET).

[0049] Power semiconductor devices are, for example, configured to convert direct current (e.g., from a battery) into alternating current (e.g., for an electric motor). Power semiconductor devices can be used, for example, in vehicles (e.g., hybrid vehicles or plug-in electric vehicles) and also in railways (e.g., commuter trains). BRIEF DESCRIPTION OF THE DRAWINGS

[0050] The methods and power semiconductor devices described herein are explained in more detail below by way of exemplary embodiments with reference to the accompanying drawings. Identical elements in the various figures are denoted by the same reference numerals. However, the relationships between the elements are not shown to scale, and individual elements may be shown exaggerated to aid understanding.

[0051] Figures 1 to 3Schematic cross-sectional views showing method steps of an exemplary embodiment of a method described herein for producing a power semiconductor device,

[0052] Figures 4 and 5 Schematic cross-sectional views showing method steps of an exemplary embodiment of a method described herein for producing a power semiconductor device,

[0053] Figure 6 Schematic cross-sectional views showing method steps of an exemplary embodiment of a method described herein for producing a power semiconductor device,

[0054] Figure 7 A comparison of voltage and capacitance characteristics between an exemplary embodiment of a power semiconductor device described herein and a modified device is shown.

[0055] Figure 8 A comparison of temperature and CC-DLTS characteristics between an exemplary embodiment of a power semiconductor device described herein and a modified device is shown.

[0056] Figure 9 Figure 2 shows the V difference between the exemplary embodiment and the modified power semiconductor device described herein. GS with I GS Comparison of characteristics, and

[0057] Figure 10 Figure 2 shows the V difference between the exemplary embodiment and the modified power semiconductor device described herein. DS with I DS Comparison of characteristics. DETAILED DESCRIPTION

[0058] exist Figures 1 to 3 , an example of a method for manufacturing a power semiconductor device 1 is illustrated.

[0059] according to Figure 1 A semiconductor body 2 is provided. The semiconductor body 2 is based on SiC. For example, the semiconductor body 2 includes a substrate and at least one epitaxially grown semiconductor layer (not shown) thereon, both of which are based on SiC. The semiconductor body 2 has a planar top side 20.

[0060] For example, the semiconductor body 2 includes a well region 24, which may be formed of n-type 4H-SiC. Furthermore, two p-type regions may be present in the semiconductor body 2. If the semiconductor body 2 is to be configured as a MOSFET, these regions may be the source region 23 and the drain region 5.

[0061] according to Figure 2, a first portion 21 of the semiconductor body 2 is irradiated with low-energy electron radiation E. Like the top side 20 , the first portion 21 is planar. It is possible that the low-energy electron radiation E is confined to the first portion 21 , or that a larger portion of the top side 20 is exposed to the low-energy electron radiation E. For example, the first portion 21 extends completely between the doped regions 23 , 25 and, seen in a plan view of the top side 20 , may also partially include the doped regions 23 , 25 .

[0062] Despite Figure 2 In the context of FIG, only one first portion 21 is illustrated, but there may be a plurality of first portions 21. Likewise, there may be many more than two doped regions 24, 25.

[0063] For example, the electron kinetic energy of the low-energy electron radiation E is at least 116 keV and at most 210 keV. As an option, the dose of the low-energy electron radiation E in the first portion 21 is at least 10 12 cm -2 and at most 10 17 cm -2 .

[0064] For example, irradiation with radiation E is carried out in an air or nitrogen atmosphere. Figure 2 Vacuum may not be required during the steps.

[0065] exist Figure 3 In a method step, in a first part 21, an electrically insulating layer 3 is applied to the top side 20 of the semiconductor body 2. The electrically insulating layer 3 is grown, for example, as a thermal oxide, at a high temperature of, for example, at least 1000° C. Optionally, after the material of the electrically insulating layer 3 is applied, an annealing can be performed, for example, in an atmosphere of N2O, NO, O2, or O3.

[0066] For example, the electrically insulating layer 3 is formed of SiO 2 .

[0067] By means of low-energy electron radiation E, carbon atoms are removed from the region immediately adjacent to the top side 20 in the first portion 21, so that silicon-rich SiC is present in the first portion. Thus, the electrical properties can be improved because the proper formation of an oxide layer that would hinder the electrically insulating layer 3 due to C clusters is suppressed.

[0068] Further, in Figure 3 : A gate electrode 4 is formed on the side of the electrically insulating layer 3 facing away from the semiconductor body 3. The gate electrode 4 can be formed from a metal or an ohmically conductive semiconductor material, such as polysilicon. Depending on the material of the gate electrode 4, an annealing step can be performed after the material of the gate electrode 4 is applied, so that a combined annealing can occur.

[0069] The finished power semiconductor device 1 is, for example, a power MOSFET or an IGBT. In the case of an IGBT, there is no drain region, but a collector region and a drift region may be present. Electrodes other than the gate electrode 4 (e.g., source electrode, drain electrode, or collector electrode) are not shown in the figure.

[0070] For example, the finished power semiconductor device 1 is configured for a current of at least 10 A and / or at most 10 kA. Alternatively or additionally, the power semiconductor device 1 is configured for a voltage of at least 0.6 kV and / or at most 6 kV.

[0071] exist Figure 4 and Figure 5 Another example of the manufacturing method is shown in FIG. Figure 4 , a semiconductor body 4 is provided, and a trench 5 is formed in the semiconductor body 2 .

[0072] In this case, the finished power semiconductor device 1 will be configured as an IGBT. Therefore, the semiconductor body 5 includes a source region 23 at the top side 20. Optionally, the source region 23 is divided into two sub-regions by the trench 5. The source region 23 is embedded in a well region 24. On the side of the well region 24 facing away from the top side 20, there is a drift region 26. On the side of the drift region 26 facing away from the drift region 26, there is a collector region 25. Again, to simplify the drawing, the electrodes of the respective semiconductor regions 23, 24, and 25 are not shown.

[0073] For example, the trench 5 extends from the top side 20 into the drift region 26 and terminates within the drift region 26. Except as shown, the trench 5 need not have a planar bottom surface, but may have a rounded bottom surface or even a V-shaped bottom region as seen in a cross section perpendicular to the top side 20.

[0074] In addition, according to Figure 4 At least the sidewalls and bottom of the trench 5 are irradiated with low-energy electron radiation E. That is, the first portion 21 may consist of the aforementioned sidewalls and bottom. Other portions of the top side 20 outside the trench 5 may also be irradiated with low-energy electron radiation E.

[0075] and Figure 4 In contrast to the situation shown in , a plurality of grooves 5 may be present.

[0076] according to Figure 5 After irradiating the first portion 21 with radiation E, an electrically insulating layer 3 is applied to the side walls and the bottom of the trench 5. Figure 5 In the embodiment shown, the electrically insulating layer 5 has a constant thickness all along the trench sidewalls and bottom; however, it is also possible that the electrically insulating layer 3 has a varying thickness.

[0077] Then, the remaining portion of the trench 5 is filled with the gate electrode 4 .

[0078] Other aspects, about Figures 1 to 3 The situation can be applied to Figure 4 and Figure 5 , and vice versa.

[0079] exist Figure 6 , another method for manufacturing a power semiconductor device 1 is illustrated. In this case, a mask material 6 is applied to the top side 20 outside the first portion 21. Therefore, a second portion 22 outside the first portion 21 may not be irradiated by the low-energy electron radiation E. Therefore, the first portion 21 can be accurately defined by the mask material 6. For example, the thickness of the mask material 6 can reach at least 10 μm or at least 30 μm.

[0080] Other aspects, about Figures 1 to 5 The content is applicable to Figure 6 , and vice versa.

[0081] Figure 7 A comparison of measured voltage U versus capacitance C characteristics is shown between an exemplary embodiment of a power semiconductor device 1 described herein and a modified device 9. Modified device 9 corresponds to power semiconductor device 1, except for the irradiation with low-energy electron radiation E. Both devices 1, 9 are MOS capacitors.

[0082] Theoretical flat band voltage V FB is obtained by the difference between the gate metal work function and the semiconductor work function: V FB =MS. This results in V FB The value of is 0.14eV. From the measured UC characteristics, the V FB is 0.38eV and the V FB is 1.80eV.

[0083] Figure 8 The figure shows the comparison of the measured temperature T versus constant capacitance deep level transient spectroscopy CC-DLTS signal S characteristics between MOS device 1 and reference device 9. It can be seen that the CC-DLTS signal of pre-irradiated device 1 is lower than that of reference device 9, which suggests that D it This occurs in the low temperature side of the CC-DLTS spectrum, i.e., close to the conduction band edge.

[0084] To demonstrate the effect of electron irradiation, TCAD simulations were performed on a SiC MOSFET before oxidation. First, a typical concentration of interface traps of about 10 12 eV -1 cm-2 After that, the SiC MOSFET in the presence of traps (these traps exist after oxidation) is considered, resulting in D it Reduced by an order of magnitude.

[0085] energy level Energy position (eV) <![CDATA[Capture cross section (cm 2 )]]> <![CDATA[Concentration (cm -3 )]]> OF1 <![CDATA[E C -0.19]]> <![CDATA[3×10 -17 ]]> <![CDATA[3×10 11 ]]> OF2 <![CDATA[E C -0.24]]> <![CDATA[10 -18 ]]> <![CDATA[3×10 11 ]]> ON1 <![CDATA[E C -0.79]]> <![CDATA[10 -15 ]]> <![CDATA[2×10 12 ]]> ON2 <![CDATA[E C -1.0]]> <![CDATA[10 -16 ]]> <![CDATA[4×10 12 ]]>

[0086] ON1, ON2, OF1, and OF2 can be considered merely labels. Each electrically active energy level lies within the band gap. For example, OF1 is found 0.19 eV below the conduction band edge. These electrically active energy levels create a potential well into which electrons fall. This well has a cross-section. The larger the cross-section, the easier it is to trap electrons. Furthermore, each electrically active energy level is associated with a defect, which in turn has a specified concentration.

[0087] Figure 9 shows the V between the exemplary embodiment of the power semiconductor device 1 described herein and the modified device 9. GS with I GS Comparison of characteristics, and Figure 10 shows the V between the exemplary embodiment of the power semiconductor device 1 described herein and the modified device 9. DS with I DS Therefore, Figure 9 The transfer characteristics of the reference device 9 and the pre-oxidation-irradiated MOSFET 1 described herein are mentioned and Figure 10 Their output characteristics are mentioned. Figure 9 In the middle, for those with standard or lower D it Simulations performed on horizontal MOSFETs have shown that the transfer characteristics are improved if the irradiation is performed before applying the electrically insulating layer. Figure 10 The output characteristics of the same MOSFET are shown. It can be seen that the curve for the illuminated MOSFET 1 shows an improvement over the reference curve 9, which means that the on-resistance R ON Reduced.

[0088] Unless otherwise indicated, the components shown in the drawings are illustratively arranged one directly on top of the other in the order specified. Components that are not in contact in the drawings are illustratively spaced apart from each other. If lines are drawn parallel to each other, the corresponding surfaces can be oriented parallel to each other. Likewise, unless otherwise indicated, the positions of the drawn components relative to each other are accurately reproduced in the drawings.

[0089] The power semiconductor devices and methods described herein are not limited to the description based on the exemplary embodiments. Instead, the power semiconductor devices and methods include any novel features and any combination of features, in particular including any combination of features in the patent claims, even if the feature or combination itself is not explicitly stated in the patent claims or exemplary embodiments.

[0090] European Patent Application 22162144.4 from which this patent application claims priority, the disclosure content of which is incorporated herein by reference.

[0091] Reference Symbols

[0092] 1 Power semiconductor devices

[0093] 2 Semiconductor body

[0094] 20 Top side

[0095] 21 Part 1

[0096] 22 Part 2

[0097] 23 Source region

[0098] 24-well region

[0099] 25 Drain region

[0100] 26 Drift Zone

[0101] 3 Electrical insulation layer

[0102] 4 Gate electrode

[0103] 5 grooves

[0104] 6 Mask materials

[0105] 9 Modified devices

[0106] C capacitance (in pF)

[0107] I DS The current density between the drain and source (in A / cm 2 (unit)

[0108] I GS The current density between the gate and the source (in A / cm 2 (unit)

[0109] S CC-DLTS signal (in mV)

[0110] T temperature (in K)

[0111] U voltage (in V)

[0112] VDS The voltage between the drain and source (in V)

[0113] V GS The voltage between the gate and the source (in V)

Claims

1. A method for manufacturing a power semiconductor device (1), the method comprising the following steps: - providing a semiconductor body (2) based on SiC, - irradiating at least one first portion (21) of the top side (20) of the semiconductor body (2) with low-energy electron radiation (E), the low-energy electron radiation having a kinetic energy of at least 116 keV and at most 210 keV, by means of the low-energy electron radiation (E) in the at least one first portion (21) carbon atoms are moved from the top side (20) into the semiconductor body (2), so that after irradiating the at least one first portion, the semiconductor body has Si 0.5+x C 0.5-x A layer, wherein x is at least 0.001 and at most 0.1, the thickness of the layer is at least 10 nm and at most 0.2 μm, and - generating an electrically insulating layer (3) by thermal growth at least in the at least one first irradiated portion (21).

2. The method according to the preceding claim, in, x is at most 0.

02.

3. The method according to any one of the preceding claims, in, The dose of the low energy electron radiation (E) in the first part (21) is at least 10 12 cm -2 And at most 10 17 cm -2 .

4. The method according to any one of the preceding claims, in, The electrically insulating layer (3) comprises oxygen.

5. The method according to the preceding claim, in, The electrical insulating layer (3) is formed of SiO2.

6. The method according to the preceding claim, in, By forming the electrical insulating layer (3), a SiO2 / n-type 4H-SiC interface is formed.

7. The method according to any one of the preceding claims, in, Generating the electrically insulating layer (3) comprises annealing the previously applied material of the electrically insulating layer (3).

8. The method according to the preceding claim, in, The annealing is performed in an atmosphere containing at least one of nitrogen and oxygen.

9. The method according to any one of the preceding claims, in, Irradiating the at least one first portion (21) is performed in a nitrogen-containing atmosphere.

10. The method according to any one of the preceding claims, in, The top side (20) is a planar surface of the semiconductor body (2).

11. The method according to any one of claims 1 to 9, The method further comprises, before irradiating the at least one first portion (21), forming at least one trench (5) into the semiconductor body (2), in, The at least one first portion (21) includes the side walls and the bottom surface of the at least one groove (5).

12. The method according to any one of the preceding claims, in, Before irradiating the at least one first portion (21), a mask material (6) is applied to the top side (20), and during irradiating the at least one first portion (21), the at least one first portion (21) is free of the mask material (6), while the rest of the top side (20) is covered by the mask material (6).

13. The method according to any one of the preceding claims, in, A gate electrode (4) is formed directly on a side of the electrical insulation layer (3) remote from the semiconductor body (2), wherein the gate electrode (4) is formed of polysilicon. In which, viewed in a cross section perpendicular to the top side (20), the electrical insulating layer (3) and the gate electrode (4) extend as a hole-free closed layer from the source region (23) across the well region (24) to the drain region (25).

14. A power semiconductor device (1), comprising: - a semiconductor body (2) based on SiC, and - a thermally grown electrically insulating layer (3) which is applied in at least one first portion (21) of the top side (20) of the semiconductor body (2), wherein, adjacent to the electrically insulating layer (3), the semiconductor body (2) is rich in silicon, Wherein, adjacent to the electrical insulating layer (3), the semiconductor body has Si 0.5+x C 0.5-x layer, and x is at least 0.001 and at most 0.1, and the thickness of the layer is at least 10 nm and at most 0.2 μm.

15. The power semiconductor device (1) according to the preceding claim, The power semiconductor device (1) is a metal insulator semiconductor field effect transistor or an insulated gate bipolar transistor, and in, The power semiconductor device (1) is configured for an operating voltage of at least 0.6 kV.

Citation Information

Patent Citations

  • SiC MOSFET threshold voltage recovery method and device under electron irradiation

    CN114005742A

  • Silicon carbide semiconductor device and method of manufacturing silicon carbide semiconductor device

    US20170141206A1

  • Silicon carbide semiconductor device and method of manufacturing silicon carbide semiconductor device

    US20180308937A1