High-stability fiber filter membrane for low-temperature catalytic oxidation of formaldehyde as well as preparation method and application of high-stability fiber filter membrane
Through low-temperature chemical reduction and layer-by-layer electrostatic self-assembly technology, a highly efficient and highly stable manganese-based nanocatalytic fiber filter membrane was prepared, which solved the problems of complex process and low catalyst load in the existing technology, and achieved efficient catalytic oxidation of formaldehyde and structurally stable fiber filter membranes, suitable for large-scale production and air purification.
Patent Information
- Application Number
- CN202410922237.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the preparation process of fiber membranes with low temperature catalytic oxidation of formaldehyde is complex and the catalyst load is low, and there are challenges in stability and solid load uniformity. The electrostatic and hydrophobicity of the surface of the common filter membrane are not suitable for the development of hydrophilic substrate materials. .
Using low-temperature chemical reduction and layer-level electrostatic self-assembly technology, a high-efficiency and high-stability manganese-based nanocatalytic fiber filter membrane was prepared. By modifying the polydiallyl dimethyl ammonium chloride layer on the hydrophobic fiber filter membrane, the polydiallyl dimethyl ammonium chloride layer was firmly used. Fix manganese oxygen nanocatalytic materials to improve loading and stability.
The fiber filter membrane that has efficient catalytic oxidation of formaldehyde has high structural stability and self-cleaning performance. It is suitable for large-scale production and actual air purification applications. The formaldehyde removal rate can reach more than 95%.
Smart Images

Figure CN118892864A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of air purification, and more specifically to a high-stability fiber filter membrane for low-temperature catalytic oxidation of formaldehyde, and a preparation method and application thereof. Background Art
[0002] Formaldehyde is a major indoor air pollutant that is recognized to be extremely toxic and is listed as a Class I carcinogen by the World Health Organization. As people's requirements for quality of life and attention to health increase, the development of long-term, green, low-carbon and environmentally friendly formaldehyde purification technology has important practical and research significance. Among the many physical and chemical formaldehyde removal technologies, the technology of catalytic oxidation and purification of formaldehyde using cheap metal catalysts is the technology with the greatest application potential in terminal treatment technology. For example, catalysts based on metal oxides such as manganese, cerium, and cobalt show excellent formaldehyde catalytic degradation performance at low temperature or room temperature.
[0003] In the terminal application of air purification, powdered catalysts often need to be immobilized to reduce the loss of nanocatalyst powder during the application process, reduce the cost of catalyst application, and avoid secondary pollution caused by dust overflow. The immobilization method of current formaldehyde catalyst mainly includes immobilizing the metal catalyst on a substrate such as an organic polymer, an inorganic porous material or a carbon fiber material by in-situ growth or multi-step assembly, or preparing a fiber membrane structure of the metal catalyst by electrostatic spinning technology. For example, CN112495387A discloses a carbon fiber-based silver / cobalt manganese layered double hydroxide composite material, which needs to be deposited on a carbon fiber substrate by an in-situ coprecipitation method, and then silver nanoparticles are loaded on the carbon fiber-based cobalt manganese layered double hydroxide by an impregnation sodium borohydride reduction method, and finally a carbon fiber-based silver / cobalt manganese layered double hydroxide composite material is obtained, and the removal rate of formaldehyde in the composite material within 60min is 71.4%, and the formaldehyde removal amount in a single experiment per gram of composite material is 11mg. However, the preparation process is relatively cumbersome, requiring the preparation of cobalt-manganese layered double hydroxide nanosheets and their loading on a substrate, and then the preparation and loading of silver nanoparticles, and the catalyst loading is low (about 0.5%), and the risk of catalyst peeling and overflowing is easily affected by airflow during use, which is not conducive to a stable and efficient purification process. CN113231108A discloses a nanofiber membrane material that can catalytically oxidize formaldehyde at low temperature, wherein La2CoMnO6 / CeO2 catalyst is synthesized by chemical precipitation, drying, roasting and grinding, and then La2CoMnO6 / CeO2 and cellulose acetate fiber are woven into nanofiber membranes by electrostatic spinning, wherein the catalyst loading is 1-4%, and the conversion rate of formaldehyde at 25°C is 86%. There are also the problems of cumbersome preparation process and low catalyst loading, and at the same time, affected by the electrostatic spinning process, most of the catalyst is embedded in the fiber membrane material, which obviously causes a waste of catalyst for the fiber membrane material with surface reaction as the purification pathway. In addition, the surface of the common air purification filter membrane has strong electrostatic and hydrophobic properties, and the development of traditional hydrophilic base membranes can no longer guide the current research direction. Therefore, there are still great challenges in the difficulty of immobilizing nanocatalytic materials on its surface, the loading amount, loading uniformity and stability of nanomaterials. Summary of the invention
[0004] To solve the above problems, the first object of the present invention is to provide a method for preparing a fiber filter membrane for catalytic oxidation of formaldehyde. The present invention innovatively constructs a novel manganese-based nanocatalytic fiber filter membrane with high efficiency and high stability that can be used for low-temperature catalytic purification of formaldehyde by combining low-temperature chemical reduction and layer-by-layer electrostatic self-assembly. The entire preparation method is green, simple and convenient, and can complete large-scale preparation and large-scale production of fiber filter membranes, laying a foundation for the application of powdered nanocatalysts in actual air purification equipment.
[0005] The second object of the present invention is to provide a fiber filter membrane for low-temperature catalytic oxidation of formaldehyde prepared by the above-mentioned preparation method. The fiber filter membrane maintains the original high-efficiency catalytic performance of manganese oxide compounds, and also has better structural stability. In multiple friction bending, wind blowing, water flushing and other actual working condition simulation experiments, the fiber filter membrane can still maintain the high stability of the original structure and catalytic performance, and is suitable for the preparation of current air purification filter membranes.
[0006] The third object of the present invention is to provide an application of the fiber filter membrane for low-temperature catalytic oxidation of formaldehyde as described above in low-temperature purification of formaldehyde.
[0007] A fourth object of the present invention is to provide a filter membrane for air purification.
[0008] A fifth object of the present invention is to provide an air purification device.
[0009] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0010] The present invention discloses a method for preparing a fiber filter membrane for catalytic oxidation of formaldehyde, comprising the following steps:
[0011] 1) dispersing a manganese salt in deionized water, adding a reducing agent and or not adding an element doping material, performing a low-temperature reduction reaction to obtain a manganese oxide compound precursor, and then dispersing the precursor in deionized water to obtain a manganese oxide compound precursor suspension;
[0012] 2) immersing the hydrophobic fiber filter membrane in a polydiallyldimethylammonium chloride solution, taking out the filter membrane, and drying it at a certain temperature to obtain a hydrophobic fiber filter membrane modified with polydiallyldimethylammonium chloride;
[0013] 3) placing the hydrophobic fiber filter membrane modified with polydiallyldimethylammonium chloride in a suspension of a manganese oxide compound precursor, taking it out after immersion for a period of time, and obtaining the fiber filter membrane after drying and heat treatment.
[0014] In the preparation method, a commercially available hydrophobic fiber filter membrane is used as the base material, and a layer of polydiallyldimethylammonium chloride (PDDA) is modified on its surface by electrostatic self-assembly. The membrane is then immersed in a suspension of a manganese oxide compound precursor prepared by a low-temperature chemical reduction method. After drying and heat treatment, the manganese oxide nano-catalytic material is firmly riveted to the surface of the fiber filter membrane under the action of polydiallyldimethylammonium chloride to prevent the manganese oxide nano-catalytic material from agglomerating and falling off, thereby obtaining a fiber filter membrane with high loading capacity, good stability and high catalytic efficiency, which is resistant to bending, wear, wind and water washing, and has self-cleaning properties.
[0015] Further, the concentration of the polydiallyldimethylammonium chloride solution mainly affects the firmness of the manganese oxide nanocatalytic material on the hydrophobic fiber filter membrane, thereby regulating the structural stability of the obtained fiber filter membrane. In a specific embodiment, the concentration of the polydiallyldimethylammonium chloride solution is 0.05-1.0wt%, and further increasing the concentration has little effect on the firmness; illustratively, the concentration of the polydiallyldimethylammonium chloride solution can be 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, etc.
[0016] The present invention does not limit the type of catalyst manganese oxide compound precursor. According to the different raw materials and additional element doping materials (such as N, N-dimethylformamide, sodium nitride, etc.), common manganese oxide compound nanocatalytic materials in the art can be obtained, such as manganese dioxide, potassium-containing manganese oxide, carbon-containing manganese oxide, nitrogen-containing manganese oxide, carbon-containing nitrogen manganese oxide and other non-metallic atom doped modified manganese oxides, manganese-cerium, manganese-cobalt, manganese-copper, manganese-nickel and other manganese-based metal composite oxides and other composite oxides. In addition, it should be noted that the present invention aims to solve the problem of how to stably exist powdered nanocatalysts on hydrophobic substrates. Therefore, the manganese-based catalysts currently reported for catalytic oxidation of formaldehyde should all be applicable to the preparation method provided by the present invention.
[0017] Further, the manganese salt includes but is not limited to one or more of manganese permanganate (e.g. potassium permanganate), manganese nitrate (e.g. manganese nitrate), manganese sulfate (e.g. manganese sulfate), and manganese acetate (e.g. manganese acetate);
[0018] The reducing agent includes but is not limited to one or more of low-valent manganese salts, ammonium salts, and N,N-dimethylformamide; the ammonium salt is a reducing ammonium-containing compound commonly used in the art, including but not limited to ammonium carbonate, ammonium bicarbonate, ammonium oxalate, and the like.
[0019] The hydrophobic fiber filter membrane is selected from microporous polymer fiber filter membrane.
[0020] Furthermore, in step 1), the concentration of the manganese salt in deionized water is 0.01-0.2 g / mL, and the volume of the deionized water is 50-100 mL.
[0021] Furthermore, the hydrophobic fiber filter membrane is selected from one or more of polyethylene terephthalate film (PET), polybutylene terephthalate film (PBT), polytetrafluoroethylene film (PTFE), and polypropylene film (PP).
[0022] Furthermore, the hydrophobic fiber filter membrane also includes a pretreatment process before impregnation, that is, the hydrophobic filter membrane is cut into a suitable size, ultrasonically treated with anhydrous ethanol and deionized water, cleaned, dried, and set aside.
[0023] Furthermore, the size of the hydrophobic filter membrane after cutting is no greater than 1000 cm 2 The shape is preferably one of the conventional film shapes such as rectangle, square, circle, oval, etc.
[0024] Further, in step 2), the immersion time of the hydrophobic filter membrane in the polydiallyldimethylammonium chloride solution is 10 to 120 min, and equilibrium can be reached within 10 min; illustratively, the immersion time can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, etc.
[0025] Further, in step 3), the immersion time is 5 to 30 minutes. Exemplarily, the immersion time can be 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc.
[0026] Furthermore, the reaction temperature of the low-temperature reduction reaction is ≤100°C, and the reaction time is 2 to 10 hours. Preferably, the reaction temperature of the low-temperature reduction reaction is 40 to 100°C.
[0027] Furthermore, in step 2), the drying temperature is 20 to 60° C., and the drying time is 10 min to 6 h.
[0028] Furthermore, in step 3), drying is to remove a large amount of water. When the reducing agent is selected from low-valent manganese salts, the drying temperature is 20-60° C. and the drying time is 0.5-2 h; when the reducing agent is not selected from low-valent manganese salts, the drying temperature is 20-40° C. and the drying time is 0.5-2 h.
[0029] Further, in step 3), the heat treatment is to complete the crystallization reaction of the manganese oxide compound precursor. When the reducing agent is selected from low-valent manganese salts, the heat treatment temperature is 40-120°C, preferably 60-110°C, and the heat treatment time is 6-24h; when the reducing agent is not selected from low-valent manganese salts, if the heat treatment temperature is too high, it is not conducive to the formaldehyde purification performance of the fiber filter membrane, preferably 40-100°C, more preferably 40-60°C, and the heat treatment time is 6-24h.
[0030] Further, in step 3), the loading amount of the manganese oxide catalytic material on the fiber filter membrane is 8-13wt%. Exemplarily, the loading amount can be 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, or 13wt%.
[0031] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0032] The invention discloses a fiber filter membrane for low-temperature catalytic oxidation of formaldehyde, which is prepared by the preparation method as described above.
[0033] In order to achieve the third object, the present invention adopts the following technical solutions:
[0034] The present invention discloses an application of the fiber filter membrane used for low-temperature catalytic oxidation of formaldehyde in low-temperature purification of formaldehyde.
[0035] Furthermore, the low temperature is 0 to 50°C.
[0036] The present invention can achieve a formaldehyde removal rate of more than 95% in an environment where the formaldehyde concentration is not greater than 100 ppm.
[0037] In order to achieve the fourth objective, the present invention adopts the following technical solutions:
[0038] The invention discloses a filter membrane for air purification comprising the fiber filter membrane as described above.
[0039] In order to achieve the fifth object, the present invention adopts the following technical solutions:
[0040] The present invention discloses an air purification device comprising the fiber filter membrane as described above.
[0041] The beneficial effects of the present invention are as follows:
[0042] The present invention discloses a fiber filter membrane for catalytic oxidation of formaldehyde. Compared with the prior art, the technical solution of the present invention has at least the following advantages:
[0043] (1) The preparation method is highly versatile: The preparation method provided by the present invention is applicable to a wide range of immobilized nanocatalysts, including not only all common formaldehyde catalytic purification nanomaterials, but also other common nanocatalytic materials, including but not limited to indoor VOCs nanocatalytic materials, industrial VOCs nanocatalytic materials, aerosol pollutant purification nanomaterials, bacteria, viruses and other biological pollutants purification nanomaterials and other materials. The fiber filter membrane substrate material used is also relatively wide, and the common hydrophobic polymer fiber membrane in the field can be selected, and the polymer fiber includes but is not limited to polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE), polypropylene (PP), etc.;
[0044] (2) The preparation method is suitable for large-scale production: The preparation method provided by the present invention utilizes a low-temperature chemical reduction method combined with a layer-by-layer electrostatic self-assembly method to prepare a fiber filter membrane with excellent catalytic performance and high stability. The synthesis has low energy consumption, simple process, convenient operation, low environmental pollution, and high film formation rate. It is suitable for large-scale preparation and large-scale production and has strong practicality.
[0045] (3) Stable structure of the fiber filter membrane: The fiber filter membrane provided by the present invention has strong structural stability while maintaining the original high-efficiency catalytic performance of manganese oxide. It maintains high stability of the filter membrane structure and catalytic performance in actual working condition simulation experiments such as multiple friction bending, long-term wind blowing, and water washing;
[0046] (4) The fiber filter membrane has good formaldehyde removal performance: the fiber filter membrane provided by the present invention can catalytically oxidize and degrade formaldehyde at low temperature (0-50°C). In an environment where the formaldehyde concentration is not more than 100 ppm, the formaldehyde removal rate can reach more than 95%. In addition, the nano-catalytic material is evenly dispersed on the provided fiber filter membrane, and the surface of the fiber filter membrane has super hydrophilicity, thus showing excellent self-cleaning performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0048] Figure 1 The scanning electron microscope pictures of the polymer film PET, PETP film and Mn / PETP film in Example 1 are shown, wherein (a) is the polymer film PET, (b) is the PETP film, and (c) and (d) are Mn / PETP films.
[0049] Figure 2The transmission electron micrographs of the carbon-doped manganese oxide catalyst nanomaterial on the Mn / PETP film obtained in Example 1 and its energy dispersive X-ray spectroscopy (EDS) elemental surface distribution diagram are shown. Among them, (a) and (b) are transmission electron micrographs of the carbon-doped manganese oxide catalyst nanomaterial, and (c-f) are EDS elemental surface distribution diagrams of the PDDA carbon-doped manganese oxide catalyst nanomaterial, among which (d) is Mn, (e) is O, and (f) is C.
[0050] Figure 3 The evaluation of the bending wear stability of the Mn / PETP film of Example 1 is shown.
[0051] Figure 4 The wind abrasion stability evaluation of the Mn / PETP film of Example 1 is shown.
[0052] Figure 5 The water washing and self-cleaning performance evaluation of the Mn / PETP film of Example 1 is shown.
[0053] Figure 6 The formaldehyde catalytic purification efficiency diagram of the PET film and the Mn / PETP film of Example 1 is shown, wherein BG represents the blank control.
[0054] Figure 7 The figure shows the efficiency of the Mn / PETP membrane of Example 1 in catalytic purification of formaldehyde at different ambient temperatures. DETAILED DESCRIPTION
[0055] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0056] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0057] Example 1
[0058] The present invention provides a method for preparing a high-stability fiber filter membrane having low-temperature and high-efficiency catalytic purification performance of formaldehyde, comprising the following steps:
[0059] (1) Pretreatment of microporous breathable hydrophobic organic polymer PET film: Cut the commercially available polymer PET film into 4×6 cm size, ultrasonically treat it with anhydrous ethanol and deionized water for 20 min respectively, with the ultrasonic temperature not higher than 30° C., wash it, dry it, and set it aside;
[0060] (2) Preparation of carbon-doped manganese oxide precursor suspension: 1.264 g of potassium permanganate was dispersed in deionized water, 5 mL of DMF was added dropwise, and the mixture was stirred in a water bath at 40-100° C. for 2-10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed with deionized water several times to obtain a carbon-doped manganese oxide precursor sample. The carbon-doped manganese oxide precursor sample was ultrasonically dispersed in 50 mL of deionized water to obtain a carbon-doped manganese oxide precursor suspension;
[0061] (3) Preparation of PETP film: Prepare a polydiallyldimethylammonium chloride (PDDA) solution with a concentration of 0.1 wt%, immerse the pretreated PET film in the PDDA solution for 10 to 120 min, and dry at 20 to 60 ° C for 10 min to 6 h to obtain a PDDA-modified PET film, referred to as PETP film;
[0062] (4) Carbon-doped manganese oxide fiber filter membrane: The PETP membrane obtained in step (3) is immersed in the carbon-doped manganese oxide precursor suspension prepared in step (2) for 10 min. The filter membrane is taken out, dried at 20-40° C. for 0.5-2 h, and then heat-treated at 60° C. for 12 h to obtain a carbon-doped manganese oxide fiber filter membrane, referred to as Mn / PETP membrane.
[0063] The scanning electron micrographs of the obtained PETP membrane and Mn / PETP membrane are shown in Figure 1 The corresponding transmission electron microscopy images and EDS element distribution maps of carbon-doped manganese oxide nanomaterials on Mn / PETP membrane are shown in Figure 2 As shown. Figure 1 It can be seen that the manganese oxide nanomaterial is successfully loaded on the fibers of the PET filter membrane. After loading the manganese oxide nanomaterial, the filter membrane still maintains a good microporous structure to ensure good air permeability of the filter membrane. The prepared carbon-doped manganese oxide nanomaterial is composed of nanocrystals and nanobelts. The elemental EDS analysis results show that carbon is successfully doped into the structure of the manganese oxide nanomaterial, with a carbon doping amount of 54.4at%, a potassium doping amount of 1.3at%, and a loading amount of 10.4wt% of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP membrane.
[0064] Example 2
[0065] This example is used to investigate the effect of the amount of DMF on the content of catalyst carbon-doped manganese oxide carbon and potassium in the obtained Mn / PETP film.
[0066] In practical applications, the amount of DMF added can be any volume within the range of 2.0 to 10 mL to adjust the carbon doping amount and potassium doping amount in the obtained manganese oxide nanomaterial, and further adjust the catalytic purification performance of the carbon-doped manganese oxide fiber filter membrane.
[0067] In practical application, based on the scheme of Example 1, only the amount of DMF added was changed to 2.5 mL and 7.5 mL, and the loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP film was about 10.8 wt% and 13.1 wt%, respectively. The carbon doping amount and potassium doping amount in the obtained carbon-doped manganese oxide material are shown in Table 1. As can be seen from Table 1, DMF as a reducing agent and an element doping agent has a great influence on the carbon doping amount and the potassium doping amount in the catalytic material.
[0068] Table 1
[0069] DMF drop amount Carbon doping amount Potassium doping amount 2.5mL 73.9at% 0at% 7.5mL 58.5at% 0.7at%
[0070] Example 3
[0071] The preparation process of Example 1 was repeated, except that the concentration of the PDDA solution was changed to 0.05 wt %. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP membrane was 10.2 wt %.
[0072] Example 4
[0073] The preparation process of Example 1 was repeated, except that the concentration of the PDDA solution was changed to 0.2 wt %. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP membrane was 10.3 wt %.
[0074] Example 5
[0075] The preparation process of Example 1 was repeated, except that the concentration of the PDDA solution was changed to 0.8 wt %. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP membrane was 9.3 wt %.
[0076] Example 6
[0077] The preparation process of Example 1 was repeated, except that the heat treatment temperature was changed to 40° C. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP film was substantially the same as that in Example 1.
[0078] Example 7
[0079] The preparation process of Example 1 was repeated, except that the heat treatment temperature was changed to 80° C. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP film was substantially the same as that in Example 1.
[0080] Example 8
[0081] The preparation process of Example 1 was repeated, except that the heat treatment temperature was changed to 100° C. The loading amount of the carbon-doped manganese oxide catalytic material on the obtained Mn / PETP membrane was substantially the same as that in Example 1.
[0082] Test Example 1: Test on the bending and abrasion resistance of fiber filter membrane
[0083] Take a piece of Mn / PETP film prepared in Example 1 and Examples 3 to 5 respectively, bend it forward and backward 50 times, bend it 10 times each time, observe the surface morphology of the Mn / PETP film and record the mass change of the Mn / PETP film, and test the bending and wear resistance of the carbon-doped manganese oxide fiber filter membrane, wherein the calculation method is as follows:
[0084] Mass percentage (%) = m / m0 × 100%
[0085] Mass loss percentage (%) = (m0-m) / m0×100%
[0086] Where m0 is the initial mass of the filter membrane, in grams, and m is the mass of the filter membrane after bending, in grams.
[0087] In practical applications, during the PDDA impregnation treatment, the concentration of the PDDA solution can be any concentration in the range of 0.05 to 1.0 wt%. It is found from the test in Table 2 that the concentration of the PDDA solution can adjust the firmness of the carbon-doped manganese oxide nanopowder on the obtained Mn / PETP membrane, and further adjust the structural stability of the carbon-doped manganese oxide fiber filter membrane.
[0088] Table 2
[0089] Example 1 Example 3 Example 4 Example 5 Percentage of mass loss 0.9% 1.4% 1% 0.6%
[0090] Figure 3 The bending and abrasion test and evaluation results of the carbon-doped manganese oxide fiber filter membrane prepared in Example 1 are shown in the figure. It can be seen from the figure that the mass loss of the present invention is small after 50 consecutive bends, indicating that the carbon-doped manganese oxide fiber filter membrane provided by the present invention has excellent bending and abrasion resistance, and the carbon-doped manganese oxide catalyst immobilized on the membrane is not easy to fall off. This shows that the selection of green, environmentally friendly and low-cost PDDA as an anchor stabilizer for the nanocatalyst on the polymer filter membrane substrate, and the purification membrane constructed by layer-by-layer electrostatic self-assembly, enhances the interaction between the manganese oxide catalyst nanomaterial and the microporous filter membrane substrate, and prevents the aggregation and shedding of the manganese oxide nanomaterial.
[0091] Example 9
[0092] The present invention provides a method for preparing a high-stability fiber filter membrane having low-temperature and high-efficiency catalytic purification performance of formaldehyde, comprising the following steps:
[0093] (1) Pretreatment of the microporous breathable hydrophobic organic polymer PET film: the polymer film PET was cut into 4×6 cm in size, and ultrasonically treated with anhydrous ethanol and deionized water for 20 min respectively, with the ultrasonic temperature not higher than 30° C., and then washed, dried, and set aside;
[0094] (2) Preparation of potassium-containing manganese oxide precursor suspension: 0.79 g of potassium permanganate was dispersed in 100 mL of deionized water and fully dissolved. 1.135 g of manganese sulfate was added to the above solution under vigorous stirring. The mixture was stirred and reacted at room temperature for 2 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and washed with deionized water several times to obtain a potassium-containing manganese oxide precursor sample. The manganese oxide precursor sample was ultrasonically dispersed in 50 mL of deionized water to obtain a potassium-containing manganese oxide precursor suspension.
[0095] (3) Preparation of PETP film: Prepare a polydiallyldimethylammonium chloride (PDDA) solution with a concentration of 0.1 wt%, immerse the pretreated PET film in the PDDA solution for 10 to 120 min, and dry at 20 to 60 ° C for 10 min to 6 h to obtain a PDDA-modified PET film, referred to as PETP film;
[0096] (4) Potassium-containing manganese oxide fiber filter membrane: The PETP membrane prepared in step 3 is immersed in the potassium-containing manganese oxide precursor suspension prepared in step 2 for 10 minutes, the filter membrane is taken out, dried at 60° C. for 0.5 to 2 hours, and then heat-treated at 100 to 110° C. for 4 hours to obtain a potassium-containing manganese oxide fiber filter membrane, and the loading amount of manganese oxide catalytic material on the obtained Mn / PETP membrane is 13.5%. The prepared fiber filter membrane has a uniform loading of catalytic material, and the mass loss is ≤1% after 50 bending tests.
[0097] Test Example 2: Wind resistance test of fiber filter membrane
[0098] Take a piece of Mn / PETP film prepared in Example 1, place it in front of a fan and blow it continuously (wind speed is 2.7 m / s), record the mass change of the Mn / PETP film every 24 hours, and explore the structural stability of the prepared purification filter membrane under long-term wind blowing conditions when it is actually used in a purification device. The calculation method formula is the same as that of Test Example 1.
[0099] Figure 4 The wind blowing test and evaluation results of the carbon-doped manganese oxide fiber filter membrane prepared in Example 1 are shown in the figure. As can be seen from the figure, the mass of the present invention has not decreased after continuous wind blowing for 15 days, indicating that the carbon-doped manganese oxide fiber filter membrane provided by the present invention has excellent wind blowing resistance, and the carbon-doped manganese oxide catalyst immobilized on the membrane is not easy to fall off.
[0100] Test Example 3: Test on water resistance and self-cleaning performance of fiber filter membrane
[0101] Ash was used to simulate the dust deposited on the surface of the fiber filter membrane during the air purification application process. A piece of Mn / PETP membrane prepared in Example 1 was taken, and the ash was dispersed on the surface of the fiber filter membrane, and then rinsed with 500 mL of tap water. After the experiment was completed, the fiber filter membrane was dried, the surface morphology of the filter membrane was observed, and the mass change of the filter membrane before and after rinsing was recorded.
[0102] The experimental process is as follows Figure 5 As shown, it can be seen that the dust deposited on the surface of the fiber filter membrane can be easily washed away by only a small amount of water (~20mL). This is because the water contact angle of the surface of the prepared carbon-doped manganese oxide fiber filter membrane is 0°, showing super-hydrophilic properties, so the self-cleaning of the fiber filter membrane can be achieved by simple water washing. And after a large amount of water washing (500mL), the structure and loading amount of the carbon-doped manganese oxide catalytic material on the surface of the fiber filter membrane did not change significantly, indicating that the prepared fiber filter membrane has good water washing resistance.
[0103] Test Example 4: Formaldehyde catalytic purification performance test
[0104] The formaldehyde catalytic purification test experiment was carried out in a 9L box-type formaldehyde reactor. During the test process, the temperature in the reactor was kept at room temperature and the humidity was about 30%. The test samples were the Mn / PETP films prepared in Example 1 and Examples 6 to 8.
[0105] First, take 4 pieces of Mn / PETP membrane to be tested, put them into dry glass culture dishes, and cover the culture dishes containing fiber filter membrane samples tightly with glass sheets. Then put the sealed culture dishes into the bottom of the box-type formaldehyde reactor. Subsequently, inject 1 μL of formaldehyde solution (38wt%) onto the glass slide placed at the bottom of the reactor with a pipette, and turn on the fan with a power of 2.5W installed at the bottom of the reactor to speed up the flow balance of the gas in the reactor. After the formaldehyde solution is completely volatilized and the formaldehyde in the reactor reaches the adsorption / desorption equilibrium, the initial concentration of formaldehyde in the reactor is detected from the upper sampling port of the reactor with the British PPM-HTV formaldehyde detector, and the initial concentration is maintained at about 8ppm. Open the sealed culture dish with a glass rod from the upper sampling port of the reactor so that the filter membrane sample contacts formaldehyde, and the formaldehyde catalytic purification performance test begins. The formaldehyde concentration change is recorded at intervals during the test.
[0106] Depend on Figure 6It can be seen from a and b that the performance test results of the blank sample (BG) prove that the box-type formaldehyde reactor is well sealed, and the formaldehyde concentration does not change significantly during the entire reaction process. For the commercially available polymer film PET, the formaldehyde removal rate within 70 minutes is only 7.2%. As for the carbon-doped manganese oxide fiber filter membrane prepared in Example 1, as the test progresses, the formaldehyde concentration drops rapidly. Within 15 minutes, the carbon-doped manganese oxide fiber filter membrane can catalytically purify and remove 90.6% of the formaldehyde, and the formaldehyde removal rate reaches 95.9% within 70 minutes. After calculation, the CADR value per unit mass of the carbon-doped manganese oxide fiber filter membrane prepared in Example 1 is 1.06m 3 / h·g. It is also found that the heat treatment temperature has a great influence on the formaldehyde purification performance of the Mn / PETP film. In order to ensure efficient formaldehyde purification performance, the heat treatment temperature should be controlled within 100°C, preferably within 60°C.
[0107] Table 3 Summary of formaldehyde removal rate within 70 min
[0108] Example 1 Example 6 Example 7 Example 8 Formaldehyde removal rate 95.9% 88.6% 76.9% 69.8%
[0109] Repeat the above test process to test the formaldehyde catalytic purification performance of the carbon-doped manganese oxide fiber filter membrane prepared in Example 1 at different ambient temperatures. The results are shown in Figure 7 , 8℃, 23℃ and 40℃ respectively simulate the ambient temperature of spring, summer, autumn and winter in actual application. The test results show that in the range of 8~40℃, the prepared carbon-doped manganese oxide fiber filter membrane exhibits a fast and efficient catalytic purification effect on formaldehyde.
[0110] The above results show that the fiber filter membrane prepared in the embodiment of the present invention has excellent structural stability and fast and efficient low-temperature catalytic formaldehyde purification performance.
[0111] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a highly stable fiber filter membrane for low-temperature catalytic oxidation of formaldehyde, It is characterized in that The steps include: 1) dispersing a manganese salt in deionized water, adding a reducing agent and or not adding an element doping material, performing a low-temperature reduction reaction to obtain a manganese oxide compound precursor, and then dispersing the precursor in deionized water to obtain a manganese oxide compound precursor suspension; 2) immersing the hydrophobic fiber filter membrane in a polydiallyldimethylammonium chloride solution, taking out the filter membrane, and drying it at a certain temperature to obtain a hydrophobic fiber filter membrane modified with polydiallyldimethylammonium chloride; 3) placing the hydrophobic fiber filter membrane modified with polydiallyldimethylammonium chloride in a suspension of a manganese oxide compound precursor, taking it out after immersion for a period of time, and obtaining the fiber filter membrane after drying and heat treatment.
2. The preparation method according to claim 1, It is characterized in that The concentration of the polydiallyldimethylammonium chloride solution is 0.05-1.0 wt %.
3. The preparation method according to claim 1, It is characterized in that The manganese salt is selected from one or more of manganese permanganate, manganese nitrate, manganese sulfate and manganese acetate; The hydrophobic fiber filter membrane is selected from microporous polymer fiber filter membrane.
4. The preparation method according to claim 1, It is characterized in that In step 3), the heat treatment temperature is 40 to 120° C., and the heat treatment time is 6 to 24 hours.
5. The preparation method according to claim 1, It is characterized in that In step 3), the loading amount of the manganese oxide compound on the fiber filter membrane is 8 to 13 wt%.
6. The preparation method according to claim 1, It is characterized in that In step 2), the immersion time is 10 to 120 minutes; In step 3), the immersion time is 5 to 30 minutes.
7. A fiber filter membrane for low-temperature catalytic oxidation of formaldehyde, It is characterized in that The preparation is obtained by the preparation method according to any one of claims 1 to 6.
8. Use of the fiber filter membrane as claimed in claim 7 in low-temperature purification of formaldehyde.
9. Filter membrane for air purification, It is characterized in that Comprising the fiber filter membrane as claimed in claim 7.
10. Air purification device, It is characterized in that Comprising the fiber filter membrane as claimed in claim 7.
Citation Information
Patent Citations
Air cleaning material, and preparation method and application thereof
CN103480267A
Nitrogen-doped carbon-coated manganese monoxide composite material with one-dimensional porous core-shell structure and preparation method of nitrogen-doped carbon-coated manganese monoxide composite material
CN105470481A
Nanofiber membrane material for low-temperature catalytic oxidation of formaldehyde and preparation method and application thereof
CN113231108A
Method for preparing Mn-based composite catalyst by using organic waste liquid and application of Mn-based composite catalyst in decomposition of indoor formaldehyde
CN113976107A
Method for purifying industrial wastewater by using silica fiber aerogel loaded with manganese oxide as ozone oxidation catalyst
WO2022236649A1