Preparation method of amidoximation COFs (Covalent Organic Frameworks) material with double functions of adsorbing and detecting uranyl
By using 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzene triformaldehyde, the problems of uranium adsorption and detection in the prior art have been solved, and efficient adsorption and detection have been achieved. Bifunctional, material is synthesized at room temperature, environmentally friendly and has low detection limit.
Patent Information
- Application Number
- CN202411056692.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-02
AI Technical Summary
It is difficult for the prior art to achieve efficient adsorption and detection of uranium at the same time, especially in harsh environments, the conditions of traditional solvent thermal synthesis methods are harsh and it is difficult to achieve the development of dual-function materials.
Cyanolated COFs materials were prepared using 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetrialdehyde as raw materials, and modified by amidoximetallization to obtain a granule with both adsorption and detection functions. Aminoxime-formulated COFs materials are used to utilize ultrasonic mixing, standstill reaction and heating and stirring at room temperature to avoid the harsh conditions of traditional methods.
High selective adsorption and rapid kinetics of hexavalent uranium are achieved, the material is easy to recover and cycle, environmentally friendly, and can be used for fluorescence analysis and detection, with a low detection limit.
Smart Images

Figure CN118894975A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemistry and environmental technology, and in particular to a method for preparing an amidoximated COFs material with dual functions of adsorbing and detecting uranyl. Background Art
[0002] Uranium is a key element in the nuclear industry. Extracting uranium from the environment is conducive to the sustainable development of the energy industry. However, uranium is also a global environmental pollutant with combined radioactive and chemical toxicity. The main valence state of uranium under natural conditions is U(VI), which has the characteristics of strong mobility, high radioactivity, and high toxicity. In particular, its radiotoxicity, due to its extremely long decay process accompanied by the generation of gamma radiation, radio- and chemotherapy toxicity can lead to irreversible human health and survival problems. However, the harsh environment and abundant interfering ions are challenges faced by uranium detection and recovery.
[0003] Covalent organic framework materials are a class of crystalline porous materials with a periodic structure that can achieve a precise combination of organic structural units. COFs have shown great potential in the adsorption and separation of metal ions due to their structural diversity, regular pore structure and large specific surface area. COFs materials modified with amidoxime groups are star materials for uranium adsorption due to their high selectivity for uranium. However, the traditional solvothermal synthesis method requires harsh conditions, such as high temperature and long reaction time. Moreover, most of the COFs materials modified with amidoxime are used for the adsorption of uranium in a single way, and the development of COFs materials with dual functions of adsorption and detection still has certain challenges. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing an amidoximated COFs material having the dual functions of adsorbing and detecting uranyl, so as to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is to provide a method for preparing an amidoximated COFs material having the dual functions of adsorbing and detecting uranyl, the steps comprising:
[0007] Using 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetricarboxaldehyde as raw materials, cyanated COFs materials are obtained after reaction;
[0008] The cyanated COFs material is subjected to amidoximation modification to obtain the amidoximated COFs material having the dual functions of adsorbing and detecting uranyl.
[0009] Furthermore, the preparation steps of the cyanated COFs material include:
[0010] Ultrasonic mixing of 3,4-diaminobenzonitrile, 2-hydroxy-1,3,5-benzenetricarbaldehyde and acetonitrile to obtain a mixed solution;
[0011] Add acetic acid to the mixed solution and stir, and allow to react at room temperature. After the reaction is completed, centrifuge, wash, and vacuum dry to obtain a cyanated COFs material.
[0012] Preferably, the molar ratio of the 3,4-diaminobenzonitrile to 2-hydroxy-1,3,5-benzenetricarbaldehyde is 3:1-5.
[0013] Preferably, the concentration of acetic acid is 12M.
[0014] Preferably, the volume ratio of the acetic acid to the mixed solution is 7:50.
[0015] Preferably, the volume ratio of the sum of the molar amounts of the 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetricarboxaldehyde to acetonitrile is 4-8 mmol:250 mL.
[0016] Preferably, the ultrasonic mixing time is 5 to 10 minutes.
[0017] Preferably, the stirring time is 10 min.
[0018] Preferably, the static reaction time is 3 to 5 days.
[0019] Preferably, the washing is performed at least once using ethanol.
[0020] Further, the step of amidoximation modification comprises:
[0021] The cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate are mixed with ethanol and water, and heated and stirred for reaction under nitrogen protection. After the reaction is completed, the solid product is collected by centrifugation, washed and vacuum dried to obtain the amidoximated COFs material with the dual functions of adsorbing and detecting uranyl.
[0022] Preferably, the mass ratio of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate is 1:1-10:1-10.
[0023] Preferably, the ratio of the sum of the masses of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate to the sum of the volumes of ethanol and water is 3-21 g:300 mL.
[0024] Preferably, the volume ratio of ethanol to water is 9:1.
[0025] Preferably, the heating temperature is 70-90°C.
[0026] Preferably, the stirring time is 6 to 10 hours.
[0027] Preferably, the washing is performed by washing alternately with water and ethanol at least once.
[0028] The second technical solution of the present invention is to provide an amidoximated COFs material prepared by the above preparation method.
[0029] The third technical solution of the present invention is to provide an application of the above-mentioned amidoximated COFs material as an adsorption material for adsorbing uranium in water.
[0030] Furthermore, the application method steps are: adding the amidoximated COFs material as an adsorption material into a water body to adsorb and enrich hexavalent uranium, the adsorption time is 5-1440 minutes, the dosage is 10-100 mg / L, the pH of the water body is 2-12, and the adsorption temperature is 25-45°C.
[0031] The fourth technical solution of the present invention is to provide an application of the above-mentioned amidoximated COFs material in detecting uranium in water.
[0032] Furthermore, the application method comprises the following steps: adding the amidoximated COFs material to a solvent to prepare a stock solution with a concentration of 1 to 25 mg / L, adding a uranyl ion solution to the stock solution with a concentration of 0 to 30 μM, testing the fluorescence emission spectrum before and after adding uranyl ions in a fluorescence spectrophotometer to obtain a change in fluorescence emission intensity, plotting a curve of fluorescence emission intensity versus uranium concentration, and then detecting the concentration of uranium in water.
[0033] Preferably, the solvent is DMF, DMAc, ethanol, THF or water.
[0034] The present invention discloses the following technical effects:
[0035] The present invention first uses 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetricarboxaldehyde as raw materials to prepare a COFs material with a cyano group. The amidoximated COFs material with dual functions of adsorbing and detecting uranyl prepared by post-modification has high adsorption selectivity and fast adsorption kinetics for uranyl.
[0036] The prepared adsorption material of the invention has unique and excellent adsorption performance for hexavalent uranium, is easy to be recovered and recycled, and is environmentally friendly.
[0037] The material prepared by the invention is simple in method, uses environmentally friendly, non-toxic and harmless raw materials, has low cost, can be synthesized at room temperature, avoids the harsh conditions of traditional solvent thermal synthesis, and can also be used for fluorescence analysis to detect uranium with a low detection limit. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 is the SEM image of COF-AO, where a is low magnification and b is high magnification;
[0040] Figure 2 The infrared spectra of 2-hydroxy-1,3,5-benzenetricarboxaldehyde, 3,4-diaminobenzonitrile, COF-CN and COF-AO in Example 1;
[0041] Figure 3 This is the graph showing the variation of the adsorption amount of hexavalent uranium of different concentrations by COF-AO with the adsorption time;
[0042] Figure 4 This is the cyclic regeneration performance diagram of the adsorption process of COF-AO;
[0043] Figure 5 The graphs are the comparison of the adsorption amount of COF-AO for different metals in simulated seawater and the selectivity coefficient graphs of COF-AO for different metals, where a is the comparison graph of the adsorption amount and b is the selectivity coefficient graph.
[0044] Figure 6 Specific surface area and pore distribution diagram of COF-AO, where a is the specific surface area and b is the pore distribution;
[0045] Figure 7 is the solid NMR image of COF-AO and COF-CN;
[0046] Figure 8 The fluorescence excitation and emission spectra of COF-AO;
[0047] Fig. 9 The fluorescence emission spectra of COF-AO added to different uranium concentrations and the fluorescence emission spectra of COF-AO added to 0-30 μM UO2 2+ Fluorescence calibration curve within the concentration range, where a is the fluorescence emission spectrum and b is the fluorescence calibration curve. DETAILED DESCRIPTION
[0048] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0049] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0050] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0051] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0052] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0053] The raw materials and reagents used in the specific implementation of the present invention are all commercially available products.
[0054] Example 1
[0055] The preparation steps of the amidoximated COFs material with dual functions of adsorption and detection of uranyl are as follows:
[0056] S1. Ultrasonic mixing (5 min) of 3,4-diaminobenzonitrile, 2-hydroxy-1,3,5-benzenetricarboxaldehyde and acetonitrile in a dosage ratio of 3 mmol:2 mmol:250 mL to obtain a mixed solution;
[0057] S2, adding an acetic acid solution with an initial concentration of 12 M to the mixed solution, with the volume ratio of the acetic acid solution to the mixed solution being 7:50, stirring for 10 min, and standing at room temperature for 3 days. After the reaction is completed, centrifugation is performed, and the reaction product is washed with ethanol for multiple times, and vacuum dried at 60° C. for 24 hours to obtain a cyanated COFs material, which is recorded as COF-CN;
[0058] S3. Mix the cyanated COFs material, hydroxylamine hydrochloride, anhydrous potassium carbonate, anhydrous ethanol and ultrapure water in a ratio of 1g:2g:2g:270mL:30mL, stir and reflux under nitrogen protection, heat in an oil bath at 85°C for 8h. After the reaction is completed, centrifuge, wash the reaction product repeatedly with water and ethanol, and dry it in a vacuum at 60°C for 24h to obtain the amidoximated COFs material, recorded as COF-AO.
[0059] Example 2
[0060] Compared with Example 1, the only difference is that the mass ratio of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate is 1:1.5:2.
[0061] Example 3
[0062] Compared with Example 1, the only difference is that the mass ratio of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate is 1:2:1.5.
[0063] Example 4
[0064] Compared with Example 1, the only difference is that the molar ratio of 2-hydroxy-1,3,5-benzenetricarboxaldehyde to 3,4-diaminobenzonitrile is
[0066] Example 5
[0067] Compared with Example 1, the only difference is that the molar ratio of 2-hydroxy-1,3,5-benzenetricarboxaldehyde to 3,4-diaminobenzonitrile is 3:1.
[0068] Example 6
[0069] Compared with Example 1, the only difference is that the static reaction days in step S2 are 4 days.
[0070] Example 7
[0071] Compared with Example 1, the only difference is that the static reaction days in step S2 are 5 days.
[0072] Example 8
[0073] Compared with Example 1, the only difference is that the oil bath heating time in step S3 is 7 hours.
[0074] Example 9
[0075] Compared with Example 1, the only difference is that the oil bath heating time in step S3 is 9 hours.
[0076] Example 10
[0077] Compared with Example 1, the only difference is that the oil bath heating time in step S3 is 10 hours.
[0078] Comparative Example 1
[0079] The preparation steps of amidoximated COFs materials are as follows:
[0080] S1. Ultrasonic mixing (5 min) of terephthalonitrile, 1,3,5-tris-(4-formylphenyl)benzene, n-butanol and o-chlorodiphenyl in a ratio of 4 mmol:1 mmol:2.5 mL:22.5 mL to obtain a mixed solution;
[0081] S2. Then, the prepared mixed solution was subjected to three liquid nitrogen freeze-thaw cycles and sealed under vacuum. After heating at 120°C for three days, the wet solid was transferred and washed with tetrahydrofuran (THF) and ethanol Soxhlet extraction for 3 days. After vacuum drying at 100°C for 10 hours, the cyanated COFs material was obtained, which was recorded as HDU-102.
[0082] S3, HDU-102 (100 mg) was soaked in anhydrous ethanol (17.5 mL) for 20 min, and then reacted with hydroxylamine hydrochloride (0.445 g) and trimethylamine (0.9 mL) at 85 ° C for 6 h. Then, after washing with ethanol and ultrapure water, it was dried at room temperature to obtain the amidoximated COFs material, which was recorded as HDU-102-AO.
[0083] Test Example 1
[0084] Adsorption experiment:
[0085] The amidoximated COFs material prepared in Example 1 was added as an adsorbent into 50 mL of uranyl solution (concentration: 100 mg / L), and the adsorbent dosage was 0.5 mg, 1 mg or 2 mg.
[0086] Test Example 2
[0087] Detection experiment:
[0088] The amidoximated COFs materials prepared in Example 1 and Comparative Example 1 were added to DMF to prepare stock solutions of 1 mg / L, 5 mg / L, 10 mg / L, and 20 mg / L, and then mixed with uranyl ion solutions of different concentrations (0-30 μM), and the fluorescence emission spectra were measured on a fluorescence spectrophotometer.
[0089] When the amidoximated COF material prepared in Comparative Example 1 was added into DMF, no fluorescence phenomenon occurred.
[0090] Figure 1 The SEM image of COF-AO, where a is low magnification and b is high magnification. Figure 1It can be seen that the amidoximated COFs material has a porous rod-like structure, and the porous structure is conducive to the adsorption of uranium.
[0091] Figure 2 is the infrared spectra of 2-hydroxy-1,3,5-benzenetricarboxaldehyde, 3,4-diaminobenzonitrile, COF-CN and COF-AO in Example 1. Figure 2 It can be seen that -CHO (~1688cm -1 ) and the stretching vibration peak of -NH2 (~3440cm) in the monomer 3,4-diaminobenzonitrile -1 ) completely disappeared, and the vibration peak of C=N (~1644cm -1 ) shows a new characteristic peak, proving the successful synthesis of COF-CN. Compared with COF-CN, in the infrared spectrum of COF-AO, -CN (~2226cm -1 ) vibration peak disappeared, and CN (~1483cm -1 ) and NO(~931cm -1 ), proving the successful oximation of the amidine and indicating the successful synthesis of the material.
[0092] Figure 3 The adsorption amount of COF-AO for different concentrations of hexavalent uranium (concentrations of 25 mg / L, 50 mg / L, and 100 mg / L) varies with adsorption time. Figure 3 It can be seen that the COF-AO material can achieve a uranium adsorption of more than 229.9 mg / g within 45 min, with rapid adsorption kinetics (5.11 mg / g / min).
[0093] The COF-AO prepared in Example 1 was subjected to a cyclic regeneration experiment, the steps being: after the COF-AO first adsorbed uranium to reach adsorption equilibrium, a Na2CO3 solution with a pH of 11 was used as an eluent and stirred for 1 hour to regenerate the COF-AO. The resulting suspension was filtered and washed several times with ultrapure water. The resulting material was dried and used for another adsorption experiment. The results are shown in FIG. Figure 4 shown.
[0094] Figure 4 The performance diagram of the COF-AO adsorption cycle is shown in Figure 2. Figure 4 It can be seen that COF-AO as a uranium adsorbent still has strong adsorption performance after 5 cycles of regeneration, indicating that the adsorption material of the present invention has stable performance and high reuse rate.
[0095] The COF-AO prepared in Example 1 was subjected to a uranium adsorption experiment in simulated seawater to determine its adsorption effect on hexavalent uranium. The steps were as follows: a simulated seawater (UO2 2+ ,Ba 2+ ,Ca 2+ ,Cu 2+ ,Fe 3+ Mg 2+ , Na + ,VO3 - ), the concentration was 300μg / L, 2mg COF-AO was added, stirred and adsorbed for 24h, and tested by ICP-MS. The experimental results are as follows Figure 5 shown.
[0096] Figure 5 The adsorption amount comparison diagram of COF-AO for different metals in simulated seawater and the selectivity coefficient diagram of COF-AO for different metals are shown in Figure 1, where a is the adsorption amount comparison diagram and b is the selectivity coefficient diagram. Figure 5 It can be seen that after 24 h of adsorption in 1 L of simulated seawater, COF-AO has a high selectivity for uranium.
[0097] The COF-AO prepared in Example 1 was subjected to nitrogen adsorption-desorption test. The results are as follows: Figure 6 shown.
[0098] Figure 6 The specific surface area and pore distribution of COF-AO, where a is the specific surface area and b is the pore distribution. Figure 6 It can be seen that COF-AO has a mesoporous structure, and the porous structure is conducive to the adsorption of uranium.
[0099] The COF-AO and COF-CN prepared in Example 1 were 13 C solid nuclear magnetic test, the experimental results are as follows Figure 7 shown.
[0100] Figure 7 is the solid NMR image of COF-AO and COF-CN, Figure 7 It can be seen that in the solid state of COF-AO 13 In the CNMR spectrum, the cyano group at 107 ppm disappeared and was replaced by the amidoxime group at 161 ppm, confirming the conversion of the cyano group to the amidoxime group and demonstrating the successful synthesis of COF-AO.
[0101] The COF-AO prepared in Example 1 was subjected to fluorescence testing, and the experimental results are as follows: Figure 8 shown.
[0102] Figure 8The fluorescence excitation and emission spectra of COF-AO are shown in Figure 2. Figure 8 It can be seen that the optimal excitation wavelength of COF-AO is 220 nm, and the optimal emission wavelength is 465 nm.
[0103] The 1 mg / L COF-AO stock solution (2.7 mL) prepared in Example 1 was added to test solutions with different uranium concentrations (0-30 μM), and then fluorescence testing was performed.
[0104] Fig. 9 The fluorescence emission spectra of COF-AO added to different uranium concentrations and the fluorescence emission spectra of COF-AO added to 0-30 μM UO2 2+ Fluorescence calibration curve within the concentration range, where a is the fluorescence emission spectrum and b is the fluorescence calibration curve. Fig. 9 It can be seen that the fluorescence intensity of COF-AO weakens with the increase of uranium concentration until it is basically quenched.
[0105] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing an amidoximated COFs material having dual functions of adsorbing and detecting uranyl, characterized in that the steps include: Using 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetricarboxaldehyde as raw materials, cyanated COFs materials are obtained after reaction; The cyanated COFs material is subjected to amidoximation modification to obtain the amidoximated COFs material having the dual functions of adsorbing and detecting uranyl.
2. The preparation method according to claim 1, characterized in that: The preparation steps of the cyanated COFs material include: Ultrasonic mixing of 3,4-diaminobenzonitrile, 2-hydroxy-1,3,5-benzenetricarbaldehyde and acetonitrile to obtain a mixed solution; Add acetic acid to the mixed solution and stir, and allow to react at room temperature. After the reaction is completed, centrifuge, wash, and vacuum dry to obtain a cyanated COFs material.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the 3,4-diaminobenzonitrile to 2-hydroxy-1,3,5-benzenetricarboxaldehyde is 3:1-5; the volume ratio of the sum of the molar amounts of the 3,4-diaminobenzonitrile and 2-hydroxy-1,3,5-benzenetricarboxaldehyde to acetonitrile is 4-8 mmol:250 mL; the concentration of the acetic acid is 12 M; and the volume ratio of the acetic acid to the mixed solution is 7:
50.
4. The preparation method according to claim 2, characterized in that: The ultrasonic mixing time is 5 to 10 minutes; the stirring time is 10 minutes; and the static reaction time is 3 to 5 days.
5. The preparation method according to claim 1, characterized in that: The step of amidoximation modification comprises: The cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate are mixed with ethanol and water, and heated and stirred for reaction under nitrogen protection. After the reaction is completed, the solid product is collected by centrifugation, washed and vacuum dried to obtain the amidoximated COFs material with the dual functions of adsorbing and detecting uranyl.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate is 1:1-10:1-10; the ratio of the sum of the masses of the cyanated COFs material, hydroxylamine hydrochloride and anhydrous potassium carbonate to the sum of the volumes of ethanol and water is 3-21 g:300 mL; the volume ratio of ethanol and water is 9:
1.
7. The preparation method according to claim 5, characterized in that: The heating temperature is 70-90° C.; the stirring time is 6-10 hours.
8. An amidoximated COFs material obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the amidoximated COFs material as claimed in claim 8 as an adsorption material for adsorbing uranium in water.
10. Use of the amidoximated COFs material as claimed in claim 8 in detecting uranium in water.
Citation Information
Patent Citations
Amidoxime group modified MOF material and preparation method thereof
CN110479213A
Amino-amidoximino bifunctional super-crosslinked microporous uranium adsorbent and preparation method thereof
CN111804285A
Amidoxime functionalized covalent organic framework and graphene oxide hybrid aerogel as well as preparation method and application thereof
CN115624922A
Preparation method and adsorption application of amidoxime functionalized three-dimensional covalent organic framework
CN115677959A
Preparation of amidoximation magnetic MXene-based composite material and application of amidoximation magnetic MXene-based composite material in uranyl adsorption
CN115945174A