Recyclable microporous rubber foam material and recycling method thereof

By introducing reversible dynamic metal ion coordination bonds and supercritical fluid foaming technology into rubber, the problem of difficult recycling of rubber foam is solved, and the efficient recycling and excellent mechanical properties of microporous rubber foam is achieved. It is suitable for many industrial fields. .

CN119081253APending Publication Date: 2024-12-06黄埔绿色先进材料技术研究院 +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411423154.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing rubber foam materials are difficult to recycle during processing, resulting in environmental pollution and energy waste. The recycling and processing process of microporous rubber foam is complex and has poor controllability.

Method used

By introducing reversible dynamic metal ion coordination bonds into the rubber, the dynamic fracture and recombination of metal ion coordination bonds are used, and combined with supercritical fluid foaming technology, the recycling and utilization of microporous rubber foam is achieved. The specific steps include molding and foaming processes, and multiple cycles are recovered using the ‘crumbing-molding-foaming’ method.

Benefits of technology

It realizes efficient recycling of microporous rubber foam, maintains regular cell structure, excellent expansion ratio and mechanical properties, and is suitable for aerospace, automobile and other fields, meeting the needs of green industry development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081253A_ABST
    Figure CN119081253A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and discloses a recyclable microporous rubber foam material and a preparation method, application and recycling method thereof based on a supercritical fluid foaming technology. The microporous rubber foam material is prepared from the following components in parts by mass: 70 to 95 parts of epoxidized rubber and 5 to 30 parts of metal salt. The foam material can be prepared through a supercritical fluid foaming technology, the foam structure is controllable, the mechanical property is excellent, the expansion rate is 1.8-2.9, the foam size is 4.4-9.0 microns, the foam density is 2.3-3.5 * 10 < 8 > / cm < 3 >, and the elongation at break is as high as 710%. Metal ions are introduced into epoxidized rubber, metal ion coordination is constructed, reversibly-crosslinked rubber is obtained, recycling of microporous rubber foam is achieved, and the regenerated microporous rubber foam material obtained through multiple times of recycling still has a uniformly-distributed foam structure and excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a recyclable microporous rubber foam material and a preparation method and application thereof based on supercritical fluid foaming technology, and a recycling method thereof. Background Art

[0002] Rubber foam materials combine the high elasticity of rubber with the advantages of light weight and heat insulation of foam, and are widely used in aerospace, automobile, construction, packaging and other fields. However, the existing rubber foam preparation methods (such as chemical foaming method, solvent foaming method, etc.) are difficult to match the rubber vulcanization and foaming process, and there are problems such as uncontrollable pore size, poor mechanical properties, chemical residues that damage product quality, and environmental pollution. In this context, the use of green and environmentally friendly supercritical fluid foaming technology with simple and controllable process to introduce microporous structure into rubber can eliminate chemical residues and achieve effective regulation of pore size and foam performance.

[0003] The preparation of microporous rubber foam by supercritical fluid foaming includes four processes: pre-vulcanization, saturation, pressure relief foaming, and post-vulcanization. By adjusting the foaming process parameters (temperature, pressure, time, etc.) and the matrix formula, the rubber vulcanization and foaming processes can be balanced, and the pore structure of the microporous rubber foam can be regulated. Zheng et al. (Industrial and Engineering Chemistry Research, 2020, 59: 1534-1548) changed the content of vulcanizer (di-tert-butyl peroxyisopropylbenzene) in ethylene propylene diene monomer (EPDM) and found that the foaming temperature window of EPDM with a micro-cross-linked structure was expanded from 40-80°C of pure EPDM to 100-200°C, and the foaming ratio was increased from 5.6 to 7.1; while the fully cross-linked EPDM no longer has melt recovery capability. Liao et al. (RSCAdvances, 2015, 5: 106981; Materials and Design, 2017, 133: 288-298) prepared silicone rubber with a pore size as low as 1.1 μm and a pore density as high as 1.25×10 10 Pieces / cm 3 Silicone rubber foam.

[0004] However, in the above processing, the microporous rubber foam is covalently cross-linked by a vulcanizing agent (diisopropylbenzene peroxide, sulfur, etc.) to form a permanent network, making it difficult to recycle and process, causing environmental pollution and energy waste. The introduction of reversible dynamic cross-linking can give the rubber matrix the ability to recycle and process. Under the stimulation of certain external conditions, the reversible dynamic bonds in the rubber matrix "break" and "reorganize", causing the rubber molecular chains to dynamically exchange and reorganize, thereby realizing rubber recycling processing by regulating process parameters such as temperature. Guo et al. (ACS Sustainable Chemistry and Engineering, 2019, 7: 11712-11720) introduced exchangeable β-hydroxy esters into EPDM / carbon black composites, and used the rearrangement of the covalent cross-linked network at high temperature to achieve the recycling of the rubber composite. However, since the processing process of microporous rubber foam is far more complicated than that of the rubber matrix, the cross-linking and foaming processes must be balanced in the rubber foaming, the operation is cumbersome and the controllability is poor. At present, there are almost no reports on the recycling of lightweight, high-performance microporous rubber foam. Therefore, the recycling and processing of high-performance microporous rubber foams through reversible dynamic cross-linking and green and controllable supercritical fluid foaming technology will meet the needs of green industrial development. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the rubber foam in the prior art that is difficult to recycle, the primary purpose of the present invention is to provide a microporous rubber foam material that can be recycled.

[0006] The material of the present invention can realize the recycling of microporous rubber foam by introducing reversible dynamic metal ion coordination bonds into rubber and utilizing the dynamic breaking and reorganization of metal ion coordination bonds. The microporous rubber foam material of the present invention has excellent mechanical properties, with an expansion ratio of 1.8-2.9, a cell size of 4.4-9.0 μm, and a cell density of 2.3-3.5×10 8 Pieces / cm 3 , the elongation at break is as high as 710%.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned microporous rubber foam material based on supercritical fluid foaming technology.

[0008] The microporous rubber foam material of the invention can be prepared by supercritical fluid foaming technology, has controllable pore structure and excellent mechanical properties.

[0009] Another object of the present invention is to provide an application of the above-mentioned microporous rubber foam material.

[0010] Another object of the present invention is to provide a recycling method for the above-mentioned microporous rubber foam material.

[0011] The material of the present invention introduces a reversible dynamic metal ion coordination bond, and utilizes the reversible characteristics of the metal ion coordination bond to achieve recycling through "crushing-molding-foaming". The recycling method of the present invention has a simple and easy recycling process, does not require the use of organic solvents and special processing equipment, and has high recycling efficiency; the recycled microporous rubber foam maintains a regular pore structure and presents a closed-cell morphology. After multiple re-circulation recycling treatments, the pore size is still at the micron level and maintains excellent mechanical properties.

[0012] The purpose of the present invention is achieved through the following solutions:

[0013] In a first aspect, the present invention provides a recyclable microporous rubber foam material, which is prepared based on supercritical fluid foaming technology and includes the following components in parts by weight: 70-95 parts of epoxidized rubber and 5-30 parts of metal salt.

[0014] Preferably, the epoxy value of the epoxidized rubber may be 20-75%.

[0015] Preferably, the epoxidized rubber can be purchased directly, or can be obtained by introducing epoxy groups into the carbon-carbon double bonds of the rubber by oxidation with peroxy acid.

[0016] Preferably, the rubber can be selected from one of natural rubber, isoprene rubber, styrene-butadiene rubber, EPDM rubber and the like.

[0017] Preferably, the metal salt is a soluble metal salt, and the metal cation may be Fe 3+ , Cu 2+ 、Zn 2+ Mg 2+ 、Ag + At least one of the above.

[0018] The microporous rubber foam material of the present invention has excellent mechanical properties, an expansion ratio of 1.8-2.9, a cell size of 4.4-9.0 μm, and a cell density of 2.3-3.5×10 8 Pieces / cm 3 , the elongation at break is as high as 710%.

[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned microporous rubber foam material, which is a preparation method based on supercritical fluid foaming technology, comprising the following steps:

[0020] (1) Molding: Epoxidized rubber latex and metal salt are mixed evenly, dried, and hot-pressed to obtain a rubber sheet containing metal ion coordination bonds;

[0021] (2) Foaming: Place the rubber sheet in a high-pressure foaming kettle and seal it, introduce a supercritical fluid, heat it to 80-150°C, maintain it at a pressure of 10-30 MPa for 0.5-8 hours, and quickly release the pressure to obtain microporous rubber foam.

[0022] In step (1), the parameters of the hot pressing may be 10-30 MPa pressure, 100-180° C., and 10-40 min.

[0023] In step (1), the solid content of the epoxidized rubber latex can be 20-60wt%. In the preparation method of the present invention, the required epoxidized rubber latex is first obtained according to the amount of epoxidized rubber in the material, and then mixed with the metal salt to make the metal salt evenly distributed in the epoxidized rubber before tableting and foaming.

[0024] In step (2), the rapid pressure relief can quickly release the pressure within 5 seconds, reducing the pressure to atmospheric pressure.

[0025] In step (2), the supercritical fluid may be any one of CO2, N2, etc.

[0026] The microporous rubber foam material of the invention can be prepared by supercritical fluid foaming technology, has controllable pore structure and excellent mechanical properties.

[0027] Thirdly, the microporous rubber foam material of the present invention has controllable pore structure and excellent mechanical properties, and can be applied to aerospace, automobile, construction, packaging and other fields.

[0028] In a fourth aspect, the present invention also provides a recycling method for the above-mentioned microporous rubber foam material, by crushing the microporous rubber foam material as a raw material and repeating the molding and foaming processes of the preparation method to obtain the recycled microporous rubber foam material.

[0029] Preferably, the crushing can be performed by shearing or other operations to make the material fragments smaller than or equal to 1×1 cm 2 .

[0030] In the present invention, metal ions are introduced into the epoxidized rubber to construct the metal ion coordination effect, thereby obtaining reversibly cross-linked rubber; the reversibly cross-linked microporous rubber foam is prepared by using supercritical fluid foaming technology; the reversible characteristics of the metal ion coordination effect and the dynamic breaking and reorganization of the metal ion coordination bonds are utilized to achieve the recycling effect of the microporous rubber foam through "crushing-molding-foaming".

[0031] In a fifth aspect, the present invention also provides a regenerated microporous rubber foam material obtained by the above-mentioned recycling method.

[0032] The microporous rubber foam material of the present invention can be recycled for multiple cycles, and the regenerated microporous rubber foam material obtained by one or more cycles of recycling still has a uniformly distributed pore structure and excellent mechanical properties, and its expansion ratio is 1.3-2.9, the pore size is 4.4-9.0 μm, and the pore density is 1.4-3.5×10 8 Pieces / cm 3 , the elongation at break is as high as 710%.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0034] (1) The present invention provides a microporous rubber foam material, which is prepared by supercritical fluid foaming technology by introducing metal ion coordination into the rubber matrix. The raw materials used are simple and easy to obtain, and the latex is directly derived from the traditional rubber industry. The metal ions are rich in variety and simple in composition, and no chemical modification and complex treatment are required; the preparation process is simple and environmentally friendly, and the pore structure can be regulated within a certain range by adjusting the process parameters of supercritical fluid foaming (such as saturation temperature, saturation pressure and saturation time, etc.), and it has universal applicability; the pore structure of the obtained microporous rubber foam is regular, presenting a closed-cell morphology, and the pore size reaches the micrometer level, and has excellent mechanical properties.

[0035] (2) The present invention provides a recycling method for microporous rubber foam, which utilizes the reversible characteristics of metal ion coordination bonds to achieve recycling through "crushing-molding-foaming". The recycling process is simple and easy, does not require the use of organic solvents and special processing equipment, and has high recycling efficiency; the recycled microporous rubber foam maintains a regular pore structure, presents a closed-cell morphology, the pore size is still at the micron level, and maintains excellent mechanical properties. The recycling method is universal and has important significance for the green development of the rubber industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 It is a recycling process for microporous rubber foam materials.

[0038] Figure 2-Figure 3 The SEM image and cell size distribution diagram of the microporous rubber foam material obtained in Example 1.

[0039] Figure 4The SEM image and pore size distribution diagram of the microporous rubber foam material recovered once in the cycle obtained in Example 5.

[0040] Figure 5 The SEM image and cell size distribution diagram of the 4-cycle recycled microporous rubber foam material obtained in Example 6.

[0041] Figure 6 This is the SEM image of the rubber material obtained in Comparative Example 1. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. The materials involved in the following examples can be obtained from commercial channels unless otherwise specified. The methods described are conventional methods unless otherwise specified. The epoxy value of the epoxidized rubber used in the present invention can be 20-75%. For the convenience of comparison, the following examples all use epoxidized rubber with an epoxy value of 35-45%.

[0043] Example 1

[0044] Epoxidized natural rubber latex (ENR) with a solid content of 20-60 wt% is blended in a mass ratio of ENR dry rubber mass: ferric chloride = 90:10, dried, and hot-pressed at a pressure of 15 MPa and 150° C. for 30 min to obtain a rubber sheet containing a metal ion coordination bond;

[0045] The obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 hour, then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample is placed in an ice water bath to shape, thereby obtaining a microporous rubber foam material.

[0046] Example 2

[0047] Epoxidized natural rubber latex (ENR) with a solid content of 20-60 wt% is blended in a mass ratio of ENR dry rubber mass: copper chloride = 70:30, dried, and hot-pressed at a pressure of 30 MPa and 100° C. for 40 min to obtain a rubber sheet containing a metal ion coordination bond;

[0048] The obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 hour, then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample is placed in an ice water bath to shape, thereby obtaining a microporous rubber foam material.

[0049] Example 3

[0050] Epoxidized ethylene propylene diene monomer rubber latex (eEPDM) with a solid content of 20-60 wt % is blended in a mass ratio of eEPDM dry rubber mass: ferric chloride = 95:5, dried, and hot-pressed at a pressure of 10 MPa and 180° C. for 10 min to obtain a rubber sheet containing a metal ion coordination bond;

[0051] The obtained sheet was placed in a high-pressure foaming kettle and sealed, supercritical N2 was introduced, the temperature was raised to 80°C, and maintained at this temperature and a pressure of 30 MPa for 8 hours, then the pressure was quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample was placed in an ice water bath for shaping to obtain a microporous rubber foam material.

[0052] Example 4

[0053] Epoxidized natural rubber latex (ENR) with a solid content of 20-60 wt% is blended in a mass ratio of ENR dry rubber mass: ferric chloride = 90:10, dried, and hot-pressed at a pressure of 15 MPa and 150° C. for 30 min to obtain a rubber sheet containing a metal ion coordination bond;

[0054] The obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 150°C, and maintained at this temperature and a pressure of 10 MPa for 0.5 h, then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample is placed in an ice water bath to shape, thereby obtaining a microporous rubber foam material.

[0055] Example 5

[0056] The microporous rubber foam prepared in Example 1 was cut into pieces with a size of less than 1×1 cm. 2 The fragments are hot-pressed at a pressure of 15 MPa and 150°C for 30 min to obtain a recycled rubber sheet; the obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 h, and then the pressure is quickly released within 5 seconds to drop to atmospheric pressure, the expanded sample is placed in an ice water bath for shaping, and a 1-cycle recycled microporous rubber foam material is obtained. Figure 1 It is a recycling process for microporous rubber foam materials.

[0057] Example 6

[0058] The microporous rubber foam prepared in Example 1 was cut into pieces with a size of less than 1×1 cm. 2The fragments are hot-pressed at a pressure of 15 MPa and 150°C for 30 min to obtain a recycled rubber sheet; the obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 h, and then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, the expanded sample is placed in an ice water bath for shaping, and a recycled microporous rubber foam material is obtained, which is then crushed, and the "crushing-molding-foaming" process is repeated for a total of 4 times to obtain 4 recycled microporous rubber foam materials.

[0059] Comparative Example 1

[0060] Drying epoxidized natural rubber latex (ENR) with a solid content of 20-60 wt%, and hot pressing at a pressure of 15 MPa and 150° C. for 30 min to obtain a rubber sheet;

[0061] The obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 hour, and then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample is placed in an ice water bath to shape, thereby obtaining a rubber material.

[0062] Comparative Example 2

[0063] Epoxidized natural rubber latex (ENR) with a solid content of 20-60 wt % is blended in a mass ratio of ENR dry rubber mass: vulcanizing agent DCP = 98:2, dried, and hot-pressed at a pressure of 15 MPa and 150° C. for 5 min to obtain a rubber sheet;

[0064] The obtained sheet is placed in a high-pressure foaming kettle and sealed, supercritical CO2 is introduced, the temperature is raised to 120°C, and maintained at this temperature and a pressure of 15 MPa for 1 hour, then the pressure is quickly released within 5 seconds to reduce the pressure to atmospheric pressure, and the expanded sample is placed in an ice water bath to shape, thereby obtaining a covalently cross-linked microporous rubber foam.

[0065] Cut the above microporous rubber foam into pieces with a size of less than 1×1 cm 2 The fragments were hot-pressed at 15 MPa pressure and 150°C for 5 minutes to obtain recycled rubber sheets. Observation of the rubber sheets showed that the fragments could not be completely connected and reshaped, and they remained fragments after hot pressing. A few of the bonded pieces were accompanied by obvious "weld marks".

[0066] The microporous rubber foams prepared in Examples 1-4, the recycled microporous rubber foams prepared in Examples 5-6, and the rubber material obtained in the comparative example were observed using SEM, and the cell size and cell density of the microporous rubber foams were calculated using Image-Pro Plus 6 graphics processing software. The results are shown in FIG. Figure 2-Figure 6 , Table 1.

[0067] The tensile properties (according to ASTM D638-2003 standard, tensile rate of 500 mm / min) of the microporous rubber foams prepared in the above Examples 1-4, the recycled microporous rubber foams prepared in Examples 5-6, and the rubber material obtained in the comparative example were tested, and the results are listed in Table 2.

[0068] Table 1

[0069]

[0070] Note: Comparative Example 2 recovered fragments, no data.

[0071] Table 2

[0072]

[0073] Note: Comparative Example 2 recovered fragments, no data.

[0074] Depend on Figure 1 It can be seen that in the recycling process of "crushing-molding-foaming", the surface of the sample is smooth and flat after shredding and re-molding, without obvious cracks, indicating that its recycling performance is excellent. Figure 2-Figure 5 It can be seen that the microporous rubber foam materials prepared by the present invention have formed a stable and uniform pore structure, the pore size is micron-level, elliptical, closed-cell, regular structure, and few defects. This shows that the present invention introduces metal ion coordination bonds to construct a reversible cross-linking structure, uses supercritical fluid foaming technology to obtain microporous rubber foam, and realizes the recycling of microporous rubber foam through "crushing-molding-foaming". Figure 6 It can be seen from the SEM image that no cellular structure is formed in Comparative Example 1, indicating that the uncrosslinked rubber cannot be successfully foamed.

[0075] As can be seen from Table 1, the foaming ratio of the microporous rubber foam material of the present invention is 1.3-2.9, the cell size is 4.4-9.0 μm, and the cell density is 1.4-3.5×10 8 Pieces / cm 3. It can be seen from Table 2 that, compared with the rubber without a cellular structure in Comparative Example 1, the tensile properties of the microporous rubber foam material of the present invention are not significantly reduced, but improved. Compared with Comparative Example 1, the tensile strength of the microporous rubber foam material of the present invention can be increased by 70%, and the elongation at break is increased by 46%. This is because the cellular structure of the microporous rubber foam material of the present invention is regular and has few defects. The presence of micropores does not reduce the strength of the material, but can passivate the crack tip, effectively prevent the crack from expanding, and maintain or even improve the mechanical properties of the rubber; at the same time, the introduced metal ion coordination bond acts as a sacrificial bond, which can effectively dissipate energy, is conducive to eliminating stress concentration, and promotes the orientation of rubber molecular chains, thereby improving the mechanical properties. This shows that the microporous rubber foam material of the present invention and the recycled microporous rubber foam material both have a regular microporous foam structure and excellent mechanical properties.

[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A recyclable microporous rubber foam material, characterized in that The invention comprises the following components in parts by weight: 70-95 parts of epoxidized rubber and 5-30 parts of metal salt.

2. The recyclable microporous rubber foam material according to claim 1, characterized in that The epoxy value of the epoxidized rubber is 20-75%.

3. The recyclable microporous rubber foam material according to claim 1, characterized in that: The metal salt is a soluble metal salt.

4. The recyclable microporous rubber foam material according to claim 1, characterized in that: In the metal salt, the metal cation includes Fe 3+ , Cu 2+ 、Zn 2+ Mg 2+ 、Ag + At least one of .

5. A method for preparing the recyclable microporous rubber foam material according to any one of claims 1 to 4, which is a method based on supercritical fluid foaming technology, characterized in that The following steps are involved: (1) Molding: Epoxidized rubber latex and metal salt are mixed evenly, dried, and hot-pressed to obtain a rubber sheet containing metal ion coordination bonds; (2) Foaming: Place the rubber sheet in a high-pressure foaming kettle and seal it, introduce a supercritical fluid, heat it to 80-150°C, maintain it at a pressure of 10-30 MPa for 0.5-8 hours, and quickly release the pressure to obtain microporous rubber foam.

6. The preparation method according to claim 5, characterized in that: In step (1), the parameters of the hot pressing are 10-30 MPa pressure, 100-180° C., and 10-40 min.

7. The preparation method according to claim 5, characterized in that: In step (1), the solid content of the epoxidized rubber latex is 20-60wt%.

8. Application of the recyclable microporous rubber foam material according to any one of claims 1 to 4 in the fields of aerospace, automobile, construction and packaging.

9. A method for recycling the recyclable microporous rubber foam material according to any one of claims 1 to 4, characterized in that The regenerated microporous rubber foam material is obtained by crushing the microporous rubber foam material as a raw material and repeating the molding and foaming processes of the preparation method.

10. A regenerated microporous rubber foam material obtained based on the recycling method according to claim 9.

Citation Information

Cited By

  • Self-repairing rubber foaming material capable of being reprocessed and recycled

    CN119798811A

  • A self-healing, reprocessable, and recyclable rubber foam material

    CN119798811B