Preparation method of catalyst and application of catalyst in full hydrogenation of polycyclic aromatic hydrocarbon
By preparing nanoTiO2-supported bimetal Ru and Pt catalysts in polycyclic aromatic hydrocarbon hydrogenation reaction, the problem of insufficient activity of non-precious metal catalysts is solved, and the polycyclic aromatic hydrocarbon hydrogenation reaction is efficiently catalyzed at low temperatures and the production of high-energy-density aviation fuels is achieved. .
Patent Information
- Application Number
- CN202410933494.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing non-precious metal catalysts are insufficient in the hydrogenation reaction of polycyclic aromatic hydrocarbons, and need to operate under high temperature and high pressure conditions, and the catalytic activity at low temperatures is insufficient to achieve deep hydrogenation, making it difficult to overcome the limitation of high resonance energy.
NanoTiO2-supported bimetallic Ru and Pt catalysts (RuPtx/TP) were prepared, and the Ru-Pt state was adjusted by introducing Pt in the preparation of titanium dioxide nanoparticles to form a Ru-Pt interface to enhance the hydrogenation activity of the catalyst.
Highly efficient catalyzed hydrogenation saturation of polycyclic aromatic hydrocarbons under near room temperature conditions, achieving the production of high energy density aviation fuel, overcoming the limitations of high resonance energy, and improving the selectivity of the catalyst.
Smart Images

Figure CN118892826A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic catalytic synthesis, and specifically relates to a method for preparing a catalyst and a method for synthesizing high-energy-density endothermic aviation fuel by one-step full hydrogenation conversion of polycyclic aromatic hydrocarbons. Background Art
[0002] The hydrogenation reaction of polycyclic aromatic hydrocarbons is a highly exothermic reversible reaction. The number of molecules decreases and the conversion rate is limited by thermodynamic equilibrium. Therefore, it has thermodynamic advantages at low temperatures, which is conducive to the deep hydrogenation of polycyclic aromatic hydrocarbons. At the same time, low temperature is also conducive to the formation of cis-saturated isomers. Catalysts play an important role in the hydrogenation reaction of polycyclic aromatic hydrocarbons. The hydrogenation performance of polycyclic aromatic hydrocarbon hydrogenation catalysts mainly depends on the distribution and state of active centers. In order to improve the catalytic activity, the catalyst needs to be reasonably designed. Non-precious metals have the advantages of low cost and strong toxicity resistance, and are commonly used hydrogenation catalysts in industry. Non-precious metals often use two or more metals as active centers to improve activity; or use non-metal doping, such as C, N, P, S, etc., to obtain activity similar to that of precious metals; metal sulfide catalysts such as NiWS, CoMoS or NiMoS on Al2O3 were first used in aromatic saturation reactions, and their catalytic performance has been relatively comprehensive (Energy & Fuels, 2019, 33 (4): 2810-2838). Due to its weak turnover frequency, sulfide metals can only achieve deep hydrogenation of polycyclic aromatic hydrocarbons under harsh conditions of high operating temperature and hydrogen pressure. Currently, the overall hydrogenation activity of non-precious metal catalysts is not high, and they often need to operate under high temperature and high pressure, which has high requirements for equipment and high energy consumption.
[0003] In the catalytic hydrogenation of polycyclic aromatic hydrocarbons, noble metals (Pd, Pt, Ru, Rh, etc.) are highly active and can achieve deep hydrogenation under relatively mild conditions. They have shown great application potential in heterogeneous catalysis. However, a long reaction time is required under low temperature conditions to achieve complete conversion of the raw materials, indicating that the catalytic activity of the catalyst is still insufficient. It is necessary to further overcome the high resonance energy of polycyclic aromatic hydrocarbons and improve the catalytic activity of the catalyst at low temperatures; therefore, it is usually necessary to further adjust the state of the metal. In the past few decades, bimetallic catalysts have received widespread attention because, compared with monometallic catalysts, metal nanoparticles (NPs) have great flexibility in regulating surface geometry and electronic structure, and have a significant effect on the adsorption strength and activation energy of the reactants, thereby affecting the activity and selectivity of the catalyst (Journal of the American Chemical Society, 2017, 139 (6): 2122-2131.). Based on this, how to rationally design bimetallic catalysts is still the focus of preparing high-activity catalysts. Summary of the invention
[0004] In order to solve the above-mentioned deficiencies and shortcomings of the prior art, the present invention prepares a nano-TiO2 loaded bimetallic Ru and Pt catalyst (RuPt x / TP). The preparation method of the catalyst of the present invention adopts tetrabutyl titanate as the titanium source, hexahydrated chloroplatinic acid as the platinum source, and ruthenium chloride as the ruthenium source in the process of preparing titanium dioxide nanoparticles; RuPt is prepared by introducing Pt to adjust the electronic state of Ru. x Bimetallic catalyst supported on nano-TiO2 (RuPt x / TP); the introduction of nano-Pt interacts with Ru, and the two synergistically enhance the hydrogenation activity of the catalyst, which is successfully applied in the catalytic reaction of one-step hydrogenation conversion of polycyclic aromatic hydrocarbons to synthesize high-energy-density endothermic aviation fuel, thereby increasing the hydrogenation activity of the catalyst.
[0005] The technical solution of the present invention is as follows:
[0006] The first aspect of the present invention discloses a method for preparing a catalyst, comprising the following steps:
[0007] (1) uniformly mixing a titanium source and a structure directing agent to obtain an aging solution;
[0008] (2) subjecting the aged liquid to hydrothermal crystallization, filtering the solid and drying it;
[0009] (3) calcining the solid obtained in step (2);
[0010] (4) dissolving a platinum source and an alkali in ethylene glycol for reduction to obtain platinum nanoparticles;
[0011] (5) preparing a ruthenium source into an aqueous solution;
[0012] (6) adding deionized water to the solid obtained in step (3); then adding the platinum nanoparticles obtained in step (4), mixing at a certain temperature and drying to obtain a solid;
[0013] (7) The solid obtained in step (6) is washed with ethanol and then dispersed in water, and the ruthenium source aqueous solution in step (5) is added; the mixture is mixed evenly and dried at a certain temperature to obtain a solid, and then reduced in a H2 / Ar atmosphere to obtain the catalyst.
[0014] Preferably, the titanium source in step (1) is tetrabutyl titanate, and the structure directing agent is acetic acid; the volume ratio of tetrabutyl titanate to acetic acid is 1:(3-5), preferably 1:4.
[0015] Preferably, the hydrothermal crystallization conditions of step (2) are 180-220° C., 12-36 h; more preferably 200° C., 24 h.
[0016] Preferably, the calcination temperature of step (3) is 300-500°C, and the calcination time is 2-6h; preferably 400°C and 4h.
[0017] Preferably, in step (4), the platinum source is chloroplatinic acid hexahydrate, and the base is sodium hydroxide; the reduction temperature is 140-180° C., preferably 160° C.; preferably, the amount of chloroplatinic acid hexahydrate is 1 g, the amount of sodium hydroxide is 1 g, and the amount of ethylene glycol is 100 mL.
[0018] Preferably, the ruthenium source in step (5) is ruthenium chloride.
[0019] Preferably, the molar ratio of ruthenium in the ruthenium source aqueous solution in step (7) to platinum in the solid is 1:(0.05-0.20), preferably 1:0.13.
[0020] Preferably, the reduction temperature in step (7) is 300-500°C, preferably 400°C.
[0021] The second aspect of the present invention discloses the use of the catalyst prepared by the preparation method for low-temperature catalytic one-step reaction of polycyclic aromatic hydrocarbons to obtain high-energy density fuel; the high-energy density fuel is one or more of perhydroacenaphthene, perhydrofluorene, decahydronaphthalene and perhydroanthracene.
[0022] Beneficial effects of the present invention:
[0023] 1. The preparation method of the present invention prepares RuPt x / TP bimetallic catalyst, the formation of Ru-Pt interface causes the change of electronic structure of Ru and Pt, the electrons of Ru are transferred to Pt, resulting in the decrease of electron density of Ru, while Ru and Pt interact with the carrier TiO2 respectively, increasing the hydrogenation activity of the catalyst. 0.13 / TP is the most suitable catalyst
[0024] 2. RuPt prepared by the preparation method of the present invention x The / TP bimetallic catalyst is used for one-step hydrogenation of polycyclic aromatic hydrocarbons to synthesize high energy density fuels. It can overcome the high resonance energy of polycyclic aromatic hydrocarbons, efficiently catalyze the hydrogenation saturation of polycyclic aromatic hydrocarbons at near room temperature, and achieve high selectivity for cis products. The catalyst of the present invention achieves the purpose of preparing high energy density aviation fuel by one-step hydrogenation saturation of polycyclic aromatic hydrocarbons at low temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the Raman photo of the catalyst prepared in Example 1-3.
[0026] Figure 2 It is the X-ray diffraction (XRD) diagram of the catalyst prepared in Example 1-4.
[0027] Figure 3 It is the X-ray photoelectron spectroscopy (XPS) graph of the catalyst prepared in Example 1-3. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with specific embodiments. These embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The embodiments in the examples are only preferred embodiments, but the present invention is not limited to the preferred embodiments.
[0029] Example 1: The amount of nano-Pt added is such that the molar ratio of nano-Pt to Ru is 0.08:1.
[0030] (1) Add 5 mL of tetrabutyl titanate to 20 mL of glacial acetic acid under stirring at room temperature; after stirring for 30 min, transfer to 100 mL of polytetrafluoroethylene liner and perform hydrothermal synthesis at 200 °C for 24 h;
[0031] (2) After cooling naturally to room temperature, the sample was washed three times with anhydrous ethanol and dried at 80°C overnight to obtain a powder;
[0032] (3) The collected powder was ground and heated in a muffle furnace at 5 °C min -1 The sample was calcined at 400℃ for 4h at a heating rate of 1.5°C. The sample was named TiO2-NP.
[0033] (4) Add 100 mL of ethylene glycol to a three-necked flask, add 1 g of sodium hydroxide under stirring at room temperature until it is completely dissolved, and then add 1 g of chloroplatinic acid hexahydrate; stir vigorously to dissolve, and the solution is now orange and transparent; then transfer the three-necked flask containing the mixed solution to an oil bath and heat it, and reduce it at 160° C. under N2 atmosphere protection for 3 h; after the reaction is completed, naturally cool it to room temperature;
[0034] (5) Add the solid obtained in step (3) into a 100 mL tall beaker, add 20 mL of deionized water; add 665 μL of the solution in step (4), and stir and dry at 90° C.; wash the obtained solid powder three times with 95% ethanol;
[0035] (6) Dissolve 0.5 g of ruthenium chloride in 50 mL of ultrapure water to make 0.01 g mL -1 of an aqueous solution of ruthenium chloride;
[0036] (7) The solid obtained in step (5) was added to a 100 mL tall beaker, and 20 mL of deionized water was added; 3.1 mL of the solution in step (7) was added (the molar ratio of Pt to Ru was 0.08:1 at this time), and the mixture was stirred and dried at 90° C. The obtained solid powder was heated in a 10 v / v% H2 / Ar atmosphere (150 mL·min-1 ) at 5℃·min -1 The catalyst is obtained by reducing the catalyst at 400°C for 1 h at a heating rate of 1.000 °C. 0.08 / TP.
[0037] Example 2: The amount of nano-Pt added is such that the molar ratio of nano-Pt to Ru is 0.13:1.
[0038] The conditions and steps are the same as those in Example 1, except that the amount of nano-Pt added in step (5) is 1 mL. 0.13 / TP.
[0039] Example 3: The amount of nano-Pt added is such that the molar ratio of nano-Pt to Ru is 0.17:1.
[0040] The conditions and steps were the same as those in Example 1, except that the amount of nano-Pt added in step (5) was 1.35 mL. 0.17 / TP.
[0041] Example 4: Same as Example 3, but without adding ruthenium source. The sample is named Pt 0.17 / TP.
[0042] Figure 1 is a Raman photo of the catalyst prepared in Example 1-3, Figure 2 is the X-ray diffraction (XRD) image of the catalyst prepared in Example 1-4; Figure 3 Figure 1 is an X-ray photoelectron spectroscopy (XPS) image of different Ru catalysts prepared in Examples 1-3. Figure 1 It can be seen that with the increase of the amount of Pt introduced, the -1 、637cm -1 、393cm -1 and 515cm -1 At RuPt0 .13 / TP vs. RuPt 0.08 / TP produced a larger blue shift, indicating that the interactions between metals and metals and between metals and carriers gradually increased, while RuPt 0.17 / TP and RuPt 0.13 / TP are comparable, indicating that there is a limit to the modification of Pt particles. Figure 2 It can be seen that no identifiable diffraction peaks related to Ru nanoclusters were found in the Ru-based catalyst, and with the increase of Pt loading, no diffraction peaks related to Pt and diffraction peaks of RuPt alloy were observed, indicating that Ru and Pt have good dispersion on the support and the particle size is quite small. Figure 3It can be seen that due to the interaction between Pt and Ru, as the amount of Pt introduced increases, the electron-deficient Ru species (Ru δ+ ) increases; however, there is an appropriate ratio between Pt and Ru, with a threshold of about 0.13 (mol Pt / mol Ru ). The XPS spectra of Pt and Ru show that there is a strong electronic coupling effect between Pt and Ru atoms; the change in the local environment of the metal surface atoms indicates that the electronic structure of the two metals (Ru and Pt) has changed significantly. Table 1 shows the Ru 3d spectrum results of the catalysts prepared in Examples 1-3.
[0043] Table 1 Ru 3d spectra of different samples
[0044]
[0045] It can be seen from Table 1 that the introduction of Pt changes the electronic state of Ru, but Ru cannot be further modified with the increase of the amount of Pt introduced.
[0046] Example 5: One-step hydrogenation conversion of polycyclic aromatic hydrocarbons to synthesize high-energy fuels; using the catalyst of Examples 1-4, the steps are:
[0047] 2 g of acenaphthene and 90 mL of decahydronaphthalene were added into a 250 mL high temperature and high pressure reactor; the hydrogen pressure was 4 MPa, heated to 60° C. and reacted for 0-3 hours at a rotation speed of 600 rpm.
[0048] The conversion rate, yield and product selectivity achieved by using the catalysts of Examples 1-4 are shown in Table 1.
[0049] Table 2 Comparison of catalytic results of catalysts of Examples 1-4
[0050]
[0051] It can be seen from Table 2 that RuPt 0.13 / TP has significantly higher catalytic activity than RuPt 0.08 / TP catalyst, but RuPt 0.17 / TP catalyst did not significantly improve, and the cis isomer selectivity decreased. 0.13 / TP is the most suitable catalyst.
[0052] Comparative Example: Hydrogenation saturation of tricyclic polycyclic aromatic hydrocarbons was achieved at near room temperature of 60°C. The catalytic activity can be compared with the Ru / TP-400 catalyst in Table 3 of CN2024109320579, and the catalysts (Ru / TP-400 vs. RuPt in Example 2) can be compared in terms of product selectivity and reactant conversion. 0.13 / TP) (hydrogenation reaction conditions: 2g acenaphthene, 60°C, 4MPa hydrogen, 0.4g catalyst)
[0053] The results are as follows: for the Ru / TP-400 catalyst in Table 3 of CN2024109320579, at a hydrogenation temperature of 60°C, the acenaphthene conversion rate was 98.8% in 3 hours, and the cis-product selectivity was 29%; and the acenaphthene conversion rate was 100% in 6 hours, and the cis-product selectivity was 95%.
[0054] The RuPt of Example 2 of the present invention 0.13 / TP catalyst, at a hydrogenation temperature of 60°C, only takes 3 hours to achieve 100% acenaphthene conversion and 96% cis product selectivity. 0.08 / TP and RuPt 0.17 The hydrogenation catalytic activity of / TP is also higher than that of the catalyst in CN2024109320579.
[0055] Therefore, the Ru hydrogenation catalytic activity of the present invention is higher than that of the hydrogenation catalyst in CN2024109320579.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a catalyst, characterized in that: The steps include: (1) uniformly mixing a titanium source and a structure directing agent to obtain an aging solution; (2) subjecting the aged liquid to hydrothermal crystallization, filtering the solid and drying it; (3) calcining the solid obtained in step (2); (4) dissolving a platinum source and an alkali in ethylene glycol for reduction to obtain platinum nanoparticles; (5) preparing a ruthenium source into an aqueous solution; (6) adding deionized water to the solid obtained in step (3); then adding the platinum nanoparticles obtained in step (4), mixing at a certain temperature and drying to obtain a solid; (7) The solid obtained in step (6) is washed with ethanol and then dispersed in water, and the ruthenium source aqueous solution in step (5) is added; the mixture is mixed evenly and dried at a certain temperature to obtain a solid, and then reduced in a H2 / Ar atmosphere to obtain the catalyst.
2. The preparation method according to claim 1, characterized in that: The titanium source in step (1) is tetrabutyl titanate, and the structure directing agent is acetic acid; the volume ratio of tetrabutyl titanate to acetic acid is 1:(3-5).
3. The preparation method according to claim 1, characterized in that: The hydrothermal crystallization conditions of step (2) are 180-220° C., 12-36 h.
4. The preparation method according to claim 1, characterized in that: The calcination temperature of step (3) is 300-500° C., and the calcination time is 2-6 hours.
5. The preparation method according to claim 1, characterized in that: In step (4), the platinum source is chloroplatinic acid hexahydrate, the base is sodium hydroxide, and the reduction temperature is 140-180°C.
6. The preparation method according to claim 1, characterized in that: The ruthenium source in step (5) is ruthenium chloride.
7. The preparation method according to claim 1, characterized in that: In step (7), the molar ratio of ruthenium in the ruthenium source aqueous solution to platinum in the solid is 1:(0.05-0.20).
8. The preparation method according to claim 1, characterized in that: The reduction temperature of step (7) is 300-500°C.
9. Use of the catalyst prepared by the preparation method according to any one of claims 1 to 8 for one-step reaction of polycyclic aromatic hydrocarbons to obtain fuel.
Citation Information
Patent Citations
Method for preparing low platinum modified carbon-loaded ruthenium nano particles and application thereof
CN101580225A
Controllable bimetallic core-shell nanostructure and catalyst, preparation methods of nanostructure and catalyst and application of catalyst
CN108579758A
1,8-dinitronaphthalene hydrogenation catalyst and preparation method thereof
CN108686652A
Method for synthesizing 3-hydroxy-2-pentanone through selective hydrogenation
CN114733538A
Synthesis and application of copper modified TiO2 nanosheet
CN115445618A