Low-gloss modified polypropylene material and preparation method thereof
By using modified aqueous magnesium silicate and sodium polystyrene sulfonate in polypropylene materials, combined with functional additives, the problem of insufficient gloss and scratch resistance of existing polypropylene materials is solved, and the problem of insufficient gloss and scratch resistance of existing polypropylene materials is achieved. A combination of low gloss and high scratch resistance.
Patent Information
- Application Number
- CN202411397257.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-05
AI Technical Summary
The existing spray-free scratch-resistant polypropylene materials for automotive use have low surface strength, short service life, difficult to withstand high-pressure scratches, and difficult to effectively reduce gloss.
Using low-gloss modified polypropylene material, prepared by blending homopolypolypropylene or copolymerized polypropylene with modified aqueous magnesium silicate and sodium polystyrene sulfonate, combined with functional additives, pelletized by twin screw extruder , form a low-gloss modified polypropylene material, reduces gloss and improves scratch resistance.
It significantly improves the scratch resistance and impact strength of the material, extends the service life, and achieves a reduction in gloss.
Smart Images

Figure SMS_6 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of high molecular polymers, and in particular to a low-gloss modified polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene resin, referred to as PP, is a colorless, odorless, non-toxic translucent solid substance. In addition, polypropylene is widely available, inexpensive, and has chemical resistance, heat resistance, electrical insulation, good mechanical properties, and wear resistance. Therefore, since the 1980s, the application of polypropylene materials has covered all aspects of our daily life, such as home appliance housings, auto parts, electronic devices, building materials, food packaging, etc.
[0003] The size of spherulites has a great influence on the gloss of polypropylene materials. Whether reducing the spherulite size to improve the gloss of polypropylene materials or increasing the spherulite size to reduce the gloss of polypropylene materials, both are current research and development hotspots of polypropylene materials.
[0004] The Chinese patent application document with publication number CN108384111A discloses a spray-free scratch-resistant polypropylene material for automobiles and a preparation method thereof. The spray-free scratch-resistant polypropylene material for automobiles comprises the following raw materials in parts by weight: 50 to 85 parts of high crystalline polypropylene, 10 to 22 parts of calcium carbonate, 5 to 10 parts of toughening agent ethylene-octene copolymer, 1 to 4 parts of organic silicon scratch-resistant agent, 0.5 to 4 parts of aluminum pigment, 0.1 to 0.5 parts of organic phosphate nucleating agent, 0.3 to 0.8 parts of coupling agent alkyl modified polysiloxane, 0.2 to 0.8 parts of hindered amine light stabilizer, 0.2 to 0.8 parts of antioxidant, and 0.3 to 0.8 parts of antistatic agent.
[0005] However, the surface strength of the spray-free scratch-resistant polypropylene material for automobiles and the preparation method thereof is relatively low, and the best cross scratch result obtained by testing is only =0.72, which results in a short service life and difficulty in withstanding high-pressure scratching, which needs to be improved. Summary of the invention
[0006] In view of this, the first object of the present application is to provide a low-gloss modified polypropylene material to achieve the purpose of effectively reducing the gloss and significantly improving the scratch resistance. The specific scheme is as follows:
[0007] A low-gloss modified polypropylene material comprises the following components:
[0008] According to the total weight of the low-gloss modified polypropylene material: 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of a modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive;
[0009] The polypropylene composition comprises 49.9-69.9 wt % of homopolypropylene or copolymer polypropylene and 0.1-10.0 wt % of a multi-component copolymer of ethylene and propylene;
[0010] The modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with surface ammonium compounds or protonated amines.
[0011] Preferably, the functional additives include 0.1-0.5 wt % of an antioxidant, 0.1-0.5 wt % of a lubricant, 0.01-0.3 wt % of a light stabilizer and 0-1 wt % of a toner.
[0012] Preferably: the antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical; the lubricant is zinc stearate, magnesium stearate or calcium stearate; the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate; and the toner is carbon black.
[0013] Preferably, the multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 0.01-3wt%.
[0014] Preferably, the ammonium compound is an ammonium polyphosphate compound, a quaternary ammonium hydroxide, a quaternary ammonium fluoride, a quaternary ammonium bromide or a quaternary ammonium iodide.
[0015] Preferably: the chemical formula of the ammonium compound is as follows: ;
[0016] Wherein, R1, R2, R3, and R4 are independently selected from C1-C8 alkyl, C6-C14 aryl, or C1-C16 hydroxyalkyl; and R1, R2, R3, and R4 are used to form at least one cyclic structure.
[0017] Preferably, the protonated amine is one of methylammonium, dimethylammonium, diethylammonium, trimethylammonium and triethylammonium.
[0018] Preferably, the melt index test is carried out according to ISO 1133: 230°C, 2.16Kg, the homopolypropylene melt flow index is 3-15g / min, the copolymer polypropylene melt flow index is 5-20g / min, and the multi-polymer melt flow index is 3-10g / min.
[0019] The second object of the present invention is to provide a method for preparing a low-gloss modified polypropylene material, comprising the following steps:
[0020] Step 1, adding 49.9-69.9wt% of homopolypropylene or copolymer and 0.1wt%-10.0wt% of multi-component copolymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition;
[0021] Step 2, adding 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of a modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive in a mixer and mixing to obtain a mixture;
[0022] Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
[0023] Preferably: the preparation method of the modified hydrated magnesium silicate comprises dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 0.3-3wt%; then heating the temperature to 40-60°C, adding an ammonium compound or a protonated amine, stirring for 4-12 hours, and controlling the molar ratio of the ammonium compound or the protonated amine to the hydrated magnesium silicate to be greater than 1; and finally filtering to obtain the product, washing with deionized water and drying.
[0024] It can be seen from the above scheme that the present application provides a low-gloss modified polypropylene material and a preparation method thereof, and the low-gloss modified polypropylene material and the preparation method thereof have the following beneficial effects:
[0025] 1. The purpose of reducing the gloss is achieved by using homopolymerized polypropylene or copolymerized polypropylene and a multi-polymer obtained by polymerizing ethylene and propylene as the main materials, combined with modified hydrous magnesium silicate and sodium polystyrene sulfonate or poly(styrene sulfonic acid) to blend and prepare the polypropylene composition;
[0026] 2. Using homopolymerized polypropylene or copolymerized polypropylene and a multi-polymer of ethylene and propylene in a polypropylene composition as the main material, and using modified hydrous magnesium silicate obtained by chemically modifying hydrous magnesium silicate with an ammonium compound or a protonated amine as an inorganic filler, thereby effectively reducing the crystallinity and achieving the effect of reducing the glossiness;
[0027] 3. Through the synergistic effect of modified hydrous magnesium silicate and polypropylene composition, sodium polystyrene sulfonate or poly(styrene sulfonic acid), in a twin-screw extruder, a micro-crosslinking reaction of modified hydrous magnesium silicate with polypropylene composition, sodium polystyrene sulfonate or poly(styrene sulfonic acid) is achieved to form a partial network structure, and combined with a self-crosslinking annular structure, the gloss of the material is reduced while improving the scratch resistance;
[0028] 4. The performance diversification and color control are achieved through functional additives and colorants, which significantly improves the practicality of the low-gloss modified polypropylene material. DETAILED DESCRIPTION
[0029] The following will be clearly and completely described in conjunction with the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0030] The low-gloss modified polypropylene material of the present application and its preparation method will be described in detail below.
[0031] A low-gloss modified polypropylene material comprises 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive, calculated on the total weight of the low-gloss modified polypropylene material.
[0032] The polypropylene composition comprises 49.9-69.9wt% of homopolypropylene or copolymer polypropylene and 0.1wt%-10.0wt% of a multi-polymer of ethylene and propylene. The melt index test is carried out according to ISO 1133: 230°C, 2.16Kg. The melt flow index of the homopolypropylene is 3-15g / min, the melt flow index of the copolymer polypropylene is 5-20g / min, and the melt flow index of the multi-polymer is 3-10g / min.
[0033] It should be mentioned that the multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 0.01-3wt%. At the same time, the modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with surface ammonium compounds or protonated amines. The ammonium compound is an ammonium polyphosphate compound, a quaternary ammonium hydroxide, a quaternary ammonium fluoride, a quaternary ammonium bromide or a quaternary ammonium iodide. The protonated amine is one of methylammonium, dimethylammonium, diethylammonium, trimethylammonium and triethylammonium.
[0034] In order to achieve a significant improvement in the contribution of modified hydrous magnesium silicate to scratch resistance and low gloss, the chemical formula of the ammonium compound used is as follows: ;
[0035] Wherein, R1, R2, R3, and R4 are independently selected from C1-C8 alkyl, C6-C14 aryl, or C1-C16 hydroxyalkyl; and R1, R2, R3, and R4 are used to form at least one cyclic structure.
[0036] It should be noted that when functional additives are used, the functional additives used include 0.1-0.5wt% antioxidant, 0.1-0.5wt% lubricant, 0.01-0.3wt% light stabilizer and 0-1wt% toner based on the total weight of the low-gloss modified polypropylene material. The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical. The lubricant is one of zinc stearate, magnesium stearate or calcium stearate. The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate. The toner is carbon black.
[0037] A method for preparing a low-gloss modified polypropylene material comprises the following steps:
[0038] Step 1, adding 49.9-69.9wt% of homopolypropylene or copolymer and 0.1wt%-10.0wt% of multi-component copolymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition;
[0039] Step 2, adding 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of a modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive in a mixer and mixing to obtain a mixture;
[0040] Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
[0041] The preparation method of modified hydrated magnesium silicate comprises the following steps: firstly dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 0.3-3wt%; then heating the temperature to 40-60°C, adding ammonium compound or protonated amine, stirring for 4-12h, and controlling the molar ratio of ammonium compound or protonated amine to hydrated magnesium silicate to be greater than 1; and finally filtering to obtain the product, washing with deionized water and drying.
[0042] Embodiment 1
[0043] A low-gloss modified polypropylene material comprises 50.0 wt% of a polypropylene composition, 40 wt% of modified hydrous magnesium silicate and 10 wt% of sodium polystyrene sulfonate, based on the total weight of the low-gloss modified polypropylene material.
[0044] The polypropylene composition includes 49.9 wt% homopolypropylene and 0.1 wt% multipolymer of ethylene and propylene. The melt index test is carried out according to ISO 1133: 230°C, 2.16 kg. The melt flow index of the homopolypropylene is 12 g / min, and the melt flow index of the multipolymer is 7 g / min.
[0045] It should be mentioned that the multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 0.2wt%. At the same time, the modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with an ammonium compound on the surface. The ammonium compound is a quaternary ammonium hydroxide. In order to significantly improve the contribution of the modified hydrous magnesium silicate to scratch resistance and low gloss, the chemical formula of the ammonium compound used is as follows: ;
[0046] Among them, R1 is ethyl group, R2 is methane aryl group, R3 is hydroxymethyl group, and R4 is hydroxyethyl group.
[0047] A method for preparing a low-gloss modified polypropylene material comprises the following steps:
[0048] Step 1, adding 49.9 wt% of homopolypropylene and 0.1 wt% of a multi-polymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition;
[0049] Step 2, adding 50.0 wt% of a polypropylene composition, 40 wt% of modified hydrous magnesium silicate, and 10 wt% of sodium polystyrene sulfonate in a mixer and mixing to obtain a mixture;
[0050] Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
[0051] The temperatures of zones 1 to 9 of the extruder are 190°C, 190°C, 195°C, 195°C, 200°C, 205°C, 215°C, 215°C, and 225°C, respectively; and the die head temperature is 210°C. The preparation method of modified hydrated magnesium silicate comprises first dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 0.3wt%; then heating the temperature to 60°C, adding ammonium compound, stirring for 12h, and controlling the molar ratio of ammonium compound to hydrated magnesium silicate to be greater than 1; finally filtering to obtain the product, washing with deionized water, and drying.
[0052] Embodiment 2
[0053] A low-gloss modified polypropylene material comprises 63 wt% of a polypropylene composition, 30 wt% of modified hydrous magnesium silicate and 7 wt% of sodium polystyrene sulfonate, based on the total weight of the low-gloss modified polypropylene material.
[0054] The polypropylene composition includes 56.5 wt% of homopolypropylene and 6.5 wt% of a multipolymer of ethylene and propylene. The melt index test is carried out according to ISO 1133:2011 at 230°C and 2.16 kg load. The melt flow index of the homopolypropylene is 14 g / min, and the melt flow index of the multipolymer is 6 g / min.
[0055] It should be mentioned that the multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 1.6wt%. At the same time, the modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with an ammonium compound on the surface. The ammonium compound is a quaternary ammonium hydroxide.
[0056] In order to achieve a significant improvement in the contribution of modified hydrous magnesium silicate to scratch resistance and low gloss, the chemical formula of the ammonium compound used is as follows: ;
[0057] Among them, R1 is pentyl, R2 is aryl, R3 is hydroxyisopropyl, and R4 is hydroxyethyl.
[0058] A method for preparing a low-gloss modified polypropylene material comprises the following steps:
[0059] Step 1, adding 56.5 wt% of homopolypropylene and 6.5 wt% of a multi-polymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition;
[0060] Step 2, adding 63 wt% of a polypropylene composition, 30 wt% of modified hydrous magnesium silicate, and 7 wt% of sodium polystyrene sulfonate in a mixer and mixing to obtain a mixture;
[0061] Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
[0062] The temperatures of zones 1 to 9 of the extruder are 190°C, 190°C, 195°C, 195°C, 200°C, 205°C, 215°C, 215°C, and 225°C, respectively; and the die head temperature is 210°C. The preparation method of modified hydrated magnesium silicate comprises first dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 2.2wt%; then heating the temperature to 50°C, adding ammonium compound, stirring for 6h, and controlling the molar ratio of ammonium compound to hydrated magnesium silicate to be greater than 1; finally filtering to obtain the product, washing with deionized water, and drying.
[0063] Embodiment 3
[0064] A low-gloss modified polypropylene material comprises 79.9 wt% of a polypropylene composition, 10.1 wt% of modified hydrous magnesium silicate and 10 wt% of poly(styrene sulfonic acid) based on the total weight of the low-gloss modified polypropylene material.
[0065] The polypropylene composition includes 69.9 wt% of copolymerized polypropylene and 10.0 wt% of a multi-polymer of ethylene and propylene. The melt index test is carried out according to ISO 1133: 230°C, 2.16 kg. The melt flow index of the copolymerized polypropylene is 17 g / min, and the melt flow index of the multi-polymer is 5 g / min.
[0066] It should be mentioned that the multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 3wt%. At the same time, the modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with surface protonated amine. The protonated amine is diethylammonium.
[0067] A method for preparing a low-gloss modified polypropylene material comprises the following steps:
[0068] Step 1, adding 69.9 wt% of copolymerized polypropylene and 10.0 wt% of a multi-component copolymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition;
[0069] Step 2, adding 79.9 wt % of a polypropylene composition, 10.1 wt % of modified hydrous magnesium silicate, and 10 wt % of poly(styrene sulfonic acid) into a mixer and mixing to obtain a mixture;
[0070] Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
[0071] The temperatures of zones 1 to 9 of the extruder are 190°C, 190°C, 195°C, 195°C, 200°C, 205°C, 215°C, 215°C, and 225°C, respectively; and the die head temperature is 210°C. The preparation method of modified hydrated magnesium silicate comprises first dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 3wt%; then heating the temperature to 40°C, adding protonated amine, stirring for 4h, and controlling the molar ratio of protonated amine to hydrated magnesium silicate to be greater than 1; finally filtering to obtain the product, washing with deionized water, and drying.
[0072] Embodiment 4
[0073] The difference between Example 4 and Example 2 is that Example 4 uses 29wt% modified hydrous magnesium silicate and 1wt% functional additives, and the functional additives include 0.1wt% antioxidant, 0.1wt% lubricant, 0.3wt% light stabilizer and 0.5wt% toner based on the total weight of the low-gloss modified polypropylene material. The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical. The lubricant is zinc stearate. The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate. The toner is carbon black.
[0074] Embodiment 5
[0075] The difference between Example 5 and Example 2 is that Example 5 uses 29wt% modified hydrous magnesium silicate and 1wt% functional additives, and the functional additives include 0.5wt% antioxidant, 0.49wt% lubricant, and 0.01wt% light stabilizer based on the total weight of the low-gloss modified polypropylene material. The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical. The lubricant is calcium stearate. The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate. The toner is carbon black.
[0076] Embodiment 6
[0077] The difference between the sixth embodiment and the second embodiment is that in the sixth embodiment
[0078] 8.1wt% modified hydrous magnesium silicate and 2wt% functional additives are used, and the functional additives include 0.5wt% antioxidant, 0.5wt% lubricant, 0.3wt% light stabilizer and 0.7wt% toner according to the total weight of the low-gloss modified polypropylene material. The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical. The lubricant is magnesium stearate. The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate. The toner is carbon black.
[0079] Embodiment 7
[0080] The difference between Example 4 and Example 2 is that in Example 2, 8.1wt% of modified hydrous magnesium silicate and 2wt% of functional additives are used, and the functional additives include 0.2wt% of antioxidant, 0.5wt% of lubricant, 0.3wt% of light stabilizer and 1wt% of colorant based on the total weight of the low-gloss modified polypropylene material. The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical. The lubricant is zinc stearate. The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate. The colorant is carbon black.
[0081] Comparative Example 1
[0082] The difference between Comparative Example 1 and Example 2 is that in Comparative Example 1, hydrated magnesium silicate is used instead of modified hydrated magnesium silicate.
[0083] Comparative Example 2
[0084] The difference between Comparative Example 2 and Example 2 is that in Comparative Example 2, the modified hydrous magnesium silicate adopts quaternary ammonium hydroxide, and R1, R2, R3 and R4 are all straight-chain alkyl groups.
[0085] Comparative Example 3
[0086] The difference between Comparative Example 3 and Example 2 is that in Comparative Example 3, copolymerized polypropylene is used instead of homopolymerized polypropylene, and the melt flow index of the copolymerized polypropylene is 17 g / min.
[0087] Comparative Example 4
[0088] The difference between Comparative Example 4 and Example 2 is that the polypropylene composition in Comparative Example 4 consists of homopolypropylene and copolymer polypropylene in a molar ratio of 1:1.
[0089] Performance Testing:
[0090] 1. Cross scratch test: Tested according to PV3952 standard, 10N load, 1mm needle diameter, leather grain type is Volkswagen K3A;
[0091] 2. Surface gloss test: tested according to ASTM D523:2014 standard, the sample size is 100mm×100mm×2mm, the light incident angle is 60°, and the leather grain type is Volkswagen K3A;
[0092] 3. Melt flow rate test: Tested according to ISO 1133:2011 standard, the test conditions are controlled at 230°C and 2.16Kg load;
[0093] 4. Impact strength test: The test is carried out according to ISO / 1A standard, the notch type is A-type notch, and the sample size is 80mm×8mm×4mm.
[0094] The test results are shown in Table 1 below:
[0095] Table 1 Performance test results of Examples 1 to 4 and Comparative Examples 1 to 4
[0096] It can be seen from Table 1 above that in the embodiment of the present application, the homopolypropylene or copolymer polypropylene in the polypropylene composition and the multipolymer polymerized by ethylene and propylene are used as the main material, and the modified hydrated magnesium silicate and sodium polystyrene sulfonate or poly (styrene sulfonic acid) are blended to achieve the purpose of reducing the gloss; at the same time, the homopolypropylene or copolymer polypropylene in the polypropylene composition and the multipolymer polymerized by ethylene and propylene are used as the main material, and the modified hydrated magnesium silicate obtained after the chemical modification of the hydrated magnesium silicate with an ammonium compound or a protonated amine is used as an inorganic filler, thereby effectively reducing the crystallinity and achieving the effect of reducing the gloss.
[0097] It can be seen from Example 2 and Comparative Example 3 that the effect of reducing crystallinity by using homopolymer polypropylene is more obvious than that of copolymer polypropylene, thereby achieving the surface gloss of cultivated land. It can be seen from Example 2, Example 3, Comparative Example 1 and Comparative Example 2 that the surface of hydrated magnesium silicate is treated by chemical modification of the corresponding ammonium compound, so that the modified hydrated magnesium silicate can achieve a micro-crosslinking reaction with the polypropylene composition, sodium polystyrene sulfonate or poly (styrene sulfonic acid) to form a partial network structure, and combined with the self-crosslinking annular structure to reduce the gloss of the material while improving the scratch resistance. It can be seen from Example 2, Example 4 and Comparative Example 4 that the polypropylene composition used has the effect of effectively improving the impact strength and wear resistance when combined with homopolymer polypropylene or copolymer polypropylene through melt grafting of the multi-copolymer and the grafting monomer vinyl siloxane.
[0098] In summary, the present application provides a low-gloss modified polypropylene material and a preparation method thereof. The low-gloss modified polypropylene material prepared by the preparation method of the low-gloss modified polypropylene material has a multi-polymer obtained by a melt grafting process, thereby improving the bonding strength between the multi-polymer and the homopolymer polypropylene or the copolymer polypropylene while reducing the crystallinity and achieving the purpose of low gloss, and the hydrous magnesium silicate is modified by an ammonium compound or a protonated amine, while achieving the reduction of gloss and improvement of scratch resistance by inorganic fillers, avoiding the adverse effect of impact resistance caused by the addition of inorganic fillers, so that the low-gloss modified polypropylene material has the purpose of reducing gloss by synergistic reduction of crystallinity by various components, and has the effect of significantly improving impact resistance and scratch resistance.
[0099] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.
[0100] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0101] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A low gloss modified polypropylene material, characterized in that: The components include: According to the total weight of the low-gloss modified polypropylene material: 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of a modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive; The polypropylene composition comprises 49.9-69.9 wt % of homopolypropylene or copolymer polypropylene and 0.1-10.0 wt % of a multi-component copolymer of ethylene and propylene; The modified hydrous magnesium silicate is obtained by chemically modifying the hydrous magnesium silicate with surface ammonium compounds or protonated amines.
2. A low gloss modified polypropylene material according to claim 1, characterized in that: The functional auxiliary agent comprises 0.1-0.5 wt % of an antioxidant, 0.1-0.5 wt % of a lubricant, 0.01-0.3 wt % of a light stabilizer and 0-1 wt % of a toner.
3. A low gloss modified polypropylene material according to claim 2, characterized in that: The antioxidant is SUNSHOW 168 purchased from Xinxiu Chemical; the lubricant is zinc stearate, magnesium stearate or calcium stearate; the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate; and the toner is carbon black.
4. The low-gloss modified polypropylene material according to claim 1, characterized in that: The multi-polymer is melt-grafted with the grafting monomer vinyl siloxane, and the grafting rate is 0.01-3wt%.
5. The low-gloss modified polypropylene material according to claim 1, characterized in that: The ammonium compound is an ammonium polyphosphate compound, a quaternary ammonium hydroxide, a quaternary ammonium fluoride, a quaternary ammonium bromide or a quaternary ammonium iodide.
6. The low-gloss modified polypropylene material according to claim 1, characterized in that: The chemical formula of the ammonium compound is shown below: ; Wherein, R1, R2, R3, and R4 are independently selected from C1-C8 alkyl, C6-C14 aryl, or C1-C16 hydroxyalkyl; and R1, R2, R3, and R4 are used to form at least one cyclic structure.
7. The low-gloss modified polypropylene material according to claim 1, characterized in that: The protonated amine is one of methylammonium, dimethylammonium, diethylammonium, trimethylammonium and triethylammonium.
8. The low-gloss modified polypropylene material according to claim 1, characterized in that: According to ISO 1133: 230°C, 2.16Kg conditions, the melt index test is carried out, the homopolymer polypropylene melt flow index is 3-15g / min, the copolymer polypropylene melt flow index is 5-20g / min, and the multi-polymer melt flow index is 3-10g / min.
9. A method for preparing a low-gloss modified polypropylene material, characterized in that: The steps include: Step 1, adding 49.9-69.9wt% of homopolypropylene or copolymer and 0.1wt%-10.0wt% of multi-component copolymer of ethylene and propylene into a mixer and mixing to obtain a polypropylene composition; Step 2, adding 50.0-79.9wt% of a polypropylene composition, 8.1-40wt% of a modified hydrous magnesium silicate, 2-10wt% of sodium polystyrene sulfonate or poly(styrene sulfonic acid) and 0-2% of a functional additive in a mixer and mixing to obtain a mixture; Step 3: Add the mixture into a twin-screw extruder, control the temperature of each zone to 190-225° C., and granulate after extrusion to obtain a low-gloss modified polypropylene material.
10. The method for preparing a low-gloss modified polypropylene material according to claim 9, characterized in that: The preparation method of the modified hydrated magnesium silicate comprises dispersing hydrated magnesium silicate in deionized water, controlling the concentration of hydrated magnesium silicate to be 0.3-3wt%; then heating the temperature to 40-60°C, adding ammonium compounds or protonated amines, stirring for 4-12 hours, and controlling the molar ratio of the ammonium compounds or protonated amines to the hydrated magnesium silicate to be greater than 1; and finally filtering to obtain the product, washing with deionized water, and drying.
Citation Information
Patent Citations
Low-luster polypropylene material
CN102206381A
Low-gloss polypropylene composite and preparation method thereof
CN104558810A
Improved synthesis process of antioxidant 168
CN117384208A
Slurry composition for secondary polishing of silicon wafer
CN1714432A
Porous silica microspheres having silanol-enriched and silanized surfaces
US5032266A