Carbon-coated graphite composite material as well as preparation method and application thereof
By using tanninic acid in an alkaline environment to react with crosslinking agent to form a carbon coating, the problem of improving the cycle rate performance of graphite negative electrode materials of lithium-ion batteries is solved, and green and environmentally friendly and low-cost coating modification is achieved. It is suitable for Industrial production has improved battery performance.
Patent Information
- Application Number
- CN202410821135.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-05
Smart Images

Figure CN118894527A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of lithium-ion batteries, and in particular to a carbon-coated graphite composite material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of light weight, high energy density, high output voltage, high charging efficiency, long cycle life, low self-discharge rate, high safety and environmental friendliness. Therefore, they are widely used in many fields such as portable electronic devices, electric vehicles and energy storage. Graphite is the most commonly used negative electrode material for lithium-ion batteries. It has the advantages of low voltage, good electrical conductivity, high energy density, low price and abundant resources, which makes it occupy the main market share of lithium-ion battery negative electrode materials. However, there are still some defects in the graphite negative electrode of lithium-ion batteries: (1) The diffusion pathway of lithium ions when embedded in graphite is from the layered edge to the interior of the material, resulting in Li + The diffusion path is long, and due to the poor isotropy of graphite and the small interlayer spacing (0.335nm), the insertion of lithium ions is hindered, limiting its rate performance; (2) The structure between graphite layers is connected by weak van der Waals forces. + During the embedding process, the co-intercalation of solvent molecules will cause the graphite layer to fall off, causing the SEI layer on the surface of the graphite particles to rupture, and then a new SEI layer will be generated, consuming the electrolyte, increasing the internal resistance, and causing the graphite negative electrode to age and fail; (3) Under high current charge and discharge conditions, the Li + A large concentration difference will cause serious battery polarization, resulting in Li + Lithium deposits on the surface of graphite negative electrode to form lithium dendrites, which affects battery performance and life and causes certain safety hazards. Therefore, in order to improve the cycle performance and capacity of the battery, it is necessary to coat and modify the graphite surface.
[0003] At present, the common methods for graphite surface coating modification are solvent method and solid phase mixing method. The solvent method uses a large amount of organic solvent, which is costly and pollutes the environment; while the solid phase mixing method cannot guarantee the uniformity of coating, and the performance improvement of the obtained product is limited. CN103072974A discloses a method for coating the surface of an artificial graphite carbon negative electrode material, comprising: using an in-situ polymerization coating method, firstly adding the artificial graphite to a certain concentration of H2O2, rapidly stirring at a stirring speed of 200-500rpm for a stirring time of 0.5-2h, and then filtering and washing; then adding the oxidized artificial graphite to a certain concentration of phenol solution, heating and stirring at a heating temperature of 70-100°C, a stirring speed of 200-500rpm, and a stirring time of 10-60min; then dripping a formaldehyde solution according to a stoichiometric ratio, adding a hydrochloric acid solution after the dripping is completed, controlling the pH value of the solution to 1.9-2.3, and stirring again for 0.5-2h; then adding an appropriate amount of hexamethylenetetramine (urotropine) to cure the phenolic resin, and after the curing is complete, washing and separating to obtain a sample, and then drying and carbonizing the sample in sequence to obtain a uniformly coated modified artificial graphite negative electrode material. Although the above method can ensure the uniformity and integrity of the coating, the process is complicated, the cost is high, and it is not suitable for industrial production.
[0004] Therefore, how to provide a coating modification method that can not only improve the cycle rate performance of the graphite negative electrode, but also be green, environmentally friendly, low-cost and simple in process flow has become a problem that needs to be solved urgently. Summary of the invention
[0005] In order to solve the above technical problems, the present disclosure provides a carbon-coated graphite composite material and a preparation method and application thereof. The preparation method has a simple process, is green and environmentally friendly, has a low reaction cost at room temperature, and can effectively improve the cycle rate performance of the graphite negative electrode, and has good application prospects.
[0006] In a first aspect, the present disclosure provides a method for preparing a carbon-coated graphite composite material, the preparation method comprising the following steps:
[0007] (1) preparing an alkaline solution;
[0008] (2) mixing an organic carbon source, a cross-linking agent and the alkaline solution obtained in step (1) to obtain a mixed solution; the organic carbon source comprises tannic acid;
[0009] (3) mixing graphite with the mixed solution obtained in step (2), and then performing solid-liquid separation; the obtained solid is dried and sintered in sequence to obtain a carbon-coated graphite composite material.
[0010] In the present disclosure, tannic acid (TA) is a substance containing a 1,2-benzenediol structure. In an aerobic alkaline environment, tannic acid will automatically undergo an oxidative polymerization reaction to form a dark brown amorphous polymer and adhere to the surface of the graphite substrate. During the reaction, the phenolic hydroxyl groups on the benzene ring of tannic acid are easily oxidized to quinones, and then undergo a disproportionate reaction with the remaining phenolic hydroxyl groups to generate semiquinone free radicals. These free radicals further react with a cross-linking agent to gradually form an isotropically growing tannic acid-cross-linking agent framework, which is eventually covered on the surface of the graphite substrate to form a complete and uniform coating layer. The resulting tannic acid-cross-linking agent polymer-coated graphite material is then sintered to obtain a carbon-coated graphite composite material (G@C). Tannic acid, as a plant polyphenol, is widely available, low in cost, green and environmentally friendly, and suitable for industrial production.
[0011] The following are preferred technical solutions of the present disclosure, but are not intended to be limitations of the technical solutions provided by the present disclosure. Through the following technical solutions, the technical objectives and beneficial effects of the present disclosure can be better achieved and realized.
[0012] As a preferred technical solution of the present disclosure, the specific steps of preparing the alkaline solution in step (1) include: mixing the solvent with the alkaline substance, adjusting the pH to 8-10, such as 8.5, 8.7, 8.9, 9, 9.2, 9.4 or 10, etc., but not limited to the listed values, and other values not listed within the range are also applicable.
[0013] In the present disclosure, an alkaline environment is conducive to the complete and uniform coating of graphite by tannic acid in the later stage. If the pH value is too low, that is, the reaction is carried out in a neutral or acidic environment, the tannic acid itself cannot undergo an oxidative polymerization reaction, and a coating layer cannot be formed on the surface of the graphite substrate, resulting in the inability to improve the cycle rate performance of the carbon-coated graphite composite material (G@C) after sintering.
[0014] As a preferred technical solution of the present disclosure, the solvent includes anhydrous ethanol and water.
[0015] Preferably, in the solvent, the volume ratio of anhydrous ethanol to water is 1:(2-5), such as 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or 1:5, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0016] In the present disclosure, the use of anhydrous ethanol is beneficial to improving the dispersibility of graphite and making the graphite surface coated more evenly.
[0017] Preferably, the alkaline substance includes any one of ammonia water, ammonium carbonate or ammonium bicarbonate, or a combination of at least two of them, such as a combination of ammonia water and ammonium carbonate, a combination of ammonium carbonate and ammonium bicarbonate, and the like.
[0018] Preferably, the concentration of the aqueous ammonia is 20-30wt%, such as 20wt%, 22wt%, 24wt%, 26wt%, 28wt% or 30wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0019] As a preferred technical solution of the present disclosure, the cross-linking agent in step (2) includes formaldehyde.
[0020] Preferably, the cross-linking agent in step (2) comprises a formaldehyde solution with a concentration of 30-40wt%, for example, 30wt%, 32wt%, 34wt%, 36wt%, 38wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0021] In the present disclosure, the cross-linking agent is selected by taking formaldehyde as an example, which can form a methylene bridge between two tannic acid (TA) molecules. The methylene bridge randomly connects the tannic acid (TA) molecules and generates cross-links to form tannic acid-formaldehyde oligomers (nanospheres), and the resulting oligomers further grow to form an isotropically grown tannic acid-formaldehyde framework, which is conducive to achieving uniform coating of graphite.
[0022] Preferably, the molar ratio of the cross-linking agent to the organic carbon source in step (2) is (134-150):3, for example 134:3, 138:3, 140:3, 142:3, 144:3, 146:3, or 150:3, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0023] In order to ensure the final coating effect, the cross-linking agent needs to be added in excess, otherwise the graphite cannot be completely coated, which will affect the final cycle performance of the material.
[0024] As a preferred technical solution of the present disclosure, stirring is performed during the mixing process in step (2), and the stirring time is 0.5-2h, for example, 0.5h, 1h, 1.5h or 2h, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0025] As a preferred technical solution of the present invention, stirring is performed during the mixing process in step (3), and the stirring time is 20-30 hours, for example, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours or 30 hours, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0026] Preferably, the solid-liquid separation in step (3) comprises centrifugal separation.
[0027] Preferably, in step (3), washing is further performed between the solid-liquid separation and the drying.
[0028] Preferably, the drying in step (3) comprises freeze-drying.
[0029] As a preferred technical solution of the present disclosure, the sintering temperature in step (3) is 600-700°C, for example, 600°C, 620°C, 640°C, 680°C or 700°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0030] Preferably, the sintering time in step (3) is 1-4 h, such as 1 h, 2 h, 3 h or 4 h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0031] Preferably, the heating rate of the sintering in step (3) is 2-4°C / min, such as 2°C / min, 3°C / min or 4°C / min, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0032] Preferably, the sintering in step (3) is carried out under a protective atmosphere.
[0033] In a second aspect, the present disclosure provides a carbon-coated graphite composite material, wherein the carbon-coated graphite composite material is prepared by the preparation method described in the first aspect.
[0034] As a preferred technical solution of the present disclosure, in the carbon-coated graphite composite material, the thickness of the carbon coating layer is 5-10nm, for example, 5nm, 6nm, 7nm, 8nm, 9nm or 10nm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0035] In a third aspect, the present disclosure further provides an application of the carbon-coated graphite composite material as described in the second aspect, wherein the carbon-coated graphite composite material is used for preparing a negative electrode of a lithium-ion battery.
[0036] Compared with the prior art, the technical solution provided by the embodiments of the present disclosure has the following advantages:
[0037] The present invention uses green, environmentally friendly and low-cost tannic acid as a carbon source, and uses a cross-linking agent to uniformly coat it on the graphite surface, and then sintering to form a uniform and complete carbon coating layer, thereby effectively improving the cycle rate performance of the graphite negative electrode. The preparation process is simple, the economic benefit is high, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present disclosure and, together with the description, serve to explain the principles of the present disclosure.
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0040] Figure 1 This is a SEM image of the original graphite used in Comparative Example 1 of the present disclosure.
[0041] Figure 2 This is a SEM image of tannic acid-formaldehyde polymer-coated graphite in Example 1 of the present disclosure.
[0042] Figure 3 This is a SEM image of the carbon-coated graphite obtained in Example 1 of the present disclosure.
[0043] Figure 4 1 is the XRD diagram of the original graphite used in Comparative Example 1 of the present disclosure and the carbon-coated graphite obtained in Example 1.
[0044] Figure 5 1 is a Raman spectrum of the original graphite used in Comparative Example 1 of the present disclosure and the carbon-coated graphite obtained in Example 1.
[0045] Figure 6 This is a comparison chart of the cycle performance of the lithium ion batteries obtained in Comparative Example 1 and Example 1 of the present disclosure. DETAILED DESCRIPTION
[0046] In order to more clearly understand the above-mentioned objectives, features and advantages of the present disclosure, the scheme of the present disclosure will be further described below. It should be noted that the embodiments of the present disclosure and the features in the embodiments can be combined with each other without conflict.
[0047] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present disclosure may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present disclosure, rather than all of the embodiments.
[0048] The present disclosure provides a method for preparing a carbon-coated graphite composite material, the preparation method comprising the following steps:
[0049] (1) mixing 30 ml of anhydrous ethanol, 150 ml of water and 20-30 wt % ammonia water, and adjusting the pH to 9.5-10.5 to obtain an alkaline solution;
[0050] (2) mixing 510 mg of tannic acid and 1 ml of a 30-40 wt % formaldehyde solution with the alkaline solution obtained in step (1), and stirring for 0.5-2 h to obtain a mixed solution;
[0051] (3) Mixing graphite with the mixed solution obtained in step (2), stirring for 20-30h, wherein the mass ratio of graphite to tannic acid is controlled to be (0.16-1):1; then centrifuging to obtain tannic acid-formaldehyde low polymer coated graphite; the obtained tannic acid-formaldehyde polymer coated graphite is washed with deionized water, freeze-dried after washing, and sintered in a nitrogen atmosphere at 600-700°C for 1-4h after drying, wherein the heating rate is 2-4°C / min, and a carbon-coated graphite composite material is obtained after sintering, wherein the carbon-coated graphite composite material has a thickness of 5-10nm. Embodiments 1-3 respectively provide a method for preparing a carbon-coated graphite composite material, and the preparation method refers to the preparation method in the specific implementation manner, and the specific condition parameters are shown in Table 1.
[0052] Table 1
[0053]
[0054] Example 4
[0055] This embodiment provides a method for preparing a carbon-coated graphite composite material. The preparation method refers to the preparation method in Example 1, with the only difference being that in step (3), the mass ratio of graphite to tannic acid is 1.5:1, so that the thickness of the carbon coating layer in the carbon-coated graphite composite material is 3 nm.
[0056] Example 5
[0057] This embodiment provides a method for preparing a carbon-coated graphite composite material. The preparation method refers to the preparation method in Example 1, with the only difference being that in step (3), the mass ratio of graphite to tannic acid is 0.09:1, so that the thickness of the carbon coating layer in the carbon-coated graphite composite material is 30 nm.
[0058] Comparative Example 1
[0059] In this comparative example, the graphite used in Example 1, that is, the original graphite without carbon coating, is used as the negative electrode material.
[0060] The SEM image of the original graphite used in Comparative Example 1 is as follows: Figure 1 shown.
[0061] In Example 1, the SEM image of tannic acid-formaldehyde polymer coated graphite is as follows: Figure 2 As shown, the SEM image of the obtained carbon-coated graphite is as follows Figure 3 shown.
[0062] from Figure 1-Figure 3It can be seen that the surface morphology of the original graphite (G) is rough; the surface of the tannic acid-formaldehyde polymer-coated graphite (G@TAF) is smooth and has protrusions; the edge contour of the carbon-coated graphite (G@C) becomes sharp and the surface becomes relatively smooth and neat. This is because the graphite surface has a complete and uniform amorphous carbon coating, forming a core-shell structure particle.
[0063] The XRD patterns of the original graphite used in Comparative Example 1 and the carbon-coated graphite obtained in Example 1 are as follows: Figure 4 As shown. Figure 4 It can be seen that the two samples of original graphite (G) and carbon-coated graphite (G@C) show similar XRD patterns, with diffraction peaks at 26.4°, 42.2°, 44.4°, 54.5° and 77.2°, corresponding to the (002), (110), (101), (004) and (110) planes of graphite (JCPDF no.08-0415), which indicates that the coating modification treatment on the graphite surface does not destroy the typical structure of graphite. After carbon coating, the diffraction intensity of the (002) crystal plane diffraction peak of G@C decreases slightly, indicating a decrease in crystallinity. The decrease in crystallinity means that the surface morphology of graphite (G) has changed slightly, that is, an amorphous surface carbon coating is formed, which is different from the Figure 3 The results are consistent.
[0064] The Raman spectra of the original graphite used in Comparative Example 1 and the carbon-coated graphite obtained in Example 1 are as follows: Figure 5 As shown. Figure 5 It can be seen that the original graphite (G) and carbon-coated graphite (G@C) have two obvious peaks, the D band (1350cm -1 ) and G band (1580cm -1 ). The D band is disordered sp 2 The G band represents the defects in the carbon atom lattice. 2 Hybridized in-plane stretching is a special hallmark of graphitic carbon with high crystallinity or two-dimensional graphene-like structure.
[0065] The degree of graphitization of the sample can be quantified by the ratio of the intensity of the D band (ID) to the G band (IG) (ID / IG). The ID / IG intensity ratio of the original graphite (G) is 0.07, but after carbon coating, the D peak intensity in the original graphite (G) becomes stronger, and ID / IG increases to 0.86. This indicates that the surface of the graphite particles is coated with an amorphous carbon layer, which is similar to the Figure 4 The results are consistent.
[0066] Comparative Example 2
[0067] This comparative example provides a method for preparing a carbon-coated graphite composite material. The preparation method refers to the preparation method in Example 1, except that the pH is adjusted to 7 in step (1), so that a complete and uniform carbon coating layer cannot be formed in the obtained carbon-coated graphite composite material.
[0068] Comparative Example 3
[0069] This comparative example provides a method for preparing a carbon-coated graphite composite material. The preparation method refers to the preparation method in Example 1, with the only difference being that in step (1), the pH is adjusted to 5, so that a complete and uniform carbon coating layer cannot be formed in the obtained carbon-coated graphite composite material.
[0070] Comparative Example 4
[0071] This comparative example provides a method for preparing a carbon-coated graphite composite material. The preparation method refers to the preparation method in Example 1, with the only difference being that no cross-linking agent is added in step (2), that is, no formaldehyde solution with a concentration of 37wt% is added, so that a complete and uniform carbon coating layer cannot be formed in the obtained carbon-coated graphite composite material.
[0072] The negative electrode materials obtained in Examples 1-5 and Comparative Examples 1-4 and the original graphite (i.e., the graphite used in Example 1) were used to prepare the negative electrode, respectively, specifically comprising: fully mixing the active material (i.e., the negative electrode materials obtained in Examples 1-5 and Comparative Examples 1-4 and the original graphite), super P (SP) conductive additive, carboxymethyl cellulose (CMC) and styrene-butadiene rubber in a mass ratio of 95.5:1.5:1.5:1.5, dissolving in deionized water, and using magnetic stirring for 12 hours to form a slurry. The obtained slurry was cast-coated on a copper foil with a scraper. The obtained copper foil was dried in a blast drying oven at 80°C for 2 hours, and further dried in a vacuum oven at 120°C for 6 hours. Finally, the copper foil was cut into 12 mm pole pieces, and the density of the electrode material on the pole piece was 1.3 mg·cm -2 .
[0073] The negative electrode obtained above is used to assemble the battery: in an inert gas-protected glove box, the battery is assembled using a CR2025 battery shell, and the water and oxygen content in the glove box is required to be less than 0.5ppm. During the production process, metallic lithium is used as the counter electrode, the electrolyte is a mixed solution formed by dissolving 1 mol / L LiPF6 in a volume ratio of 1:1:1 dimethyl carbonate (DMC) / ethylene carbonate (EC) / ethyl methyl carbonate (EMC), and the diaphragm is a polypropylene microporous membrane (Celgard2400).
[0074] The lithium ion batteries obtained in Examples 1-5 and Comparative Examples 1-4 were subjected to cycle rate performance tests, and the test method included: leaving the assembled batteries at room temperature for 24 hours, and using a Neware battery test system to perform electrochemical performance tests. The cycle performance at a charge and discharge rate of 2C (1C = 360 mAh / g) was tested at room temperature (25°C ± 2°C), a voltage range of 0.05-2.0V, and a test result as shown in Table 2.
[0075] The comparison of the cycle performance between Comparative Example 1 and Example 1 at a charge and discharge rate of 2C is shown in the figure below: Figure 6 As shown. Figure 6 It can be seen that at a charge and discharge rate of 2C, the discharge capacity of the original graphite (G) is 65 mAh / g after 40 cycles, and the battery fails after 365 cycles; while the discharge capacity of the carbon-coated graphite (G@C) is 124 mAh / g after 40 cycles at a 2C rate, and the capacity retention rate is 95% after 380 cycles.
[0076] Here, capacity retention rate (%) = discharge specific capacity after 380 cycles / discharge specific capacity after 40 cycles.
[0077] Table 2
[0078]
[0079] As can be seen from Table 2, the lithium ion batteries prepared using the carbon-coated graphite composite materials disclosed in Examples 1-5 have good cycle performance, and the specific capacity is still above 100 mAh / g after 380 cycles, while the capacity retention rate is above 84%; and by controlling the reaction environment, sintering temperature, and the addition ratio of graphite to carbon source, the cycle performance of the lithium ion battery can be further improved, and the specific capacity is above 116 mAh / g after 380 cycles, while the capacity retention rate is above 95%.
[0080] Compared with Example 1, in the preparation process of Comparative Examples 2 and 3, the reaction environment is neutral or acidic, which results in the inability of tannic acid itself to undergo self-oxidative polymerization reaction, thereby making it impossible for the carbon source to achieve uniform coating of graphite, ultimately resulting in the inability to effectively improve the cycle rate performance of the battery.
[0081] Compared with Example 1, Comparative Example 4 does not add a cross-linking agent. The organic carbon source tannic acid can only self-polymerize in an alkaline environment to form crystals rather than spheres, thereby hindering the coating. Therefore, the graphite cannot be evenly and completely coated, thereby affecting the material properties.
[0082] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0083] The above description is only a specific embodiment of the present disclosure, so that those skilled in the art can understand or implement the present disclosure. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure will not be limited to the embodiments described herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a carbon-coated graphite composite material, characterized in that: The preparation method comprises the following steps: (1) preparing an alkaline solution; (2) mixing an organic carbon source, a cross-linking agent and the alkaline solution obtained in step (1) to obtain a mixed solution; the organic carbon source comprises tannic acid; (3) mixing graphite with the mixed solution obtained in step (2), and then performing solid-liquid separation; the obtained solid is dried and sintered in sequence to obtain a carbon-coated graphite composite material.
2. The preparation method according to claim 1, characterized in that: The specific steps of preparing the alkaline solution in step (1) include: mixing the solvent with the alkaline substance, and adjusting the pH to 8-10.
3. The preparation method according to claim 2, characterized in that: The solvent includes anhydrous ethanol and water; Preferably, in the solvent, the volume ratio of anhydrous ethanol to water is 1:(2-5); Preferably, the alkaline substance includes any one of ammonia water, ammonium carbonate or ammonium bicarbonate, or a combination of at least two of them.
4. The preparation method according to any one of claims 1 to 3, characterized in that The cross-linking agent in step (2) includes formaldehyde; Preferably, the molar ratio of the cross-linking agent to the organic carbon source in step (2) is (134-150):
3.
5. The preparation method according to any one of claims 1 to 4, characterized in that: Stirring is performed during the mixing process of step (2), and the stirring time is 0.5-2h.
6. The preparation method according to any one of claims 1 to 5, characterized in that: Stirring is performed during the mixing process of step (3), and the stirring time is 20-30 hours; Preferably, the solid-liquid separation in step (3) comprises centrifugal separation; Preferably, in step (3), washing is further performed between the solid-liquid separation and the drying; Preferably, the drying in step (3) comprises freeze-drying.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The mass ratio of the graphite in step (3) to the organic carbon source in step (2) is (0.16-1):
1.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The sintering temperature in step (3) is 600-700° C. Preferably, the sintering time in step (3) is 1-4h; Preferably, the heating rate of the sintering in step (3) is 2-4°C / min; Preferably, the sintering in step (3) is carried out under a protective atmosphere.
9. A carbon-coated graphite composite material, characterized in that: The carbon-coated graphite composite material is prepared by the preparation method according to any one of claims 1 to 8; Preferably, in the carbon-coated graphite composite material, the thickness of the carbon coating layer is 5-10 nm.
10. An application of the carbon-coated graphite composite material as claimed in claim 9, characterized in that: The carbon-coated graphite composite material is used for preparing the negative electrode of a lithium ion battery.
Citation Information
Cited By
Tannic acid-based hard carbon material as well as preparation method and application thereof
CN120987298A