Electrochemical device and electronic device
Patent Information
- Application Number
- CN202280093206.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-28
AI Technical Summary
The reaction between lithium manganate and the electrolyte causes manganese to dissolve, destroying the SEI film of the negative electrode, causing safety hazards, and affecting the low-temperature performance and cycle life of the electrochemical device.
Add lithium iron phosphate to the cathode material, control its mass percentage, particle size and specific surface area to form a core-shell structure or coating layer to inhibit manganese dissolution, and improve the quality through a reasonable combination of lithium nickel cobalt manganate and other elements. Conductivity.
It effectively inhibits manganese dissolution, improves the safety and low-temperature performance of electrochemical devices, avoids drying and cracking of pole pieces, extends cycle life, and reduces costs.
Abstract
Description
Electrochemical devices and electronic devices Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art
[0002] Electrochemical devices, such as lithium-ion batteries, are widely used in various fields due to their high energy density, high power, and long cycle life. To reduce the cost of electrochemical devices, lithium manganese oxide (LiMnO) is often used as the positive electrode material. However, LiMnO may react with hydrofluoric acid in the electrolyte, causing manganese to dissolve and subsequently deposit at the negative electrode. This can ultimately damage the solid electrolyte interphase (SEI) at the positive electrode, leading to lithium deposition during the charge and discharge process and posing a safety hazard.
[0003] Summary of the Invention
[0004] In some embodiments of the present application, an electrochemical device is provided, comprising: a positive electrode, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer located on one side or both sides of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode material, the positive electrode material comprising lithium manganate and lithium iron phosphate; based on the total mass of the positive electrode material, the mass percentage a of the lithium iron phosphate satisfies: 5wt%≤a≤20wt%, the Dv50 of the lithium iron phosphate is 0.8μm to 2.0μm, the Dn10 of the lithium iron phosphate is 0.2μm to 0.5μm, and the specific surface area of the lithium iron phosphate is not less than 5m 2 The present invention improves safety by suppressing manganese dissolution through lithium iron phosphate and solves the problems of lithium iron phosphate floating and electrode drying and cracking by rationally controlling the mass content, particle size and specific surface area of lithium iron phosphate.
[0005] In some embodiments of the present application, in some embodiments, the mass percentage of lithium iron phosphate satisfies 10wt%≤a≤20wt%, in some embodiments, the Dv50 of lithium iron phosphate is 1.1μm to 1.8μm, in some embodiments, the Dn10 of lithium iron phosphate is 0.2μm to 0.4μm, and in some embodiments, the specific surface area of lithium iron phosphate is greater than 8m 2 / g.
[0006] In some embodiments of the present application, the specific surface area of lithium manganate is 0.2 m 2 / g to 0.7m 2 / g. In some embodiments, lithium iron phosphate adheres to the surface of lithium manganate. The specific surface area of lithium manganate affects the buoyancy and sinking force of lithium iron phosphate. When the specific surface area of lithium manganate is too small, lithium manganate and lithium iron phosphate tend to sink in the slurry. When the specific surface area of lithium manganate is too large, lithium manganate and lithium iron phosphate tend to float in the slurry. When the specific surface area of lithium manganate is within the above range, the buoyancy and sinking force reach equilibrium, avoiding the problem of uneven distribution caused by slurry deposition and the problem of slurry floating.
[0007] In some embodiments of the present application, the positive electrode material further includes: lithium nickel cobalt manganate. Based on the total mass of the positive electrode material, the mass percentage content b of lithium nickel cobalt manganate satisfies: 0 wt% < b ≤ 10 wt%. In some embodiments, lithium nickel cobalt manganate can form a coating on lithium manganate, reducing the reactivity of the electrolyte with lithium manganate. At the same time, controlling the lithium nickel cobalt manganate within the above mass range can reduce costs while ensuring the effect.
[0008] In some embodiments of the present application, at least part of the positive electrode material has a core-shell structure, with lithium manganate located in the core of the core-shell structure and lithium iron phosphate and lithium nickel cobalt manganate located in the shell layer of the core-shell structure, thereby preventing the dissolution of manganese. In some embodiments of the present application, at least part of the positive electrode material has a core-shell structure, with lithium manganate located in the core of the core-shell structure and lithium iron phosphate located in the shell layer of the core-shell structure. In some embodiments, lithium iron phosphate forms a coating on lithium manganate, reducing the reactive sites of the electrolyte and lithium manganate, thereby preventing the dissolution of manganese.
[0009] In some embodiments of the present application, the positive electrode material contains at least one of B, Mg, Al, Si, S, Ti, Cr, Cu, Zn, Ga, Ge, Y, Zr, Mo, Ag, Ba, W, In, Sn, Pb or Sb, thereby improving the conductivity.
[0010] In some embodiments of the present application, the positive electrode active material layer includes a first layer and a second layer. The first layer is located between the positive electrode current collector and the second layer. The difference in the mass percentage content of iron element between the first layer and the second layer is not greater than 0.5%, which indicates that lithium iron phosphate is evenly distributed in the positive electrode active material layer in the present application, without the problems of sinking and floating. In some embodiments of the present application, the difference in thickness between the first layer and the second layer is not greater than 20%. In some embodiments of the present application, the first layer includes lithium manganate and lithium iron phosphate, and the second layer includes lithium manganate and lithium iron phosphate; or the first layer includes lithium manganate, lithium iron phosphate or lithium nickel cobalt manganate, and the second layer includes lithium manganate, lithium iron phosphate and lithium nickel cobalt manganate.
[0011] In some embodiments of the present application, based on the total mass of the positive electrode material, the mass percentage of lithium manganese oxide in the second layer is d; based on the total mass of the positive electrode material, the mass percentage of lithium manganese oxide in the first layer is e; wherein d<e.
[0012] In some embodiments of the present application, the positive electrode active material layer further comprises a binder and a conductive agent. In some embodiments of the present application, an electronic device is further provided, comprising any of the above electrochemical devices.
[0013] The present application also proposes an electronic device, comprising any electrochemical device proposed in the present application. The positive electrode of the present application comprises a positive electrode current collector and a positive electrode active material layer located on one side or both sides of the positive electrode current collector, the positive electrode active material layer comprises a positive electrode material, and the positive electrode material comprises lithium manganate and lithium iron phosphate; based on the total mass of the positive electrode material, the mass percentage a of the lithium iron phosphate satisfies: 5wt%≤a≤20wt%, the Dv50 of the lithium iron phosphate is 0.8μm to 2.0μm, the Dn10 of the lithium iron phosphate is 0.2μm to 0.5μm, and the specific surface area of the lithium iron phosphate is not less than 5m 2 While improving the safety of the electrochemical device, the present application solves the problems of lithium iron phosphate floating and electrode drying and cracking by rationally controlling the mass content, particle size and specific surface area of lithium iron phosphate. DETAILED DESCRIPTION
[0014] The following examples may enable those skilled in the art to more fully understand the present application, but are not intended to limit the present application in any way.
[0015] In this application, two objects are "equal" or "identical" when they differ by less than 30%, 20%, 10%, or 5%. The difference is calculated by subtracting the smaller object from the larger object, dividing the difference by the smaller object, and then multiplying the difference by 100%.
[0016] Electrochemical devices, such as lithium-ion batteries, are widely used in various fields. To reduce the cost of electrochemical devices, lithium manganese oxide is used as the positive electrode material in the positive electrode. The spinel structure of lithium manganese oxide has the characteristics of low temperature resistance, good rate performance, and easy preparation. However, the lithium manganese oxide material itself is unstable. Lithium manganese oxide easily reacts with hydrofluoric acid in the electrolyte, causing manganese dissolution, which in turn leads to the destruction of the negative electrode SEI film and lithium precipitation, posing a safety hazard. Lithium manganese oxide also has poor high-temperature performance and cycle performance, all of which are caused by the characteristics of manganese.
[0017] In some embodiments of the present application, an electrochemical device is proposed, which can be a lithium-ion battery. The electrochemical device includes: a positive electrode, and can also include a negative electrode and a separator. The positive electrode includes a positive electrode collector and a positive electrode active material layer located on one side or both sides of the positive electrode collector. The positive electrode collector can be made of copper foil or aluminum foil. The positive electrode active material layer includes a positive electrode material, and the positive electrode material includes lithium manganate and lithium iron phosphate. Based on the total mass of the positive electrode material, the mass percentage a of the lithium iron phosphate satisfies: 5wt%≤a≤20wt%, the Dv50 of the lithium iron phosphate is 0.8μm to 2.0μm, and the Dn10 of the lithium iron phosphate is 0.2μm to 0.5μm. Dn10 is the particle size corresponding to when the cumulative number distribution percentage reaches 10%, that is, the particle size of 10% of the particles is not greater than this particle size, and the specific surface area of the lithium iron phosphate is not less than 5m 2 / g.
[0018] In the present application, lithium iron phosphate and lithium manganate are used simultaneously in the positive electrode material. Lithium iron phosphate can effectively absorb hydrofluoric acid and form a coating on lithium manganate, reducing the reaction active points between the electrolyte and lithium manganate, thereby effectively inhibiting manganese dissolution. However, because the particle size of lithium iron phosphate is nanometer-scale, it is easy to float during the preparation of the slurry, and causes the positive electrode active material layer to crack during the positive electrode drying process. In order to solve the problem of lithium iron phosphate floating and cracking, the present application controls the mass percentage content, Dv50, Dn10 and specific surface area of lithium iron phosphate. When the above characteristics of lithium iron phosphate meet the range limited by this application, it can inhibit lithium iron phosphate from floating and prevent cracking. When it cannot be fully satisfied, the problem of lithium iron phosphate floating or cracking of the positive electrode active material layer will occur, which will lead to poor performance of the electrochemical device. The electrochemical device proposed in the embodiment of the present application adopts the above-mentioned positive electrode material, which effectively solves the problems of electrode cracking and lithium iron phosphate floating while reducing the cost of the positive electrode material and preventing manganese dissolution.
[0019] In the embodiments of the present application, the mass percentage of lithium iron phosphate in the positive electrode material is not less than 5wt%, thereby ensuring sufficient lithium iron phosphate to inhibit manganese dissolution. When the mass percentage of lithium iron phosphate in the positive electrode material does not exceed 20wt%, the electrochemical device has better low-temperature performance. When the mass percentage of lithium iron phosphate exceeds 20%, the low-temperature performance of the electrochemical device will be significantly deteriorated. In some embodiments of the present application, the electrochemical device is charged from 0% SOC (state of charge) to 3.65V at a current of 2A at a room temperature of 20°C to 25°C to obtain a charging capacity C1. After standing for 2h in an environment of -20°C, it is discharged to 2.5V at a rate of 0.5C to obtain a discharge capacity C2. The ratio of the discharge capacity C2 of the electrochemical device to C1 is greater than 75%, which indicates that the electrochemical device in the present application has good low-temperature performance.
[0020] In some embodiments of the present application, in some embodiments, the mass percentage of lithium iron phosphate satisfies 10wt%≤a≤20wt%. In some embodiments, if the mass percentage of lithium iron phosphate is too low, it may not be able to absorb hydrofluoric acid well. The mass percentage of lithium iron phosphate is controlled to be no less than 10% to ensure the protection of lithium manganese oxide.
[0021] The mass content of the compound (e.g., lithium iron phosphate, lithium manganate, or lithium nickel cobalt manganate) in the active material layer can be measured by X-ray photoelectron spectroscopy. X-ray diffraction can also be used to test the content of characteristic elements and deduce the active material content. The specific testing principles and test details belong to the existing technology in this field and will not be repeated in this application.
[0022] In some embodiments, the Dv50 of lithium iron phosphate is 1.1 μm to 1.8 μm, in some embodiments, the Dn10 of lithium iron phosphate is 0.2 μm to 0.4 μm, and in some embodiments, the Dv50 and Dn10 of lithium iron phosphate characterize the particle size of lithium iron phosphate. If the particle size of lithium iron phosphate is too small, the electrolyte will be consumed more quickly. If the particle size is too large, it is not conducive to the rate performance and cannot protect the lithium manganese oxide well. In some embodiments, the specific surface area of lithium iron phosphate is greater than 8 m 2 / g, In some embodiments, the specific surface area of lithium iron phosphate affects its contact area with the electrolyte on the one hand, and its contact area with lithium manganate on the other hand. Therefore, the specific surface area of lithium iron phosphate cannot be too small, otherwise it will not cover the lithium manganate well and will not absorb hydrofluoric acid well. In some embodiments, the specific surface area of lithium iron phosphate is greater than 8m 2 / g is less than 17m 2 In some embodiments, the specific surface area of lithium iron phosphate is greater than 8m 2 / g is less than 15m 2 / g.
[0023] In some embodiments of the present application, the specific surface area of lithium manganate is 0.2 m 2 / g to 0.7m 2 / g. In some embodiments, lithium iron phosphate adheres to the surface of lithium manganate. The specific surface area of lithium manganate affects the buoyancy and sinking force of lithium iron phosphate. When the specific surface area of lithium manganate is too small, lithium manganate and lithium iron phosphate tend to sink in the slurry. When the specific surface area of lithium manganate is too large, lithium manganate and lithium iron phosphate tend to float in the slurry. When the specific surface area of lithium manganate is within the above range, the buoyancy and sinking forces are basically balanced, avoiding the problem of uneven distribution caused by slurry sedimentation and the floating of the slurry.
[0024] In some embodiments of the present application, the specific surface area of the particles can be measured using a specific surface area tester. The specific test details are not repeated here.
[0025] In some embodiments of the present application, the positive electrode material further includes: lithium nickel cobalt manganese oxide. Based on the total mass of the positive electrode material, the mass percentage b of lithium nickel cobalt manganese oxide satisfies: 0 wt% < b ≤ 10 wt%. In some embodiments, lithium nickel cobalt manganese oxide can form a coating on lithium manganate, reducing the reactivity of the electrolyte with lithium manganate. At the same time, controlling lithium nickel cobalt manganese oxide within the above mass range can reduce costs while ensuring the effect. In some embodiments of the present application, 1 wt% < b ≤ 10 wt%.
[0026] In some embodiments of the present application, the positive electrode material contains at least one of B, Mg, Al, Si, S, Ti, Cr, Cu, Zn, Ga, Ge, Y, Zr, Mo, Ag, Ba, W, In, Sn, Pb, or Sb. In some embodiments, the impurity atoms in the positive electrode material form carriers, thereby improving the conductivity of the positive electrode material, which is beneficial to improving the rate performance and cycling performance of the electrochemical device.
[0027] In some embodiments, the positive electrode active material layer includes a first layer and a second layer. The first layer is located between the positive electrode current collector and the second layer, and the thicknesses of the first layer and the second layer can be the same or different. The types of active materials included in the first layer and the second layer can be the same or different.
[0028] In some embodiments, the types of active materials included in the first layer and the second layer are the same. For example, the first layer includes lithium manganate and lithium iron phosphate, and the second layer includes lithium manganate and lithium iron phosphate. Or the first layer includes lithium manganate, lithium iron phosphate, or lithium nickel cobalt manganese oxide, and the second layer includes lithium manganate, lithium iron phosphate, and lithium nickel cobalt manganese oxide.
[0029] In some embodiments of the present application, the first layer is located between the positive electrode current collector and the second layer, and the difference between the mass percentage of iron element in the first layer and the mass percentage of iron element in the second layer is not greater than 0.5%. In some embodiments, the thicknesses of the first layer and the second layer can be the same. For a target area on the positive electrode current collector, the difference between the mass percentage of iron element in the first layer and the mass percentage of iron element in the second layer in the target area is not greater than 0.5%. In some embodiments, for the positive electrode active material layer on either side of the positive electrode current collector, when it is divided into the first layer and the second layer along the thickness direction, for any target area, it is detected that the mass percentage of iron element in the first layer in the target area and the mass percentage of iron element in the second layer in the target area are almost the same, which indicates that lithium iron phosphate is uniformly distributed in the positive electrode active material layer and there is no problem of lithium iron phosphate floating up. In some embodiments, the difference degree of the thicknesses of the first layer and the second layer is not greater than 20%.
[0030] In some embodiments, the first layer and the second layer contain different types of active materials. Based on the total mass of the positive electrode material, the mass percentage of lithium manganese oxide in the second layer is d. Based on the total mass of the positive electrode material, the mass percentage of lithium manganese oxide in the first layer is e. Where d < e. This arrangement allows the first layer, closer to the current collector, to contain more lithium manganese oxide than the second layer, further from the current collector. This also results in a lower hydrofluoric acid concentration in the first layer, which helps reduce manganese dissolution from the positive electrode active material layer.
[0031] In some embodiments of the present application, at least part of the positive electrode material is a core-shell structure, lithium manganese oxide is located in the core of the core-shell structure, and lithium iron phosphate is located in the shell of the core-shell structure. In some embodiments, lithium iron phosphate forms a coating on the lithium manganese oxide, reducing the reactive sites between the electrolyte and lithium manganese oxide, thereby preventing manganese dissolution and reducing the corrosion of the electrolyte on the lithium manganese oxide. In some embodiments of the present application, at least part of the positive electrode material is a core-shell structure, lithium manganese oxide is located in the core of the core-shell structure, and lithium iron phosphate and lithium nickel cobalt manganese oxide are located in the shell of the core-shell structure, thereby further preventing manganese dissolution.
[0032] In some embodiments of the present application, the positive electrode active material layer further includes a binder and a conductive agent. The binder may be polyvinylidene fluoride, and the conductive agent may be one or more of conductive carbon black, carbon nanotubes, and graphite.
[0033] In some embodiments, the electrochemical device comprises a separator disposed between the positive and negative electrodes. In some embodiments, the separator comprises at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, or aramid. For example, the polyethylene comprises at least one selected from high-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene. Polyethylene and polypropylene are particularly effective in preventing short circuits and can improve battery stability through a shutdown effect. In some embodiments, the separator has a thickness ranging from approximately 5 μm to 50 μm.
[0034] In some embodiments, the surface of the isolation membrane may further include a porous layer, disposed on at least one surface of the isolation membrane. The porous layer includes inorganic particles and a binder, wherein the inorganic particles are selected from at least one of aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. In some embodiments, the pores of the isolation membrane have a diameter ranging from approximately 0.01 μm to 1 μm. The binder of the porous layer is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene. The porous layer on the surface of the separator can improve the separator's heat resistance, oxidation resistance, and electrolyte wettability, and enhance the adhesion between the separator and the electrode.
[0035] In some embodiments of the present application, the electrochemical device may be wound or stacked. In some embodiments, the positive electrode and / or negative electrode of the electrochemical device may be a multi-layer structure formed by winding or stacking, or a single-layer structure consisting of a single-layer positive electrode, a separator, and a single-layer negative electrode.
[0036] In some embodiments, the electrochemical device includes a lithium-ion battery, but the present application is not limited thereto. In some embodiments, the electrochemical device may further include an electrolyte. The electrolyte may be one or more of a gel electrolyte, a solid electrolyte, and an electrolyte, the electrolyte including a lithium salt and a non-aqueous solvent. The lithium salt is selected from one or more of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, or lithium difluoroborate. For example, the lithium salt is selected from LiPF6 because it has high ionic conductivity and can improve cycle characteristics.
[0037] The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents or a combination thereof. The carbonate compound may be a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.
[0038] Examples of chain carbonate compounds are diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methylethyl carbonate (MEC), and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate (VEC), or combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, or combinations thereof.
[0039] Examples of the carboxylic acid ester compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.
[0040] Examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.
[0041] Examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphoric acid esters or combinations thereof.
[0042] In some embodiments of the present application, using a lithium-ion battery as an example, a positive electrode, a separator, and a negative electrode are sequentially wound or stacked to form an electrode component, which is then encapsulated in, for example, an aluminum-plastic film. An electrolyte is then injected, followed by formation and packaging to produce a lithium-ion battery. The prepared lithium-ion battery is then subjected to performance testing.
[0043] Those skilled in the art will appreciate that the above-described method for preparing an electrochemical device (eg, a lithium-ion battery) is merely an example, and other methods commonly used in the art may be employed without departing from the disclosure of this application.
[0044] The present application proposes an electronic device, including an electrochemical device; the electrochemical device is any electrochemical device of the present application. The electronic device of the embodiment of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a drone, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera or a large household battery, etc.
[0045] Some specific embodiments and comparative examples are listed below to better illustrate the present application, wherein a lithium-ion battery is used as an example.
[0046] Preparation of positive electrode: The positive electrode material, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride were dissolved in N-methylpyrrolidone solution at a weight ratio of 96.2:0.8:0.6:2.4 to form a positive electrode slurry. Aluminum foil was used as the positive electrode current collector (16 μm). The positive electrode slurry was coated on the positive electrode current collector (coating weight 0.23 kg / m 2 ), and the positive electrode is obtained after drying, cold pressing (electrode thickness 0.17mm) and cutting.
[0047] Preparation of the negative electrode: The negative electrode materials graphite, styrene acrylate and lithium carboxymethyl cellulose were mixed in a mass ratio of 98:1:1, and deionized water was used as the solvent to form a slurry of the negative electrode active material layer. Copper foil was used as the negative electrode current collector, and the slurry of the negative electrode active material layer was coated on the negative electrode current collector. The negative electrode was dried at 90°C to obtain a negative electrode sheet.
[0048] Preparation of the separator: The separator was 8 μm thick polyethylene (PE).
[0049] Preparation of the electrolyte: In an environment with a water content of less than 10 ppm, lithium hexafluorophosphate and a non-aqueous organic solvent (ethylene carbonate (EC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): vinylene carbonate (VC) = 20:30:20:28:2, weight ratio) are prepared in a weight ratio of 8:92 to form an electrolyte.
[0050] Preparation of a lithium-ion battery: The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide insulation. The electrodes are then wound to form an electrode assembly. The electrode assembly is then placed in an aluminum-plastic film package. After dehydration at 80°C, the electrolyte is injected and the battery is packaged. The battery undergoes a series of processes, including formation, degassing, and trimming, to produce a lithium-ion battery.
[0051] The test methods of this application are described below.
[0052] 1. Dn10 test
[0053] A scanning electron microscope is used to scan the cross section of the electrode along the thickness direction to obtain a scanning electron microscope (SEM) photograph. Specifically, sampling: the electrochemical device to be tested is disassembled, the electrode is removed, and soaked in a dimethyl carbonate (DMC) solution for 6 hours to remove residual electrolyte. Finally, the electrode is dried in a drying oven; sample preparation: the dried electrode is cut with a blade to obtain the cross section to be tested, that is, the cross section of the active material layer along the thickness direction; the test sample is adhered to paraffin using a hot plate, and the cross section to be tested is polished using an ion polisher. After the surface is smooth, the SEM test sample is obtained; testing: a SEM photograph of the active material layer of the electrochemical device to be tested is obtained using a scanning electron microscope (SEM). In the obtained SEM photograph, the average particle size of the active material is determined. Specifically, for a single particle, the length of the longest diagonal of the particle in the SEM photograph containing the particle is determined, and the length of the shortest diagonal of the particle is determined. The particle size of the particle is the arithmetic average of the length of the longest diagonal and the length of the shortest diagonal. Randomly select n (e.g., 100) active material particles from the SEM image and determine the particle size of each active material particle, obtaining n particle sizes. These n particles are sorted in ascending order of particle size, and the particle size of the 10%th particle in this ascending order is defined as Dn10.
[0054] 2. Dv50 test
[0055] The cumulative particle size distribution curve of the negative electrode active material was measured using a MasterSizer 2000. Dv50 is the cumulative diameter of 50% in the volume reference distribution of the particles measured using a laser scattering particle size analyzer.
[0056] 3. Pole crack detection: Take any positive electrode from the electrochemical device. If the crack in the positive electrode active material layer is no larger than 0.5 mm, it is considered to be free of cracks; otherwise, it is considered to be cracked.
[0057] 4. Lithium iron phosphate uniform distribution test (Fe ion uniform distribution):
[0058] The positive electrode active material layer on one side of the positive electrode current collector was evenly divided into an upper layer (second layer) and a lower layer (first layer) in the thickness direction. The layers were scanned by an energy spectrometer, and an area on the positive electrode current collector was randomly selected to obtain the difference in Fe mass content between the two layers.
[0059] 5. -20℃ low temperature discharge performance test:
[0060] The electrochemical device was charged from 0% SOC (state of charge) to 3.65 V at a current of 2 A at room temperature of 20°C to 25°C to obtain a charge capacity C1. After standing in an environment of -20°C for 2 h, it was discharged at a rate of 0.5C to 2.5 V to obtain a discharge capacity C2. The ratio of the discharge capacity C2 to C1 of the electrochemical device was calculated.
[0061] The difference between the embodiments and comparative examples lies in the different compositions and material properties of the positive electrode materials. Specific differences and performance tests are shown in the table below.
[0062] Table 1
[0063]
[0064] The positive electrode material used in the examples and comparative examples in Table 1 is a mixture of lithium iron phosphate, lithium nickel cobalt manganese oxide and lithium manganese oxide. Table 1 shows the mass percentage of lithium iron phosphate and lithium nickel cobalt manganese oxide in the positive electrode material, and the rest is lithium manganese oxide.
[0065] Please refer to Example 1 and Comparative Examples 1 to 3. In Example 1, no electrode cracking occurs, and there is almost no difference in the Fe content of the upper and lower layers, indicating that the lithium iron phosphate is evenly distributed in the positive electrode active material layer and does not cause the positive electrode active material layer to crack, and it has good low-temperature discharge performance.
[0066] In Comparative Example 1, the mass percentage of lithium iron phosphate is too low, which will cause manganese dissolution (not written in the table, but manganese dissolution occurred in Comparative Example 1 after testing), creating a safety hazard. In Example 1, no manganese dissolution occurred, and the safety performance was high.
[0067] In Comparative Examples 2 and 3, the mass percentage of lithium iron phosphate is too high. It can be seen that it causes the low-temperature cycle performance to begin to decline. The higher the content, the lower the low-temperature cycle performance, and the positive electrode active material layer begins to have problems of uneven Fe distribution and cracking. This may be because the mass percentage of lithium iron phosphate is too high. At this time, there is too much lithium iron phosphate and it cannot be fully adsorbed on the surface of lithium manganese oxide. The excess lithium iron phosphate floats up, resulting in a large difference in Fe content in the upper and lower layers, cracking of the pole piece, and the low-temperature performance of the electrochemical device is affected when there is too much lithium iron phosphate.
[0068] It can be seen from this that the mass percentage a of lithium iron phosphate needs to be controlled within 5wt%≤a≤20wt%.
[0069] Please refer to Examples 2 to 3 and Comparative Examples 4 to 7. In Examples 2 to 3, the Dv50 is 0.8 μm and 2.0 μm, the pole pieces do not have cracks larger than 0.3 mm, and the difference in Fe content between the upper and lower layers is small, while having good low-temperature discharge performance.
[0070] In Comparative Examples 4, 6, and 7, the Dv50 of the lithium iron phosphate was too small, resulting in cracking of the pole piece and uneven distribution of the Fe element. In Comparative Example 5, the Dv50 of the lithium iron phosphate was too large, resulting in a significant decrease in low-temperature discharge performance.
[0071] It can be seen from this that the Dv50 of lithium iron phosphate needs to be controlled between 0.8μm and 2.0μm.
[0072] Please refer to Examples 4 to 5 and Comparative Example 8. In Examples 4 to 5, the Dn10 of the lithium iron phosphate is 0.2 μm and 0.5 μm, there is no crack in the pole piece, and the difference in Fe content between the upper and lower layers is small, and it has good low-temperature discharge performance.
[0073] In Comparative Example 8, the Dn10 of its lithium iron phosphate is too small, resulting in cracks in the electrode and uneven distribution of the Fe element. This may be because the lithium iron phosphate has a small particle size and is easy to float in the positive electrode slurry, resulting in uneven distribution of lithium iron phosphate in the positive electrode active material layer, which in turn causes cracks in the positive electrode active material layer.
[0074] It can be seen from this that the Dn10 of lithium iron phosphate needs to be controlled between 0.2μm and 0.5μm.
[0075] Please refer to Example 6 and Comparative Examples 9 and 10. In Example 6, the specific surface area of lithium iron phosphate is greater than 5m 2 / g, while the specific surface area of lithium iron phosphate in Comparative Examples 9 and 10 is less than 5m 2 / g, the low-temperature discharge performance of lithium iron phosphate in comparative examples 9 and 10 is significantly reduced, which may be because the lithium iron phosphate may not be well coated with lithium manganese oxide, resulting in manganese dissolution and reducing the low-temperature performance.
[0076] It can be seen that the specific surface area of lithium iron phosphate needs to be greater than 5m 2 / g.
[0077] In Examples 4, 7 to 12, they all meet the requirements of 5wt%≤a≤20wt% defined in this application, the Dv50 of lithium iron phosphate is 0.8μm to 2.0μm, the Dn10 of lithium iron phosphate is 0.2μm to 0.5μm, and the specific surface area of lithium iron phosphate is not less than 5m 2 / g, while in Examples 4, 7 to 12, there are no cracks, and the difference in Fe content between the upper and lower layers in each example is no more than 0.3%, and the low-temperature discharge performance at -20°C is good, which shows that within the range defined in this application, lithium iron phosphate does not float up to cause differences in Fe element distribution, and the pole piece does not crack, while ensuring low-temperature performance.
[0078] It can also be seen in Examples 4, 7 to 12 that the difference in Fe content between the upper and lower layers is the largest in Example 4. This may be because the particle size of the lithium iron phosphate in Example 4 is smaller, the mass percentage of the lithium iron phosphate is higher, and the specific surface area is large. In this case, lithium iron phosphate with small particles is easy to float. It can be seen that the mass percentage of lithium iron phosphate, the particle size and the specific surface area jointly affect the performance of the positive electrode. Only when the characteristic range specified in this application is met at the same time can it have better overall performance.
[0079] In Example 4, the mass percentage of lithium nickel cobalt manganese oxide is 0. It can be seen that when the positive electrode material contains only lithium iron phosphate and lithium manganese oxide, as long as the 5wt%≤a≤20wt% specified in this application is met, the Dv50 of lithium iron phosphate is 0.8μm to 2.0μm, the Dn10 of lithium iron phosphate is 0.2μm to 0.5μm, and the specific surface area of lithium iron phosphate is not less than 5m 2 / g, the electrode quality, the uniformity of Fe element distribution and the low temperature performance can be guaranteed.
[0080] In Example 12, the mass percentage of lithium nickel cobalt manganese oxide is 5%, and the capacity retention rate of the lithium ion battery during low-temperature discharge reaches 90%, which has excellent low-temperature discharge performance. This is because 10wt%≤a≤20wt%, the Dv50 of lithium iron phosphate is 1.1μm to 1.8μm, the Dn10 of lithium iron phosphate is 0.2μm to 0.4μm; and the specific surface area of lithium iron phosphate is greater than 8m 2 / g, at this time the parameters of lithium iron phosphate are optimal, so it has the best low-temperature performance, and the Fe element distribution is more uniform.
[0081] The above description is only an illustration of some preferred embodiments of the present disclosure and the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the embodiments of the present disclosure is not limited to the technical solutions formed by the specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the above-mentioned inventive concept. For example, the above-mentioned features are replaced with (but not limited to) technical features with similar functions disclosed in the embodiments of the present disclosure.
Claims
1. An electrochemical device, characterized in that include: A positive electrode, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer located on one side or both sides of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode material, and the positive electrode material comprising lithium manganese oxide and lithium iron phosphate; Based on the total mass of the positive electrode material, the mass percentage a of the lithium iron phosphate satisfies: 5wt%≤a≤20wt%, the Dv50 of the lithium iron phosphate is 0.8μm to 2.0μm, the Dn10 of the lithium iron phosphate is 0.2μm to 0.5μm, and the specific surface area of the lithium iron phosphate is not less than 5m 2 / g.
2. The electrochemical device according to claim 1, wherein Satisfy at least one of the following: (a) 10 wt% ≤ a ≤ 20 wt%; (b) the Dv50 of the lithium iron phosphate is 1.1 μm to 1.8 μm; (c) the lithium iron phosphate has a Dn10 of 0.2 μm to 0.4 μm; (d) The specific surface area of the lithium iron phosphate is greater than 8m 2 / g.
3. The electrochemical device according to claim 1, wherein The specific surface area of the lithium manganate is 0.2 m 2 / g to 0.7m 2 / g.
4. The electrochemical device according to claim 1, wherein The positive electrode material also includes: lithium nickel cobalt manganese oxide. Based on the total mass of the positive electrode material, the mass percentage b of the lithium nickel cobalt manganese oxide satisfies: 0wt% <b≤10wt%。 5. The electrochemical device according to claim 4, characterized in that At least part of the positive electrode material is a core-shell structure, the lithium manganese oxide is located in the core of the core-shell structure, and the lithium iron phosphate and the lithium nickel cobalt manganese oxide are located in the shell of the core-shell structure.
6. The electrochemical device according to claim 1, wherein At least part of the positive electrode material is a core-shell structure, the lithium manganese oxide is located in the core of the core-shell structure, and the lithium iron phosphate is located in the shell of the core-shell structure.
7. The electrochemical device according to claim 1, wherein The positive electrode material contains at least one of B, Mg, Al, Si, S, Ti, Cr, Cu, Zn, Ga, Ge, Y, Zr, Mo, Ag, Ba, W, In, Sn, Pb or Sb.
8. The electrochemical device according to claim 1, wherein The positive electrode active material layer includes a first layer and a second layer, the first layer is located between the positive electrode current collector and the second layer, and the difference in the mass percentage of iron element in the first layer and the mass percentage of iron element in the second layer is not greater than 0.5%.
9. The electrochemical device according to claim 8, characterized in that The difference in thickness between the first layer and the second layer is no more than 20%.
10. The electrochemical device according to claim 8, characterized in that satisfy: The first layer includes lithium manganate and lithium iron phosphate, and the second layer includes lithium manganate and lithium iron phosphate; or The first layer includes lithium manganese oxide, lithium iron phosphate or lithium nickel cobalt manganese oxide, and the second layer includes lithium manganese oxide, lithium iron phosphate and lithium nickel cobalt manganese oxide.
11. The electrochemical device according to claim 8, characterized in that Based on the total mass of the positive electrode material, the mass percentage of lithium manganese oxide in the second layer is d; Based on the total mass of the positive electrode material, the mass percentage of the lithium manganese oxide in the first layer is e; wherein d<e.
12. An electronic device comprising the electrochemical device according to any one of claims 1 to 11.
Citation Information
Patent Citations
Lithium iron phosphate coated lithium manganate composite electrode material and its preparation method
CN104253270A
Electrochemical device and electronic device
CN113422000A
Recycling method of lithium iron phosphate battery
CN113611938A
Positive pole piece and electrochemical device and electronic device comprising same
CN113994513A
Preparation method and application of lithium iron phosphate battery with long cycle life