Preparation method of ultrathin cast film tape and cast film tape production system
Through the pulse fluctuation and parallel beam drying technology of the airbag-type pulse damper buffering slurry supply system, the problems of uneven thickness and uneven drying of cast film belt are solved, and high-quality ceramic cast film belt production is realized. In the large-scale production of ultra-thin products.
Patent Information
- Application Number
- CN202411077968.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-05
AI Technical Summary
In the existing casting process, the pulse fluctuation of the slurry supply system results in uneven thickness of the ceramic casting film belt, and the drying technology is difficult to ensure the quality of ultra-thin products. The wind patterns caused by hot air drying and the heating plate drying lead to edge cracks or warping. question.
The pulse pressure fluctuation of the slurry supply system is buffered by airbag pulse damper and dried by parallel beam irradiation. The irradiation temperature, width and cast film belt movement rate are controlled to ensure slurry stability and dry uniformity.
The cast film tape is uniform in thickness and high appearance pass rate, avoids the air pattern problems caused by hot air drying, and controls the heating temperature in real time, which is suitable for the large-scale production of ultra-thin ceramic cast film tape.
Smart Images

Figure BDA0004982896680000081 
Figure BDA0004982896680000082 
Figure BDA0004982896680000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of casting, and in particular relates to a method for preparing an ultra-thin cast film tape and a cast film tape production system. Background Art
[0002] Chip ceramic capacitors (MLCC) are gradually developing towards the modern direction of miniaturization and high capacitance. The preparation process must first go through powder slurry, casting, printing, lamination, cutting, debinding sintering, and external electrode preparation to obtain MLCC products of different specifications. Especially for ultra-thin layer MLCC products, the quality of the ceramic cast film tape obtained in the casting process is crucial to the subsequent processes and product qualification rate.
[0003] The casting process generally uses a slurry supply system to transport the prepared slurry to the casting knife, and the ceramic casting film tape of the required thickness is obtained by setting the casting knife parameters, and the casting film tape is dried to make its surface initially dry and solidify. The slurry dispersion, slurry supply stability and drying effect directly determine the quality of the resulting casting film tape. The gear pump used in the slurry supply system realizes slurry supply by meshing to change the cavity pressure, but its pulsed fluctuation makes the slurry supply stability poor, affecting the thickness consistency of the casting film tape; especially when using slurry with a high solid content for casting, its poor fluidity and dispersibility are easy to lead to further deterioration of the coating consistency and other quality. After reducing the solid content to improve the slurry fluidity and dispersibility, it is not conducive to the subsequent drying process and the preparation of ultra-thin specification products. The commonly used drying technologies include drying the cast film tape with hot air or drying it by adding a heating plate under the cast film tape. However, in actual use, the air drying method will leave local protrusions or depressions on the film surface due to the wind ripples caused by the hot air, which is very likely to cause poor appearance such as uneven thickness. The heating plate drying method cannot control the heating rate of the edge and middle parts of the cast film tape in real time. If the drying time is too long or the heating temperature is too high, cracks or warping may occur at the edge. Otherwise, the drying effect cannot be achieved. Therefore, it is difficult to adjust the local temperature according to the real-time drying conditions of the film, which is not conducive to the large-scale production of ceramic cast film tapes and the quality assurance of ultra-thin cast film tapes. Summary of the invention
[0004] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a method for preparing a cast film tape.
[0005] A second object of the present invention is to provide a ceramic product.
[0006] A third object of the present invention is to provide a cast film tape production system.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A first aspect of the present invention provides a method for preparing a cast film tape, comprising the following steps:
[0009] S1: preparing a cast film tape by allowing the slurry transported by the slurry supply system to be buffered by an airbag pulse damper, wherein the airbag pressure in the airbag pulse damper is P, 0.01MPa≤P≤0.05MPa;
[0010] S2: moving the cast film tape at a speed of 40 to 150 m / min and irradiating the cast film tape with a parallel light beam to dry the cast film tape;
[0011] The irradiation temperature of the parallel light beam is 30-100°C;
[0012] The irradiation width of the parallel light beam is 300 to 500 mm;
[0013] The irradiation direction of the parallel light beam is perpendicular to the moving direction of the cast film tape.
[0014] In the present invention, when the airbag pressure in the airbag pulse damper is 0.01MPa~0.05MPa, for example, it can be selected from 0.01MPa, 0.015MPa, 0.02MPa, 0.025MPa, 0.03MPa, 0.035MPa, 0.04MPa, 0.045MPa, and 0.05MPa. Under the above-mentioned airbag pressure, the pulse pressure fluctuations generated when the slurry supply system transports the slurry can be buffered, thereby ensuring the stability of the slurry when preparing the cast film tape, thereby obtaining a cast film tape with good thickness uniformity. If the airbag pressure in the airbag pulse damper is too low (i.e. less than 0.01MPa) or there is no pressure, the gas in the airbag cannot replenish the pressure of the slurry supply system and cannot stabilize the pressure; if the airbag pressure in the airbag pulse damper is too high (i.e. greater than 0.05MPa), the gas pressure in the airbag is too high and cannot absorb the pressure fluctuations of the slurry supply system, resulting in failure to play a buffering role, thereby causing poor stability of the slurry during cast film and inconsistent thickness of the cast film tape.
[0015] The present invention uses a parallel light beam to dry the cast film tape, and synchronously controls the irradiation temperature, irradiation width and movement speed of the cast film tape during the drying process, so that the surface of the cast film tape will not be uneven due to hot air ripples, which is conducive to obtaining a high-quality cast film tape with good surface flatness and uniform thickness. Specifically:
[0016] If the irradiation temperature of the parallel light beam is too low (i.e., less than 30°C), it only has a preheating effect, and the rapid drying and curing process of the organic solvent or resin component in the cast film cannot be achieved. Insufficient drying in the early stage causes uneven thickness and the appearance of the cast film is prone to poor; if the irradiation temperature of the parallel light beam is too high (i.e., greater than 100°C), the slurry is cured in a very short time, which hinders the natural spreading process of the slurry during casting, resulting in the cast film being thick in the middle and thin around. In severe cases, it may even cause local vacancies in the cast film, resulting in poor quality of the cast film. Therefore, the irradiation temperature in the present invention is 30 to 100°C, for example, it can be selected from 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, and 100°C. At the above irradiation temperature, it is conducive to obtaining a cast film with good thickness uniformity and excellent appearance.
[0017] If the irradiation width of the parallel light beam is narrow (i.e. less than 300mm) or the movement speed of the cast film tape is fast (i.e. greater than 150m / min), the heating time for the moving cast film tape is insufficient, affecting the quality of the cast film tape; if the irradiation width is wide (i.e. greater than 500mm) or the movement speed of the cast film tape is slow (i.e. less than 40m / min), it causes unnecessary energy waste and is not conducive to improving production efficiency. Therefore, the irradiation width in the present invention is 300-500mm, and the movement speed of the cast film belt is 40-150m / min. For example, the irradiation width can be selected from 300mm, 310mm, 320mm, 330mm, 340mm, 350mm, 360mm, 370mm, 380mm, 390mm, 400mm, 410mm, 420mm, 430mm, 440mm, 450mm, 460mm, 470mm, 480mm, 490mm, 500mm, and the movement speed of the cast film belt can be selected from 40m / min, 45m / min, 50m / min, 60m / min, 70m / min, 80m / min, 90m / min, 100m / min, 110m / min, 120m / min, 130m / min, 140m / min, 150m / min, 160m / min, 170m / min, 180m / min, 190m / min, 200m / min, 210m / min, 220m / min, 230m / min, 240m / min, 250m / min, 260m / min, 270m / min, 280m / min, 290m / min, 300m / min, 310 in, 55m / min, 60m / min, 65m / min, 70m / min, 75m / min, 80m / min, 85m / min, 90m / min, 95m / min, 100m / min, 105m / min, 110m / min, 115m / min, 120m / min, 125m / min, 130m / min, 135m / min, 140m / min, 145m / min, 150m / min, under the above irradiation width and movement rate of the cast film tape, it is conducive to obtaining high quality cast film tape with high production efficiency.
[0018] Preferably, the thickness of the cast film tape is 8 to 20 μm.
[0019] Preferably, the irradiation temperature of the parallel light beam is 50-80°C.
[0020] Preferably, the irradiation width of the parallel light beam is 350-450 mm.
[0021] Preferably, the movement speed of the cast film tape is 70 to 120 m / min.
[0022] Preferably, the ratio of the irradiation width of the parallel light beam to the movement speed of the cast film tape is 3.75×10 -3 ~5×10 -3 min.
[0023] The second aspect of the present invention provides a ceramic product, comprising a cast film tape produced by the preparation method described in the first aspect of the present invention.
[0024] Preferably, the ceramic product comprises a chip ceramic capacitor.
[0025] The third aspect of the present invention provides a cast film tape production system, which is used to implement the preparation method described in the first aspect of the present invention, and the cast film tape production system includes a slurry supply system and a drying device; the slurry supply system includes a conveying pump and an airbag pulse damper; the drying device includes a parallel beam lighting lamp.
[0026] Preferably, the slurry supply system comprises a supply tank, a delivery pump, a filter, an airbag pulse damper and a casting knife which are arranged in sequence. When the slurry supply system of the present invention is used, the prepared slurry is first stored in the slurry supply tank, and then delivered to the filter by the delivery pump for filtration to remove larger solid particles in the slurry, and then reaches the casting knife position under the cushioning effect of the airbag of the airbag pulse damper, and is scraped into a casting film strip with a certain thickness by the casting knife, and then the casting film strip is dried by the drying device.
[0027] The present invention adds an airbag pulse damper between the filter and the casting knife in the slurry supply system. Compared with the traditional gear pump directly supplying slurry, the airbag pulse damper can eliminate the pulse pressure fluctuations generated by the delivery pump in the slurry supply system when the slurry is delivered. The airbag pulse damper is used to compress the airbag to achieve the function of balancing the pressure when the pressure in the entire slurry supply system is too high. When the pressure in the system decreases, the gas in the airbag expands to supplement the pressure, thereby achieving the function of balancing the slurry supply pressure, improving the slurry supply stability, and ensuring the consistency of the subsequent casting thickness.
[0028] The drying device in the present invention adopts a parallel beam lighting lamp, and cooperates with the set parameters of irradiation temperature, irradiation width and movement speed of the cast film tape to solidify and shape the cast film tape without affecting the casting quality, thereby improving its thickness uniformity. It not only avoids the adverse effects of hot air patterns caused by traditional wind blowing methods, but also realizes real-time regulation of the heating temperature of the cast film tape, and does not cause the problem of local excessive heating of the cast film tape. At the same time, it can ensure that there will be no abnormal drying phenomenon, which is beneficial to the large-scale production of cast film tapes and the quality assurance of ultra-thin cast film tapes.
[0029] Preferably, the delivery pump is a gear pump.
[0030] Preferably, the parallel beam illumination lamp is a parallel single beam light source. A parallel beam illumination lamp refers to a light source that emits parallel and non-divergent light.
[0031] Preferably, the number of the parallel beam lighting lamps is two, and the two parallel beam lighting lamps are respectively located on both sides of the width direction of the cast film strip and are relatively parallelly arranged, and the irradiation direction of the two parallel beam lighting lamps is perpendicular to the vertical plane where the movement direction of the cast film strip is located.
[0032] Preferably, the number of the parallel beam illumination lamp is one, and the parallel beam illumination lamp is arranged directly above the cast film strip in the vertical direction, and the irradiation direction of the parallel beam illumination lamp is perpendicular to the horizontal plane where the movement direction of the cast film strip is located.
[0033] The beneficial effects of the present invention are as follows: the preparation method of the present invention uses an airbag pulse damper to buffer the pulse pressure fluctuations generated by the slurry transported by the slurry supply system, thereby ensuring the stability of the slurry during the casting preparation process, and at the same time cooperates with a parallel light beam to locally irradiate the cast film tape for drying, thereby obtaining a high-quality cast film tape with good thickness uniformity, high appearance qualification rate, and no defects such as cracks and wind marks on the surface, which is suitable for large-scale production of ultra-thin ceramic cast film tapes. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the structure of the cast film tape production system in an embodiment of the present invention.
[0035] Figure 2 It is a schematic diagram of the structure of the drying device in Examples 1 to 11 and Comparative Examples 1 to 4 of the present invention; wherein A is a top view and B is a side view.
[0036] Figure 3 It is a schematic diagram of the structure of the drying device in Example 12 of the present invention; wherein A is a top view and B is a side view.
[0037] Figure 4 This is a schematic diagram of the structure of the drying device in Comparative Example 6 of the present invention.
[0038] Figure 5 It is a schematic diagram of the structure of the drying device in comparative example 7 of the present invention.
[0039] Reference numerals:
[0040] Cast film belt 1, casting knife 2, lighting lamp 3. DETAILED DESCRIPTION
[0041] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0042] The specific structure of the cast film tape production system used in the embodiments and comparative examples of the present invention is as follows: Figure 1 As shown, the cast film tape production system includes a slurry supply system and a drying device. The slurry supply system includes a feed tank, a gear pump, a filter, an airbag pulse damper and a cast knife connected in sequence. The feed tank is used to store ceramic slurry. The outlet of the feed tank is connected to the inlet of the gear pump through a pipeline. The gear pump is used to transport ceramic slurry. The outlet of the gear pump is connected to the inlet of the filter through a pipeline. The filter is used to filter and remove large particles of solid in the ceramic slurry. The outlet of the filter is connected to the inlet of the airbag pulse damper. The ceramic slurry reaches the cast knife position under the airbag buffering effect of the airbag pulse damper. The airbag pulse damper is used to balance the pressure fluctuations that may occur during the transportation of the ceramic slurry. The ceramic slurry is scraped by the cast knife 2 to form a cast film tape, and then dried by the drying device. The drying device includes using a light lamp 3 for drying. The light lamp 3 is a parallel beam light lamp.
[0043] In one embodiment of the present invention, the drying device includes two lighting lamps 3, which are respectively arranged on both sides of the width direction of the cast film strip 1 and the two lighting lamps 3 are arranged relatively parallel, and the irradiation direction of the lighting lamp 3 is perpendicular to the vertical plane where the movement direction of the cast film strip 1 is located. The two lighting lamps 3 use parallel light beams. Figure 2 As shown, Figure 2 A and Figure 2 B are the top view and side view of the drying device respectively.
[0044] In one embodiment of the present invention, the drying device includes a light lamp 3, which is arranged directly above the cast film strip 1 in the vertical direction, and the irradiation direction of the light lamp 3 is perpendicular to the horizontal plane where the moving direction of the cast film strip is located, and the light lamp 3 uses a parallel light beam, specifically as follows Figure 3 As shown, Figure 3 A and Figure 3 B are the top view and side view of the drying device respectively.
[0045] The width of the lamp is recorded as a, which is Figure 2 , Figure 3 or Figure 4 The width of the red area in the figure is X, the speed of the cast film strip is X, and the ratio of the light width to the speed of the cast film strip is a / X, with a unit of 10 -3 min.
[0046] The specific implementation of the present invention is further described in detail below with reference to the embodiments:
[0047] The thickness of the cast film tapes prepared in Examples 1 to 12 of the present invention and Comparative Examples 1 to 7 is all 10 μm.
[0048] Example 1
[0049] This example provides a method for preparing an ultra-thin cast film tape, comprising the following preparation steps:
[0050] (1) The ceramic slurry in the feed tank is transported to the filter through a gear pump for filtration, and then reaches the casting knife position under the cushioning effect of the airbag of the airbag pulse damper, and is scraped by the casting knife to form a casting film strip with a thickness of 10 μm; the airbag pressure of the airbag pulse damper is 0.03 MPa;
[0051] (2) The cast film belt moves to the drying device (using Figure 2 The ultra-thin cast film strip is dried in the drying device in the drying device to obtain the ultra-thin cast film strip. The irradiation temperature of the light lamp 3 is 60°C, and the light irradiation width a (is Figure 2 The width of the red area is 400 mm, and the speed of the cast film belt is 100 m / min. -1 , the ratio of a to X is 4×10 -3 min, the number of lighting lamps 3 is 2.
[0052] The parameters of the airbag pressure, irradiation temperature, irradiation width, cast film strip movement speed, number of irradiation lamps, etc. in this example are all recorded in Table 1 below.
[0053] Example 2
[0054] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the air bag pressure in this example is 0.01 MPa, and the other process parameters in this example are shown in Table 1.
[0055] Example 3
[0056] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the air bag pressure in this example is 0.05 MPa, and the other process parameters in this example are shown in Table 1.
[0057] Example 4
[0058] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 30° C., and the other process parameters in this example are shown in Table 1.
[0059] Example 5
[0060] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 50° C., and the other process parameters in this example are shown in Table 1.
[0061] Example 6
[0062] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 80° C., and the other process parameters in this example are shown in Table 1.
[0063] Example 7
[0064] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 100° C., and the other process parameters in this example are shown in Table 1.
[0065] Example 8
[0066] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation width a in this example is 300 mm, and the movement speed X of the cast film tape is 40 m·min -1 , the ratio of a / X is 7.5×10 -3 min, other process parameters in this example are shown in Table 1.
[0067] Example 9
[0068] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation width a in this example is 500 mm, and the moving speed X of the cast film tape is 150 m·min -1 , the ratio of a / X is 3.33×10 -3 min, other process parameters in this example are shown in Table 1.
[0069] Example 10
[0070] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation width a in this example is 350 mm, and the moving speed X of the cast film tape is 70 m·min-1 , the ratio of a / X is 5×10 -3 min, other process parameters in this example are shown in Table 1.
[0071] Embodiment 11
[0072] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation width a in this example is 450 mm, and the movement speed X of the cast film tape is 120 m·min -1 , the ratio of a / X is 3.75×10 -3 min, other process parameters in this example are shown in Table 1.
[0073] Example 12
[0074] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that: Figure 3 The drying device is used for drying, the number of the light lamp 3 is 1, and other process parameters in this example are shown in Table 1.
[0075] Comparative Example 1
[0076] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that: there is no airbag pulse damper in this example, that is, the airbag pressure is 0 MPa. The other process parameters in this example are shown in Table 1.
[0077] Comparative Example 2
[0078] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the air bag pressure in this example is 1 MPa, and the other process parameters in this example are shown in Table 1.
[0079] Comparative Example 3
[0080] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 25° C., and the other process parameters in this example are shown in Table 1.
[0081] Comparative Example 4
[0082] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that the irradiation temperature in this example is 110° C., and the other process parameters in this example are shown in Table 1.
[0083] Comparative Example 5
[0084] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that no drying device is used for drying in this example. Other process parameters in this example are shown in Table 1.
[0085] Comparative Example 6
[0086] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that: Figure 4 The drying device in the drying process is used for drying, and the drying device includes a light lamp 3, which is arranged on one side of the width direction of the cast film strip; the angle between the irradiation direction of the light lamp 3 and the horizontal plane where the movement direction of the cast film strip is located is an acute angle.
[0087] Comparative Example 7
[0088] The preparation method of the ultra-thin cast film tape in this example is different from that in Example 1 only in that: Figure 5 The drying device in the drying process is used for drying, and the drying device includes a light lamp 3, which is arranged on one side of the width direction of the cast film belt; the light lamp 3 uses non-parallel scattered light.
[0089] Table 1 Process parameters in the preparation methods of Examples 1 to 12 and Comparative Examples 1 to 5
[0090]
[0091] Performance Testing
[0092] According to the test items, test instruments and test methods described in Table 2 below, the slurry supply stability and the quality of the cast film tape (thickness uniformity, appearance qualification rate) of the preparation methods of Examples 1 to 12 and Comparative Examples 1 to 7 were tested respectively, and the test results are recorded in Table 3 below.
[0093] Table 2 Test items, test instruments and test methods
[0094]
[0095]
[0096] Table 3 Test results of slurry supply stability and cast film tape quality in Examples 1 to 12 and Comparative Examples 1 to 7
[0097] Pressure fluctuation / % thickness / % Appearance / % Example 1 1.5 1.9 98.5 Example 2 1.7 2.5 96.5 Example 3 1.9 2.6 96.5 Example 4 1.5 2.0 95.1 Example 5 1.5 2.0 97.8 Example 6 1.5 2.2 97.5 Example 7 1.5 2.7 95.5 Example 8 1.5 2.7 96.8 Example 9 1.5 2.6 97.0 Example 10 1.5 2.1 98.3 Embodiment 11 1.5 2.1 98.1 Example 12 1.5 2.0 98.3 Comparative Example 1 2.5 3.2 94.5 Comparative Example 2 2.2 3.3 94.7 Comparative Example 3 1.5 2.8 90.7 Comparative Example 4 1.5 3.8 93.2 Comparative Example 5 1.5 2.3 90.5 Comparative Example 6 1.5 2.5 94.3 Comparative Example 7 1.5 2.5 94.7
[0098] It can be seen from Table 3 that, compared with Comparative Examples 1 to 7, the process parameters such as the airbag pressure, irradiation temperature, irradiation width, and cast film tape movement speed in Examples 1 to 12 are all within the range defined by the present invention, and all have high slurry supply stability, the slurry supply pressure fluctuation is less than 2%, the thickness change of the cast film tape is within 3%, the appearance qualification rate is greater than 95%, and there is no cracking, warping, texture, uneven convexity and concave appearance defect; the specific analysis is as follows:
[0099] In Example 1, by setting parameters such as airbag pressure, irradiation temperature, irradiation width, and cast film strip movement speed, when the number of lamps is 2, the slurry supply stability is improved, the cast film strip thickness consistency and appearance qualification rate are high, and the cast film strip quality is better;
[0100] In Examples 2 to 3, the airbag pressure of the airbag pulse damper is set within the range specified in the present invention, the slurry supply stability is better, the thickness consistency and the appearance qualification rate are better;
[0101] In Examples 4 to 7, the irradiation temperature is set within the range specified by the present invention, and the thickness and appearance are better. In Examples 5 to 6, the irradiation temperature is within the preferred range, and the performance is better.
[0102] In Examples 8 to 11, the irradiation width a and the moving speed X of the cast film tape are set within the range defined by the present invention, wherein a / X in Examples 10 to 11 is within the preferred range, and the quality of the cast film tape is better;
[0103] In Example 12, one irradiation lamp 3 is used for drying, and the thickness consistency and appearance of the cast film tape obtained are good.
[0104] In Comparative Example 1, no airbag pulse damper was used, and there was no pressure replenishment during the ceramic slurry supply process, which affected the subsequent casting process. The airbag pressure in Comparative Example 2 was 1 MPa, which was too high to buffer the pulsation during the ceramic slurry supply process, resulting in poor slurry supply stability and poor quality of the resulting cast film tape.
[0105] Comparative Examples 3 to 4 set the irradiation temperature outside the range specified by the present invention, which cannot achieve the effect of real-time drying, and the thickness uniformity and / or appearance qualification rate of the cast film tapes obtained are poor;
[0106] Comparative Example 5 is set to be the case where lamp drying is not used and only an airbag pulse damper is added. The slurry supply stability is good, but the problem of poor thickness and appearance of the cast film tape cannot be solved.
[0107] In comparative example 6, the irradiation direction of light is not perpendicular to the horizontal plane where the film strip moves. Comparative example 7 uses scattered light, which also leads to the same situation. Both fail to improve the quality of the cast film strip.
[0108] To sum up, the preparation method of the present invention uses an airbag pulse damper to buffer the pulse pressure fluctuations generated during the slurry transportation process, and at the same time cooperates with a parallel light beam to irradiate the cast film tape for drying, thereby achieving a good regulating effect on the slurry supply stability before casting and the drying process of the cast film tape after casting. Compared with the traditional casting preparation and drying process, the slurry supply stability, the thickness uniformity of the cast film tape and the appearance qualification rate are simultaneously improved, and it is suitable for the large-scale production of ultra-thin ceramic cast film tapes.
[0109] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing a cast film tape, Features: The following steps are involved: S1: preparing a cast film tape by allowing the slurry transported by the slurry supply system to be buffered by an airbag pulse damper, wherein the airbag pressure in the airbag pulse damper is P, 0.01MPa≤P≤0.05MPa; S2: moving the cast film tape at a speed of 40 to 150 m / min and irradiating the cast film tape with a parallel light beam, drying the cast film tape; The irradiation temperature of the parallel light beam is 30-100°C; The irradiation width of the parallel light beam is 300 to 500 mm; The irradiation direction of the parallel light beam is perpendicular to the moving direction of the cast film tape.
2. The method for preparing a cast film tape according to claim 1, Features: The ratio of the irradiation width of the parallel light beam to the movement speed of the cast film tape is 3.75×10 -3 ~5×10 -3 min.
3. The method for preparing a cast film tape according to claim 1, Features: The irradiation width of the parallel light beam is 350-450 mm; and / or the movement speed of the cast film tape is 70-120 m / min.
4. The method for preparing a cast film tape according to claim 1, Features: The irradiation temperature of the parallel light beam is 50-80°C.
5. A ceramic product, Features: The invention comprises a cast film tape produced by the preparation method according to any one of claims 1 to 4.
6. The ceramic product according to claim 5, Features: The ceramic product includes a chip ceramic capacitor.
7. A cast film tape production system, Features: The cast film tape production system is used to implement the preparation method described in any one of claims 1 to 4, and the cast film tape production system includes a slurry supply system and a drying device; the slurry supply system includes a delivery pump and an airbag pulse damper; the drying device includes a parallel beam lighting lamp.
8. The cast film tape production system according to claim 7, Features: The slurry supply system comprises a supply tank, a delivery pump, a filter, an airbag type pulse damper and a casting knife which are arranged in sequence.
9. The cast film tape production system according to claim 7, Features: There are two parallel beam lighting lamps, which are respectively located on both sides of the width direction of the cast film strip and are arranged relatively parallel. The irradiation direction of the two parallel beam lighting lamps is perpendicular to the vertical plane where the movement direction of the cast film strip is located.
10. The cast film tape production system according to claim 7, Features: The number of the parallel beam illumination lamp is one, and the parallel beam illumination lamp is arranged directly above the cast film strip in the vertical direction, and the irradiation direction of the parallel beam illumination lamp is perpendicular to the horizontal plane where the moving direction of the cast film strip is located.