Temporary fixing adhesive
By using side chain alkyl monofunctional acrylates, polyfunctional acrylates and polyisobutylene homopolymers in the temporary fixing composition, combining photoradical polymerization initiator and UV absorber, the curing speed during temporary fixing uses is solved. and the problem of insufficient peeling speed, efficient spin coating process and heat resistance are achieved, and are suitable for a variety of peeling processes.
Patent Information
- Application Number
- CN202410928826.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-05-17
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has problems such as curing speed, spin coating process suitability, heat resistance, low gas ejaculation under high temperature vacuum and insufficient peeling speed in temporary fixed applications, especially the adaptability of the UV laser peeling process is not sufficient.
An alkyl monofunctional (meth)acrylate, polyfunctional (meth)acrylate, polyisobutylene homopolymer and/or copolymer, photoradical polymerization initiator and UV absorption are used with 18 or more side chain carbon atoms. The temporary fixation composition of the agent is cured by light at a wavelength of 385 nm to 700 nm and peeled by laser light at a wavelength of less than 385 nm.
It achieves excellent curing speed, spin coating process suitability, heat resistance and low gas ejaculation under high temperature vacuum, and is suitable for mechanical peeling and various laser peeling processes, including UV laser peeling.
Smart Images

Figure BDA0004939040930000101 
Figure BDA0004939040930000381 
Figure BDA0004939040930000391
Abstract
Description
[0001] This application is a divisional application of an invention patent application with an application date of May 17, 2021, application number 202180032669.7 (PCT / JP2021 / 018671), and invention name “Composition”. Technical Field
[0002] The present invention relates to a temporary fixing adhesive used for temporary fixing purposes. Background Art
[0003] Electronic devices are obtained by using a substrate of an inorganic material represented by silicon as the main material, and performing processes such as insulating film formation, circuit formation, and thinning by grinding on its surface. When using a wafer-type substrate during processing, a substrate with a thickness of several hundred μm is mostly used, but most substrates are made of brittle and easily broken materials, so measures are required to prevent damage, especially when thinning by grinding. This measure has been adopted in the past by sticking a temporary fixing protective tape that can be peeled off after the processing step is completed on the surface opposite to the grinding object surface (also called the back side). This tape uses an organic resin film as a substrate and has flexibility, but on the other hand, it lacks strength and heat resistance and is not suitable for use in high-temperature processes.
[0004] Therefore, the following system is proposed: the electronic device substrate is bonded to a support such as silicon or glass via an adhesive, thereby imparting sufficient durability for the conditions of the back grinding and back electrode formation process. At this time, the adhesive layer when the substrate is bonded to the support is important. It is necessary to be able to bond the substrate to the support without a gap, have sufficient durability to withstand the subsequent processes, and finally, it must be possible to easily peel the thinned wafer from the support.
[0005] Necessary properties of adhesives include: (1) having a viscosity suitable for coating and being a Newtonian fluid (or shear viscosity that is independent of shear rate); (2) being able to withstand the shear adhesion of grinding / polishing when thinning the substrate; (3) similarly, when thinning the substrate, in order to avoid local concentration of the grindstone load applied to the substrate due to grinding / polishing and causing damage to the substrate, the load is dispersed in the planar direction and the substrate is prevented from sinking locally to maintain planarity; (4) heat resistance that can withstand the insulating film formation and reflow soldering processes; (5) chemical resistance that can withstand thinning and etching processes; (6) easy peelability that allows the substrate to be easily peeled off from the support; (7) agglomeration properties that prevent adhesive residues from remaining on the substrate after peeling; and (8) easy cleaning.
[0006] As adhesives and methods for stripping them, there are proposed a technique for stripping the adhesive layer from the support by irradiating an adhesive containing a light-absorbing substance with high-intensity light to decompose the adhesive layer (Patent Document 1), and a technique for using a heat-melting hydrocarbon compound as an adhesive to perform bonding / stripping in a heated and molten state (Patent Document 2). The former technique requires expensive equipment such as lasers, and has problems such as a longer processing time for each substrate. The latter technique is simple because it is controlled only by heating, but on the other hand, it has a narrow range of application because of insufficient thermal stability at high temperatures exceeding 200°C.
[0007] A method for disassembling an adhesive body is disclosed, which includes a step of irradiating an adhesive body formed by bonding substrates to each other using an adhesive composition and then curing the adhesive composition with excimer light having a central wavelength of 172nm or 193nm, wherein the adhesive composition contains one or more (meth)acrylates having one or more acryloyl groups, wherein at least one substrate shows transmittance to the excimer light (Patent Document 3). However, Patent Document 3 does not describe the use of light with a longer wavelength. The present invention does not require the use of high-energy excimer light for peeling.
[0008] A technology for an adhesive sealing composition for electronic devices is disclosed, wherein the composition comprises a polyisobutylene resin and a multifunctional (meth)acrylate as a resin composition and does not comprise a tackifier (Patent Document 4). In addition, although it also records the use of a monofunctional (meth)acrylate as a monomer, the glass transition temperature of the monofunctional (meth)acrylate is not recorded, and thus there is a problem that the method for presenting the required flexibility when the resin composition is used as a temporary fixing agent for an electronic device manufacturing process is unclear.
[0009] A technique for an adhesive sealing composition for electronic devices such as organic electroluminescent devices is also disclosed, wherein the composition comprises a monofunctional (meth)acrylate, a multifunctional (meth)acrylate, and a polyisobutylene polymer as a resin composition (Patent Document 5). However, since the glass transition temperature of the monofunctional (meth)acrylate is not described, there is a problem that the method for presenting the required flexibility when the resin composition is used as a temporary fixing agent for an electronic device manufacturing process is unclear.
[0010] A resin composition for bonding different substrates and a bonding / disassembly method containing a monofunctional (meth)acrylate, a multifunctional (meth)acrylate and an isobutylene-maleic anhydride copolymer as a resin composition is disclosed (Patent Document 6). However, the polymer of Patent Document 6 is limited in type in that it contains a component derived from maleic anhydride, and the bonding method is not described in detail. Patent Document 6 does not describe spin coating suitability such as viscosity.
[0011] A technology for a composite resin composition that can be cured by active energy rays is disclosed, wherein the composition is formed of a urethane (meth) acrylate resin and a polyisobutylene resin containing an olefin polymer structure (Patent Document 7). A photocurable composition is disclosed, comprising a component (A): a (meth) acrylate compound having a polyisobutylene skeleton and a component (B): a (meth) acrylamide compound, wherein the component (B) is contained in an amount of 0.1 to 15 parts by mass relative to 100 parts by mass of the component (A) (Patent Document 8). However, Patent Documents 7 to 8 do not describe temporary fixing applications.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Application Publication No. 2004-064040
[0015] Patent Document 2: Japanese Patent Application Publication No. 2006-328104
[0016] Patent Document 3: International Publication No. 2011 / 158654
[0017] Patent Document 4: Japanese Patent No. 5890177
[0018] Patent Document 5: Japanese Patent Application No. 2009-524705
[0019] Patent Document 6: Japanese Patent No. 6139862
[0020] Patent Document 7: Japanese Patent Application Publication No. 2017-226785
[0021] Patent Document 8: International Publication No. 2020 / 080309 Summary of the invention
[0022] Problems to be solved by the invention
[0023] Therefore, for example, even if the composition involved in the prior art is used for temporary fixing, the following problems cannot be solved: the curing speed, suitability for the spin coating process, heat resistance, low outgassing under high temperature vacuum, and insufficient stripping speed, and in particular, the adaptability to the UV laser stripping process is also insufficient.
[0024] Means for solving problems
[0025] That is, in the present invention, the following aspects can be provided.
[0026] <1> A temporary fixing composition comprising the following (A) to (C).
[0027] (A) (meth)acrylate containing the following (A-1) and (A-2)
[0028] (A-1) a monofunctional (meth)acrylate having an alkyl group having 18 or more carbon atoms in the side chain and a homopolymer having a Tg of -100°C to 60°C
[0029] (A-2) Multifunctional (meth)acrylate
[0030] (B) Polyisobutylene homopolymer and / or polyisobutylene copolymer
[0031] (C) Photoradical polymerization initiator
[0032] <2> The temporary fixing composition according to Embodiment 1 further comprises the following (D).
[0033] (D) UV absorber
[0034] <3> The temporary fixing composition according to aspect 1 or 2, wherein the molecular weight of the (A-1) monofunctional (meth)acrylate is 550 or less.
[0035] <4> The temporary fixing composition according to any one of Embodiments 1 to 3, wherein the component (A-1) is a monofunctional (meth)acrylate having an alkyl group of a linear structure or a branched structure in a side chain.
[0036] <5> The temporary fixing composition according to any one of aspects 1 to 4, wherein the component (A-1) is one or more selected from the group consisting of stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, 2-decyl-1-tetradecyl (meth)acrylate, 2-dodecyl-1-hexadecyl (meth)acrylate, and 2-tetradecyl-1-octadecyl (meth)acrylate.
[0037] <6> The temporary fixing composition according to any one of Embodiments 1 to 5, wherein the molecular weight of the (A-2) polyfunctional (meth)acrylate is 900 or less.
[0038] <7> The temporary fixing composition according to any one of Embodiments 1 to 6, wherein the component (A-2) is a polyfunctional (meth)acrylate having an alicyclic skeleton.
[0039] <8> The temporary fixing composition according to any one of aspects 1 to 7, wherein the component (A-2) is one or more selected from the group consisting of tricyclodecanedimethanol di(meth)acrylate and 1,3-di(meth)acryloyloxyadamantane.
[0040] <9> The temporary fixing composition according to any one of aspects 1 to 8, wherein the component (B) is a polyisobutylene homopolymer and / or a polyisobutylene copolymer having a weight average molecular weight of 1,000 to 5,000,000 and a molecular weight distribution of 1.1 to 5.0.
[0041] <10> The temporary fixing composition according to any one of aspects 1 to 9, wherein the component (C) is a photoradical polymerization initiator that generates radicals by light having a wavelength of 350 nm or more.
[0042] <11> The temporary fixing composition according to any one of embodiments 1 to 10, wherein the component (C) is selected from bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-butan-1-one, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime, and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime).
[0043] <12> The temporary fixing composition according to any one of aspects 1 to 11, wherein the component (C) is contained in an amount of 0.01 to 5 parts by mass based on 100 parts by mass of the total of the components (A) to (B).
[0044] <13> A temporary fixing adhesive comprising the temporary fixing composition according to any one of aspects 1 to 12.
[0045] <14> A cured product obtained by curing the temporary fixing composition according to any one of aspects 1 to 12.
[0046] <15> The cured product according to aspect 14, wherein the temperature at which the heating mass reduction rate reaches 2 mass % is 250° C. or higher.
[0047] <16> An adhesive body obtained by bonding substrates using the temporary fixing adhesive described in Embodiment 13.
[0048] <17> An adhesive body obtained by bonding substrates using a temporary fixing adhesive, wherein the temporary fixing adhesive contains the following (A) to (C):
[0049] (A) (meth)acrylate containing the following (A-1) and (A-2)
[0050] (A-1) a monofunctional (meth)acrylate having an alkyl group having 18 or more carbon atoms in the side chain and a homopolymer having a Tg of -100°C to 60°C
[0051] (A-2) Multifunctional (meth)acrylate
[0052] (B) Polyisobutylene homopolymer and / or polyisobutylene copolymer
[0053] (C) Photoradical polymerization initiator
[0054] The temporary fixing adhesive is cured by light having a wavelength of 385 nm to 700 nm, and the base material is peeled off by laser light having a wavelength less than 385 nm.
[0055] <18> A method for manufacturing a thin wafer using the temporary fixing adhesive described in embodiment 13.
[0056] <19> A method for manufacturing a semiconductor wafer, comprising:
[0057] A step of applying a temporary fixing adhesive to the semiconductor wafer substrate and / or the supporting member to bond the semiconductor wafer substrate to the supporting member;
[0058] A step of curing the temporary fixing adhesive by irradiating light with a wavelength of 350nm to 700nm to obtain an adhesive body; and
[0059] The step of irradiating the adhesive body with a laser beam having a wavelength less than 385 nm to peel off the semiconductor wafer substrate.
[0060] <20> The manufacturing method according to aspect 18 or 19, wherein the cured temporary fixing adhesive constitutes a single layer in the adhesive body.
[0061] <21> The temporary fixing adhesive according to aspect 13 is used for at least one application selected from the group consisting of mechanical peeling, IR laser peeling, and UV laser peeling.
[0062] <22> A single-layer cured body formed from the temporary fixing composition according to any one of Embodiments 1 to 12.
[0063] <23> A cured body comprising: a first cured layer containing component (A-1), component (A-2), component (B), and component (C) and excluding component (D); and a second cured layer formed from the temporary fixing composition according to embodiment 2,
[0064] The concentration distribution of the components differs in the thickness direction.
[0065] <24> A cured product comprising: a first cured layer obtained by curing the temporary fixing composition according to embodiment 1 comprising components (A-1), (A-2), (B), and (C); and a second cured layer obtained by coating a UV absorber on the first cured layer.
[0066] The concentration distribution of the components differs in the thickness direction.
[0067] <25> The cured product comprises: a first cured layer obtained by curing the temporary fixing composition according to embodiment 1 comprising components (A-1), (A-2), (B), and (C); and a light-to-heat conversion (LTHC) cured layer.
[0068] <26> The cured product according to any one of Embodiments 22 to 25, which satisfies all of the following conditions.
[0069] The light transmittance of the cured product having a thickness of 50 μm is 70% or more in a wavelength region of 395 nm or more among the wavelengths of the light source used for curing.
[0070] The light transmittance of the cured product having a thickness of 50 μm is 20% or more in a wavelength region of 385 nm or more and less than 395 nm among the wavelengths of the light source used for curing.
[0071] The light transmittance of the cured product having a thickness of 50 μm was 1% or less at the wavelength (355 nm) of the UV laser used for UV laser lift-off.
[0072] <27> A structure comprising: the cured product according to any one of aspects 22 to 26; and an adherend.
[0073] <28> A method for manufacturing a structure, comprising:
[0074] A step of applying a temporary fixing composition comprising the components (A-1), (A-2), (B), and (C) and excluding the component (D) on a wafer and partially curing the composition;
[0075] A step of coating the temporary fixing composition described in method 2 on the partially cured temporary fixing composition; and
[0076] A step of further placing a transparent substrate on the applied temporary fixing composition and photocuring the composition.
[0077] <29> A method for manufacturing a structure, comprising:
[0078] A step of applying a temporary fixing composition comprising the components (A-1), (A-2), (B), and (C) and excluding the component (D) on a wafer and partially curing the composition as necessary;
[0079] A step of coating the temporary fixing composition described in Embodiment 2 on a transparent substrate and partially curing it as necessary; and
[0080] A step of bonding the wafer and the transparent substrate, the surfaces of which the temporary fixing composition is applied, by bringing them into close contact with each other and then photocuring them.
[0081] <30> A method for manufacturing a structure, comprising:
[0082] A step of applying the temporary fixing composition according to Embodiment 1, which comprises the components (A-1), (A-2), (B), and (C) and does not comprise the component (D), onto a wafer and partially curing the composition as required;
[0083] The steps of coating a light-to-heat conversion (LTHC) layer on a transparent substrate, drying it, and curing it; and
[0084] A step of bonding the surface of the wafer coated with the temporary fixing composition to the surface of the transparent substrate coated with the LTHC layer by photocuring.
[0085] Effects of the Invention
[0086] According to the present invention, for example, a composition having excellent curing speed, suitability for spin coating process, heat resistance, low outgassing under high temperature vacuum, and peeling speed can be obtained, and a temporary fixing composition suitable for mechanical peeling process and / or various laser peeling processes (UV laser peeling process, etc.) can be obtained. DETAILED DESCRIPTION
[0087] The present invention is described below. In the present specification, unless otherwise specified, a numerical range includes its upper limit and lower limit.
[0088] A monofunctional (meth)acrylate refers to a compound having one (meth)acryloyl group in one molecule. A polyfunctional (meth)acrylate refers to a compound having two or more (meth)acryloyl groups in one molecule. An n-functional (meth)acrylate refers to a compound having n (meth)acryloyl groups in one molecule.
[0089] First, the first embodiment of the present invention can provide a temporary fixing composition (hereinafter, sometimes referred to as a composition) for temporary fixing use, which contains the following (A) to (C) components.
[0090] (A) (meth)acrylate containing the following (A-1) and (A-2)
[0091] (A-1) a monofunctional (meth)acrylate having an alkyl group having 18 or more carbon atoms in the side chain and a homopolymer having a Tg of -100°C to 60°C
[0092] (A-2) Multifunctional (meth)acrylate
[0093] (B) Polyisobutylene homopolymer and / or polyisobutylene copolymer
[0094] (C) Photoradical polymerization initiator
[0095] Moreover, secondly, the temporary fixing composition further comprising the following (D) component can be provided.
[0096] (D) UV absorber
[0097] Moreover, thirdly, it is also possible to provide a multilayer (plural-layer) structure including: a layer containing (A) to (C); and a layer containing one or more of (A) to (D).
[0098] (A-1) The monofunctional (meth)acrylate whose side chain is an alkyl group having 18 or more carbon atoms and whose homopolymer Tg is -100°C to 60°C means a monofunctional (meth)acrylate whose homopolymer glass transition temperature (hereinafter sometimes referred to as Tg) is -100°C to 60°C when polymerized alone and whose side chain is an alkyl group (functional group formed by aliphatic hydrocarbon with a chain structure or a cyclic structure). More preferably, the monofunctional (meth)acrylate whose homopolymer Tg is -50°C to 0°C.
[0099] Examples of the monofunctional (meth)acrylates having a side chain of an alkyl group having 18 or more carbon atoms and a homopolymer having a Tg of -100 to 60°C include stearyl (meth)acrylate (Tg of the homopolymer of acrylate: 30°C, Tg of the homopolymer of methacrylate: 38°C), isostearyl (meth)acrylate (Tg of the homopolymer of acrylate: -18°C, Tg of the homopolymer of methacrylate: 30°C), behenyl (meth)acrylate (Tg of the homopolymer of acrylate: 50°C, Tg of the homopolymer of methacrylate: 60°C), and methacrylic acid. Tg: 47°C), 2-decyl-1-tetradecyl (meth)acrylate (homopolymer Tg of acrylate: -36°C, homopolymer Tg of methacrylate: -29°C), 2-dodecyl-1-hexadecyl (meth)acrylate (homopolymer Tg of acrylate: -23°C, homopolymer Tg of methacrylate: -14°C), 2-tetradecyl-1-octadecyl (meth)acrylate (homopolymer Tg of acrylate: -8°C, homopolymer Tg of methacrylate: 1°C), etc. One or more of the above (meth)acrylates may be used.
[0100] The so-called glass transition refers to the following change: a material such as glass that is liquid at high temperature increases its viscosity sharply within a certain temperature range due to a decrease in temperature, and almost loses fluidity and becomes an amorphous solid. The method for measuring the glass transition temperature is not particularly limited, and generally refers to the glass transition temperature calculated by differential scanning calorimetry, differential thermal measurement, dynamic viscoelasticity measurement, etc. Among these, dynamic viscoelasticity measurement is preferred.
[0101] The glass transition temperature of the homopolymer of (meth)acrylate is described in J. Brandrup, EH Immergut, Polymer Handbook, 2nd Ed., J. Wiley, New York 1975, Photocuring Technology Data Book (Techno-netbooks Co.), and the like.
[0102] As (A-1), a monofunctional (meth)acrylate having a molecular weight of 550 or less is preferred.
[0103] As (A-1), a monofunctional alkyl (meth)acrylate having an alkyl group is preferred.
[0104] As the alkyl group, it is preferably one or more selected from a linear alkyl group, a branched alkyl group, and an alicyclic alkyl group, and more preferably one or more selected from a linear alkyl group and a branched alkyl group. From the viewpoint of improving compatibility with the (B) component (especially improving compatibility with the high molecular weight (B) component), the (A-1) component preferably has a long-chain, branched or cyclic alkyl group, preferably a branched alkyl group or a cycloalkyl group such as isostearyl, isocosanyl (2-decyl-1-tetradecyl, etc.), isotriacontyl (2-tetradecyl-1-octadecyl, etc.) having 18 to 40 carbon atoms, and more preferably 18 to 32 carbon atoms. By using such a long-chain, high-molecular-weight component with strong aliphatic hydrocarbon characteristics (especially preferably improving the properties of the aliphatic hydrocarbon of the entire system), the low volatility, chemical resistance and heat resistance required for the temporary fixing composition can be improved.
[0105] (A-1) is preferably at least one selected from the group consisting of stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, 2-decyl-1-tetradecyl (meth)acrylate, 2-dodecyl-1-hexadecyl (meth)acrylate, and 2-tetradecyl-1-octadecyl (meth)acrylate.
[0106] As the monofunctional alkyl (meth)acrylate having an alkyl group (A-1), a (meth)acrylate of the following formula 1 is preferred.
[0107] [Chemical formula 1]
[0108]
[0109] R 1 is a hydrogen atom or a methyl group. 2 It is an alkyl group.
[0110] R 1 More preferably, it is a hydrogen atom.
[0111] R 2 The number of carbon atoms of is preferably 18 to 32. One or more of the (meth)acrylates may be used.
[0112] As R 2 The monofunctional alkyl (meth)acrylate having an alkyl group having 18 to 32 carbon atoms is preferably a (meth)acrylate having a linear or branched alkyl group such as stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, 2-decyl-1-tetradecyl (meth)acrylate, 2-tetradecyl-1-octadecyl (meth)acrylate, etc.
[0113] In the total of 100 parts by mass of components (A) to (B), the amount of (A-1) monofunctional (meth) acrylate is preferably 35 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 45 parts by mass or more. In the total of 100 parts by mass of components (A) to (B), the amount of (A-1) monofunctional (meth) acrylate is preferably 54 to 90 parts by mass, more preferably 54 to 80 parts by mass, and further preferably 54 to 75 parts by mass. If it is 54 parts by mass or more, the mixed resin composition will not phase separate, and flexibility at room temperature can be obtained. If it is 90 parts by mass or less, the viscosity, heat resistance and curing properties required for coating can be obtained. The amount of monofunctional (meth) acrylate used in the composition described in Patent Document 7 is less than 53 parts by mass, and the flexibility required for temporary fixing composition for electronic device manufacturing may not be obtained.
[0114] (A-2) The polyfunctional (meth)acrylate refers to a compound having two or more (meth)acryloyl groups in one molecule. As the polymerizable functional group, it may have only an acryloyl group, only a methacryloyl group, or both an acryloyl group and a methacryloyl group.
[0115] The molecular weight of the (A-2) polyfunctional (meth)acrylate is preferably 900 or less, more preferably 700 or less, most preferably 500 or less, and still more preferably 400 or less.
[0116] (A-2) As polyfunctional (meth)acrylate, bifunctional (meth)acrylate, trifunctional (meth)acrylate, tetrafunctional or higher functional (meth)acrylate, etc. are mentioned.
[0117] Examples of the bifunctional (meth)acrylate include 1,3-di(meth)acryloyloxyadamantane, tricyclodecane dimethanol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, neopentyl glycol-modified trimethylolpropane di(meth)acrylate, stearic acid-modified pentaerythritol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 2,2-bis(4-(meth)acryloxydiethoxyphenyl)propane, 2,2-bis(4-(meth)acryloxypropoxyphenyl)propane, 2,2-bis(4-(meth)acryloxytetraethoxyphenyl)propane, isocyanuric acid ethylene oxide-modified di(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene di(meth)acrylate, and the like.
[0118] Examples of the trifunctional (meth)acrylate include isocyanuric acid ethylene oxide-modified tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tris[(meth)acryloyloxyethyl]isocyanurate.
[0119] Examples of tetrafunctional or higher-functional (meth)acrylates include di(trimethylolpropane)tetra(meth)acrylate, dimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol ethoxytetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0120] Among (A-2), polyfunctional (meth)acrylates having an alicyclic skeleton are preferred, and polyfunctional (meth)acrylates having an alicyclic skeleton having 5 or more carbon atoms are more preferred. As the polyfunctional (meth)acrylate having an alicyclic skeleton having 5 or more carbon atoms, at least one selected from tricyclodecane dimethanol di(meth)acrylate and 1,3-di(meth)acryloyloxyadamantane is preferred.
[0121] The amount of the (A-2) multifunctional (meth)acrylate used in 100 parts by mass of the total of the components (A) to (B) is preferably 1 to 40 parts by mass, more preferably 20 to 30 parts by mass. If it is 1 part by mass or more, good curability, heat resistance, and peelability can be obtained, and if it is 40 parts by mass or less, the mixed composition will not undergo phase separation and the heat resistance will not decrease.
[0122] In the selection of component (B), a polyisobutylene homopolymer refers to a homopolymer obtained by polymerization using isobutylene as a raw material monomer. As a homopolymer, Oppanol can be obtained from BASF, for example. In addition, in the selection of component (B), a so-called polyisobutylene copolymer refers to a copolymer (or heteropolymer) obtained by polymerization using isobutylene as a raw material monomer. The copolymer can be a random copolymer or a block copolymer, and a block copolymer is particularly preferably used. As a block copolymer, for example, SIBSTAR comprising a polyisobutylene block chain and a polystyrene block chain can be obtained from Kaneka. It should be noted that the above-mentioned isobutylene polymer can have a (meth) acrylate group at one end or both ends. As such a polymer, EP400V of the EPION series that can be obtained from Kaneka can be cited as an example of an isobutylene polymer containing an acrylate group at both ends.
[0123] The isobutylene polymer may have a polymerizable functional group other than a (meth)acrylate group at one or both ends. For example, "NOF Polybutene (trademark)" which is an isobutylene polymer having an ethylenically unsaturated group is available from NOF Corporation.
[0124] As for the component (B), from the viewpoint of obtaining a moderate viscosity when combined with the component (A), the so-called high molecular weight grade is preferred, for example, preferably, the weight average molecular weight is 1,000 to 5,000,000, more preferably 80,000 to 5,000,000. In addition, the molecular weight distribution of the component (B) is preferably 1.1 to 5.0, more preferably 2.2 to 2.9. It is particularly preferred that the weight average molecular weight can be 80,000 to 5,000,000 and the molecular weight distribution is 2.2 to 2.9. As the component (B), one or more of the above-mentioned polyisobutylene homopolymers and / or polyisobutylene copolymers can be used.
[0125] In a preferred embodiment, it is suitable to include a polyisobutylene copolymer as component (B). The polyisobutylene copolymer is the following concept: it includes isobutylene monomer units and monomer units other than this, and its copolymerization form includes block copolymers, random copolymers, and alternating copolymers. Block copolymers are preferably used. The reasons are as follows. When comparing block copolymers with random copolymers, generally, random copolymers are characterized in that the average value of various properties such as the glass transition temperature of homopolymers formed by multiple monomers as their constituent components is obtained, while block copolymers are characterized in that various properties such as the glass transition temperature of homopolymers formed by each monomer are not averaged but maintained as they are, and both are presented at the same time. In addition, especially with regard to triblock copolymers, it is known that the physical properties of the blocks at both ends are more strongly presented than the central block. For example, in the case of a triblock copolymer having a structure in which a polystyrene block chain having a glass transition temperature of about 100°C is sandwiched between two ends of a polyisobutylene block chain having a glass transition temperature of about -60°C, the polystyrene block chains at both ends have a high glass transition temperature, thereby showing a high thickening effect compared with a polyisobutylene homopolymer of the same molecular weight. Due to this high thickening effect, the molecular weight of the copolymer used can be lower than that of the polyisobutylene homopolymer. If the molecular weight of the polymer used is low, the advantage that the polymer is not easily separated and precipitated during low temperature storage at about 5°C can also be obtained. In addition, by including polystyrene, which is an aromatic hydrocarbon with a higher polarity than polyisobutylene, which is an aliphatic hydrocarbon, in the components, there is an advantage that the compatibility with the (A-2) component, which has a high polarity due to a plurality of (meth)acrylic groups, is further improved compared with the (meth)acrylate monomer having an aliphatic hydrocarbon side chain as the (A-1) component.
[0126] The weight average molecular weight in this specification is a value measured by gel permeation chromatography (GPC) and converted to standard polystyrene. Specifically, the average molecular weight is obtained under the following conditions, using tetrahydrofuran as a solvent and using a GPC system (SC-8010 manufactured by Tosoh Corporation) to prepare a calibration curve with commercially available standard polystyrene.
[0127] Flow rate: 1.0ml / min
[0128] Set temperature: 40℃
[0129] Column structure: 1 "TSK guardcolumn MP (×L)" manufactured by Tosoh Corporation, 6.0 mm ID × 4.0 cm, and 2 "TSK-GELMULTIPOREHXL-M" manufactured by Tosoh Corporation, 7.8 mm ID × 30.0 cm (theoretical number of stages: 16,000), 3 in total (theoretical number of stages: 32,000 as a whole)
[0130] Sample injection volume: 100μl (sample solution concentration is 1mg / ml)
[0131] Liquid delivery pressure: 39kg / cm 2
[0132] Detector: RI detector (differential refractive index detector)
[0133] In the total of 100 parts by mass of (A) to (B) components, the amount of (B) component used is preferably 30 parts by mass or less, and more preferably 25 parts by mass or less. In the total of 100 parts by mass of (A) to (B) components, the amount of (B) component used is preferably 1 to 20 parts by mass, and more preferably 5 to 20 parts by mass. If the (B) component is 1 part by mass or more, the desired viscosity is obtained during coating, and if it is 20 parts by mass or less, the mixed composition will not phase separate, and good curability and heat resistance can be obtained. By using the so-called polymer grade (B) component mentioned above, not only can the desired viscosity be easily obtained by adding a small amount, but also the effect of not only being able to obtain spin coating suitability but also being able to obtain rod coating suitability (i.e., a process that can select a suitable object) can be exerted.
[0134] (C) The photoradical polymerization initiator refers to a compound whose molecules are cut and split into two or more radicals by irradiation with ultraviolet light or visible light (e.g., wavelength 350nm to 700nm, preferably 385nm to 700nm or 365nm to 500nm, more preferably 385nm to 450nm).
[0135] As (C) the photoradical polymerization initiator, it is preferred to use at least one selected from the group consisting of acylphosphine oxide compounds, titanocene compounds, or α-aminoalkylphenone compounds in view of the reaction speed, heat resistance after curing, low outgassing, and absorption characteristics in a region different from the wavelength of the UV laser used in the UV laser stripping described later and the absorption wavelength region of the UV absorber used in the UV laser stripping. In addition, as a photoradical polymerization initiator for a resin composition for temporary fixing purposes for preventing damage from the bonding of the processing target substrate to the supporting substrate until the heating process, which is not a layer for dealing with the UV laser stripping process in the temporary fixing composition having the structure described later, in addition to the above, an oxime ester compound may also be selected.
[0136] Examples of the acylphosphine oxide-based compounds include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide. Among these, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide is particularly preferred.
[0137] Examples of the titanocene-based compounds include bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium.
[0138] Examples of the α-aminoalkylphenone compounds include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one and 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-butan-1-one.
[0139] Examples of the oxime ester compounds include 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime), etc. Among these, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime) is preferred.
[0140] As the photoradical polymerization initiator (C), preferably selected from bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(η 5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-butan-1-one, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime, and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime).
[0141] In the case of providing a temporary fixing composition for the UV laser stripping process of the present invention, the most preferred photoradical polymerization initiator is an acylphosphine oxide compound. The preferred acylphosphine oxide compound is bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and / or 2,4,6-trimethylbenzoyldiphenylphosphine oxide. The above-mentioned photoradical polymerization initiator is highly sensitive, has excellent deep curing properties due to its light fading properties, and the absorption wavelength region for generating free radicals extends to a longer wavelength region. Specifically, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide is in the range of wavelengths below about 440nm, which is greatly different from the absorption wavelength region of the UV absorber used in the UV laser stripping process described later. That is, free radical polymerization can be initiated by light of a longer wavelength with a small degree of UV curing hindrance caused by the added UV absorber. Therefore, even in the coexistence of a UV absorber, free radical polymerization can be initiated at a higher speed and efficiency for curing.
[0142] It is most preferred that the photoradical polymerization initiator can be selected based on absorbance. Specifically, the photoradical polymerization initiator can be selected from one or more compounds that satisfy any one or more of the following conditions: when dissolved at a concentration of 0.1% by mass in a solvent that does not have a maximum absorption in the wavelength region of 300nm to 500nm (e.g., acetonitrile, toluene, etc.), the absorbance at a wavelength of 365nm is 0.5 or more; the absorbance at a wavelength of 385nm is 0.5 or more; and the absorbance at a wavelength of 405nm is 0.5 or more. Examples of compounds satisfying such conditions include 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime) having an absorbance of 0.5 or more at a wavelength of 365 nm when dissolved in acetonitrile as a solvent at a concentration of 0.1% by mass, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime having an absorbance of 0.5 or more at wavelengths of 365 nm and 385 nm, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide having absorbances of 0.5 or more at wavelengths of 365 nm, 385 nm and 405 nm.
[0143] In addition, from the viewpoint of achieving both curability by a photoradical polymerization initiator and UV laser stripping, a double (η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium can also be used as a photoradical polymerization initiator.
[0144] From the viewpoint of reaction speed, heat resistance after curing, and low outgassing, the amount of the photoradical polymerization initiator (C) used is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the total of (A) to (B). If it is 0.01 parts by mass or more, sufficient curing properties can be obtained, and if it is 5 parts by mass or less, low outgassing and heat resistance will not be impaired.
[0145] In addition, the UV absorber that can be used as the (D) component refers to, for example, the following compounds: when irradiated with ultraviolet rays or visible light lasers, the molecules are cut and decomposed / gasified, and the decomposition / gasification occurs at the interface between the supporting substrate (or support body) and the temporary fixing agent, thereby causing the adhesive force between the temporary fixing agent and the supporting substrate (or support body) maintained until the peeling process is about to be carried out to be lost.
[0146] The (D) UV absorber is preferably at least one selected from benzotriazole compounds and hydroxyphenyltriazine compounds from the viewpoints of the degree of overlap with the UV laser wavelength in the UV absorption wavelength region, UV absorption characteristics at the wavelength, low outgassing, and heat resistance.
[0147] As the benzotriazole compound, in terms of compatibility with the resin component, UV absorption characteristics, low outgassing and heat resistance, it is particularly preferred to be one or more selected from the group consisting of 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl]benzotriazole.
[0148] As the hydroxyphenyltriazine-based compound, from the viewpoints of compatibility with the resin component, UV absorption characteristics, low outgassing and heat resistance, it is particularly preferred to use one or more selected from the group consisting of 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bisbutoxyphenyl)-1,3,5-triazine and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine.
[0149] In the case of providing a temporary fixing composition for a UV laser lift-off process of the present invention, the most preferred UV absorber is one or more selected from the group consisting of 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bisbutoxyphenyl)-1,3,5-triazine, or 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol]. These have excellent compatibility with the resin components (A) to (B), high melting points, and low vapor pressures under temperature conditions of about 300° C. or less. Therefore, they can be selected from a wide range of usage amounts and can contribute to reducing outgassing under the present temperature conditions from the temporarily fixing composition after curing.
[0150] As the UV absorber (D), the absorbers selected according to the UV transmittance listed below can be most preferably used. When the component (D) has such a UV transmittance, the effect of being able to appropriately control the curing and peeling of the composition can be obtained.
[0151] When the UV absorber is dissolved in a solvent having no maximum absorption at a wavelength of 290 to 410 nm at a concentration of 0.002 mass %, the transmittance at a wavelength of 355 nm is preferably 50% or less, and the transmittance at a wavelength of 385 to 420 nm is higher than 50% when the optical path length is 1 cm. It is more preferably 40% or less at a wavelength of 355 nm, and the transmittance at a wavelength of 385 to 420 nm is 60% or higher.
[0152] As the most preferable (D) UV absorber, for example, the following are mentioned.
[0153] 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (Tinuvin 900 manufactured by BASF, Adekastab LA-24 manufactured by Adeka, EVERSORB 76 / EVERSORB 234 manufactured by Everlight Chemical Co., Ltd., molecular weight 447) having a transmittance of 20% or less at a wavelength of 355 nm and a transmittance of 60% or more at a wavelength of 385 to 420 nm when dissolved in toluene used as a solvent at a concentration of 0.002 mass % at an optical path length of 1 cm.
[0154] 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinuvin 928 manufactured by BASF, EVERSORB 89 / 89FD manufactured by Everlight Chemical, molecular weight 442) which, when dissolved in toluene as a solvent at a concentration of 0.002 mass%, has a transmittance of 30% or less at a wavelength of 355 nm and a transmittance of 70% or more at a wavelength of 385 to 420 nm when the optical path length is 1 cm.
[0155] 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (Tinuvin 405 manufactured by BASF, molecular weight 584) which, when dissolved in tetrahydrofuran as a solvent at a concentration of 0.002 mass%, has a transmittance of 40% or less at a wavelength of 355 nm when the optical path length is 1 cm, and a transmittance of 90% or more at a wavelength of 385 to 420 nm.
[0156] 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine (Tinuvin 460 manufactured by BASF, molecular weight 630) which, when dissolved in tetrahydrofuran as a solvent at a concentration of 0.002 mass%, has a transmittance of 10% or less at a wavelength of 355 nm when the optical path length is 1 cm, and a transmittance of 80% or more at a wavelength of 385 to 420 nm.
[0157] The UV transmittance of the cured product in this specification is a value obtained by reflectivity spectrometry. Specifically, the transmittance is obtained under the following conditions using a film of a cured product having a thickness of about 50 μm made by sandwiching a sheet of PET resin and using a reflectivity spectrometer (V-650 manufactured by JASCO Corporation).
[0158] Cuvette length: 10mm
[0159] Metering mode: T (Transmittance)
[0160] Measuring range: 450-200nm
[0161] Data acquisition interval: 1nm
[0162] UV / vis bandwidth: 2.0nm
[0163] Response: medium
[0164] Scanning speed: 40nm / min
[0165] Light source switching: 340nm
[0166] Light source: D2 / WI
[0167] Filter switching: Step
[0168] Calibration: Baseline
[0169] The amount of the UV absorber as component (D) is preferably 0.01 to 5 parts by mass, more preferably 0.5 to 2.5 parts by mass, relative to 100 parts by mass of the total of (A) to (B). If it is 0.01 parts by mass or more, a sufficient UV laser stripping rate can be obtained, and if it is 5 parts by mass or less, low outgassing and heat resistance will not be impaired.
[0170] A composition having such characteristics can be preferably used in a back surface process after thinning, particularly in a process including a high-temperature vacuum process such as electrode formation by ion implantation, annealing, or sputtering.
[0171] When a cured film having a thickness of 50 μm is produced using the temporary fixing composition of the present invention, preferably at least one of the following conditions is satisfied, and more preferably all of the following conditions are satisfied. The following conditions can be satisfied, for example, by using a UV absorber or the above-mentioned photoradical polymerization initiator.
[0172] The light transmittance of the cured film is 70% or more in a wavelength region of 395 nm or more among the wavelengths of the light source used for curing.
[0173] The light transmittance of the cured film is 20% or more in a wavelength region of 385 nm or more and less than 395 nm among the wavelengths of the light source used for curing.
[0174] The light transmittance of the cured film at the wavelength (355 nm) of UV laser used for UV laser lift-off is 1% or less.
[0175] By satisfying these conditions, a curing speed and UV laser stripping speed that are sufficiently high for practical use can be achieved simultaneously. In addition, in addition to achieving a sufficiently high curing speed and UV laser stripping speed simultaneously, the ratio of mass reduction under heating conditions after curing can also be reduced (or the amount of outgassing under high-temperature vacuum can be reduced). A temporary fixing agent having such characteristics can be preferably used in a high-temperature vacuum process including electrode formation by ion implantation, annealing, or sputtering, especially in a back process after thinning.
[0176] In order to maintain the peelability after exposure to high temperature, the composition of the present invention may use an antioxidant. Examples of the antioxidant include methyl hydroquinone, hydroquinone, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), catechol, hydroquinone monomethyl ether, mono-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, p-benzoquinone, 2,5-diphenyl-p-benzoquinone, 2,5-di-tert-butyl-p-benzoquinone, picric acid, citric acid, phenothiazine, tert-butylcatechol, 2-butyl-4-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, and 4-((4,6-bis(octylthio)-1,3,5-triazin-2-yl)amino)-2,6-di-tert-butylphenol.
[0177] The amount of the antioxidant used is preferably 0.001 to 3 parts by mass relative to 100 parts by mass of the total of (A) to (D). If it is 0.001 parts by mass or more, the peelability after exposure to high temperature can be maintained, and if it is 3 parts by mass or less, good adhesion can be obtained without causing uncuring.
[0178] As a coating method for the composition, known coating methods such as spin coating, screen printing, and various coating machines can be used. As for the viscosity of the composition of the present invention, from the perspective of coating and operability, at 23°C (under atmospheric pressure), it is preferably 100mPa·s or more, more preferably 1000mPa·s or more, and most preferably 2000mPa·s or more. From the perspective of coating and operability, the viscosity of the composition of the present invention is preferably 10000mPa·s or less, more preferably 5000mPa·s or less, and most preferably 4000mPa·s or less. If it is 100mPa·s or more, the coating, especially the coating based on spin coating, is excellent. If it is 10000mPa·s or less, the operability is excellent.
[0179] Spin coating refers to a method in which, for example, a liquid composition is dripped onto a substrate and the substrate is rotated at a predetermined rotation speed to apply the composition onto the surface of the substrate. Spin coating can efficiently produce a high-quality coating film.
[0180] The composition of the present invention can be used as a temporary fixing resin composition, a temporary fixing adhesive, an adhesive sheet, or a temporary fixing adhesive for electronic device manufacturing. In the present invention, the temporary fixing composition, the temporary fixing resin composition, and the temporary fixing adhesive are sometimes collectively referred to as a temporary fixing agent.
[0181] When the composition of the present invention is used to bond a substrate to be processed to an optically transparent supporting substrate (or support), it is preferred that the composition be applied to the substrate at an energy of 1 to 20,000 mJ / cm2 under visible light or ultraviolet light (wavelength or center wavelength 365 to 405 nm). 2 If the energy is 1mJ / cm 2 If the adhesiveness is above 20000mJ / cm 2 The productivity is excellent, the decomposition products from the photo-radical polymerization initiator are not easily generated, and the generation of outgassing can be suppressed. From the perspective of productivity, adhesion, low outgassing, and easy peelability, 1000 to 10000 mJ / cm 2 .
[0182] The substrate bonded by the composition of the present invention is not particularly limited, and preferably at least one substrate is a transparent substrate that transmits light. As the transparent substrate, inorganic substrates such as crystal, glass, quartz, calcium fluoride, magnesium fluoride, organic substrates such as plastics, etc. can be cited. Among these, from the aspect of having versatility and obtaining a large effect, preferably an inorganic substrate. Among the inorganic substrates, preferably one or more selected from glass and quartz.
[0183] In one embodiment, the composition of the present invention is a photocurable type, and the cured product provided thereby has excellent heat resistance and peelability. In one embodiment, the cured product of the composition of the present invention has a small amount of outgassing even when exposed to high temperatures, and is suitable for joining, sealing, and coating of various optical components, optical devices, and electronic components. The composition of the present invention is suitable for applications requiring durability in many aspects such as solvent resistance, heat resistance, and adhesion, especially for semiconductor manufacturing processes.
[0184] The cured body of the composition of the present invention can be used in processes with a wide temperature range from room temperature to high temperature. The heating temperature in the process is preferably below 350°C, more preferably below 300°C, and most preferably below 250°C. In a preferred embodiment, the temperature at which the heating mass reduction rate of the cured body becomes 2% can be above 250°C. The bonded body bonded by the temporary fixing adhesive of the present invention has a high shear adhesion, so it can withstand thinning processes, etc., and can be easily peeled off after a heating process such as insulating film formation. When used at high temperatures, the cured body of the composition of the present invention can be used in high-temperature processes, for example, preferably above 200°C, more preferably above 250°C.
[0185] Furthermore, in one embodiment of the present invention, the following effects can be achieved: a bonded body formed by bonding substrates with an adhesive can be peeled off by applying external force to the bonded body, for example, by inserting a blade, sheet or wire into the bonded portion.
[0186] Furthermore, in one embodiment of the present invention, an adhesive body obtained by bonding substrates with an adhesive can be peeled by irradiating the adhesive body with UV laser or IR laser in a manner of scanning the entire surface of the optically transparent substrate side.
[0187] <Method for Manufacturing Thin Wafer>
[0188] In an embodiment of the present invention, a method for manufacturing a thin wafer can also be provided. The manufacturing method is characterized in that the above-mentioned temporary fixing composition or temporary fixing adhesive (hereinafter sometimes referred to as adhesive or temporary fixing agent) is used as an adhesive layer between a wafer having a semiconductor circuit and a support. The manufacturing method of a thin wafer of the present invention has the following steps (a) to (e).
[0189] [Step (a)]
[0190] Process (a) is the following process: when the circuit-forming surface of a chip having a circuit-forming surface on the surface and a circuit-non-forming surface on the back is joined to a supporting body via an adhesive, the adhesive is applied on the supporting body or the chip with the circuit by spin coating, and then bonded to another supporting body or chip with the circuit under vacuum.
[0191] The wafer having a circuit forming surface and a circuit non-forming surface is a wafer having a circuit forming surface on one side and a circuit non-forming surface on the other side. The wafer to which the present invention can be applied is usually a semiconductor wafer. As the semiconductor wafer, not only silicon wafers but also gallium nitride wafers, lithium tantalate wafers, lithium niobate wafers, silicon carbide wafers, germanium wafers, gallium-arsenic wafers, gallium-phosphorus wafers, gallium-arsenic-aluminum wafers, etc. can be mentioned. The thickness of the wafer is not particularly limited, but is preferably 600 to 800 μm, and more preferably 625 to 775 μm. As a support, for example, a transparent substrate that transmits light can be used.
[0192] [Step (b)]
[0193] Step (b) is a step of photocuring the adhesive. After forming the above-mentioned wafer processing body (laminated substrate), it is preferred to cure the adhesive with an energy of 1 to 20,000 mJ / cm in the visible light or ultraviolet light region (the wavelength or central wavelength is preferably 350 to 405 nm, more preferably 365 to 405 nm, and most preferably 385 to 405 nm). 2 If the energy is 1mJ / cm 2 If the adhesiveness is above 20000mJ / cm 2 The productivity is excellent, the decomposition products from the photo-radical polymerization initiator are not easily generated, and the generation of outgassing can also be suppressed. From the perspective of productivity, adhesion, low outgassing, and easy peelability, 1000 to 10000 mJ / cm is more preferred. 2 .
[0194] When curing the composition, a black light lamp, UV-LED, or visible light-LED may be used as a light source, and for example, the following light sources may be used. As a black light lamp, a lamp containing a component having a wavelength of 385 nm or more may be preferably used regardless of its central wavelength. It should be noted that in this specification, when a wavelength range is described, whether it is included in the range is determined based on whether the central wavelength is included in the range.
[0195] Black light (central wavelength 365nm, illumination 10mW / cm 2 , TUV-8271 manufactured by Toyo adtechno Co., Ltd.)
[0196] UV-LED (wavelength 385±5nm, illumination 350mW / cm 2 (Conditions: Working distance from the front end of the mirror unit 20mm), H-4MLH200-V2-1S19 + dedicated mirror unit manufactured by HOYA Corporation)
[0197] UV-LED (wavelength 395±5nm, illumination 375mW / cm2 (Conditions: Working distance from the front end of the mirror unit 20 mm), H-4MLH200-V3-1S19 + dedicated mirror unit manufactured by HOYA Corporation)
[0198] UV-LED (wavelength 405±5nm, illumination 400mW / cm 2 (Conditions: working distance from the front end of the mirror unit 20mm), HOYA Corporation H-4MLH200-V4-1S19 + dedicated mirror unit)
[0199] UV-LED (Central wavelength 405nm, illumination 10mW / cm 2 , HLDL-120V0-NWPSC made by CCS)
[0200] Visible light-LED (wavelength 451±5nm, illumination 550mW / cm 2 (Conditions: working distance from the front end of the irradiation unit 10 mm), HLDL-155VL450-PSC manufactured by CCS Corporation)
[0201] Visible light-LED (wavelength 492±5nm, illumination 400mW / cm 2 (Conditions: working distance from the front end of the irradiation unit 10 mm), HLDL-155BG-PSC manufactured by CCS Corporation)
[0202] In a preferred embodiment, compared with a black light lamp, which has a tendency to have a large cumulative light amount and a long irradiation time due to a generally wide irradiation wavelength, a UV-LED or a visible light-LED with a small cumulative light amount (short irradiation time) is preferably used as a light source. That is, by using an LED light source with a narrow irradiation wavelength band, the following effect can be obtained: temporary fixing can be performed in a short time, and as a result, the time consumed in the manufacturing process can be shortened.
[0203] [Step (c)]
[0204] Step (c) is a step of grinding and / or polishing the non-circuit forming surface of the wafer bonded to the support, that is, a step of grinding the back side of the wafer of the wafer processing body obtained by bonding in step (a) to thin the thickness of the wafer. The thickness of the thinned wafer is preferably 10 to 300 μm, more preferably 30 to 100 μm. There is no particular restriction on the method of grinding / polishing the back side of the wafer, and a known grinding / polishing method can be used. Grinding is preferably performed while cooling by applying water to the wafer and the grindstone (a grindstone with a diamond blade, etc.).
[0205] [Step (d)]
[0206] Process (d) is a process for processing a wafer processing body whose non-circuit forming surface has been ground / polished, that is, a wafer processing body whose non-circuit forming surface has been thinned by back grinding / polishing. This process includes various processes used at the wafer level. For example, electrode formation, metal wiring formation, protective film formation, etc. can be cited. More specifically, the following can be cited: metal sputtering for forming electrodes, etc.; wet etching for etching a metal sputtering layer; application of a resist for preparing a mask for forming metal wiring; pattern formation by exposure and development; stripping of the resist; dry etching; formation of a metal plating layer; silicon etching for forming TSV; oxide film formation on the silicon surface; and other previously known processes.
[0207] [Step (e)]
[0208] Step (e) is a stripping step. This step is a step of stripping the wafer processed in step (d) from the wafer processing body. For example, it is a step of stripping the wafer from the wafer processing body before cutting after various processes are performed on the thinned wafer. At this time, a dicing tape can be affixed to the thinned and processed surface in advance. The stripping step is usually carried out under relatively low temperature conditions of room temperature to about 60°C. As the stripping step, any of the known UV laser stripping steps, IR laser stripping steps, or mechanical stripping steps can be used.
[0209] The so-called UV laser stripping process refers to a process in which, for example, a UV laser is irradiated on the entire surface in a manner of scanning back and forth in a straight line along the tangent direction from the end of the optically transparent support body side of the wafer processing body, and the adhesive layer is decomposed and stripped by the energy of the laser. Such a stripping process is described in, for example, Japanese Patent Table No. 2019-501790 and Japanese Patent Table No. 2016-500918. The temporary fixing composition of the present invention is particularly suitable for the UV laser stripping process by including the (D) component and satisfying the preferred requirements of the above-mentioned (C) component and / or (D) component.
[0210] The so-called IR laser stripping process refers to a process in which, for example, the adhesive layer is heated and decomposed by the energy of the laser light and then stripped by irradiating the entire surface with IR laser light in a manner of scanning back and forth in a straight line along the tangent direction from the end of the optically transparent support body side of the wafer processing body. Such a stripping process is described in, for example, Japanese Patent Gazette No. 4565804. In order to implement the IR laser stripping process, a light-to-heat conversion layer (for example, 3M's LTHC; Light-To-Heat-Conversion release coating) that absorbs IR laser light and converts it into heat can be provided between the temporary fixing agent layer and the glass support body. When using 3M's LTHC, for example, the LTHC can be spin-coated on a glass support body and cured, and the temporary fixing agent layer can be bonded to the above-mentioned glass support body on which the LTHC layer is formed after being spin-coated on the wafer, and UV curing is performed. The method of implementing the IR laser stripping process using 3M's LTHC is described, for example, in the same Japanese Patent Gazette No. 4565804 as described above.
[0211] The so-called mechanical stripping process, for example, refers to a stripping process including the following steps: inserting a blade into the interface end of the wafer processing body, in order to cause cracking between the wafer and the support body, the wafer of the wafer processing body is previously fixed horizontally with the wafer facing downward, and after the blade is inserted, an upward stress is applied to the upper support body and / or the blade to develop the above cracking and to strip the wafer and the support body. Such a stripping process is described in, for example, Japanese Patent No. 6377956 and Japanese Patent Publication No. 2016-106404.
[0212] When the composition involved in the embodiment of the present invention is peeled off, any one of the above-mentioned peeling methods can be used. At this time, it is preferred to fix one of the wafer or the support of the wafer processing body horizontally in advance, insert a blade, or use a solvent (for example, a solvent of aliphatic or aromatic hydrocarbons such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) to swell the periphery of the adhesive layer, make the start of peeling, and then lift the other from the horizontal direction at a certain angle. The above-mentioned peeling method is usually implemented at room temperature, preferably heated at an upper limit of about 90°C. When using a laser, it is preferred to use a YAG laser or a YVO4 laser.
[0213] The step (e) of peeling the processed wafer from the support body preferably further comprises, in the case of a mechanical peeling step:
[0214] (f) a step of bonding a dicing tape to a wafer surface of a wafer on which processing has been performed;
[0215] (g) vacuum-adsorbing the dicing tape surface onto the adsorption surface; and
[0216] (h) A step of peeling the support body from the processed wafer while the temperature of the adsorption surface is in the temperature range of 10 to 100°C.
[0217] By performing the above steps, the support body can be easily peeled off from the processed wafer, and the subsequent dicing step can be easily performed.
[0218] In addition, when the peeling is performed using a UV laser or an IR laser, the manufacturing method preferably further includes, for example:
[0219] (i) placing / fixing the processed wafer in a horizontal position preferably via a dicing tape with the optically transparent support facing upward; and
[0220] (j) A step of irradiating the entire surface of the processed wafer by scanning with a laser beam from the support body side thereof.
[0221] By performing the above steps, the support body can be easily peeled off from the processed wafer, and the subsequent dicing step can be easily performed.
[0222] In addition, after the step (e) of peeling the processed wafer from the support using UV laser or IR laser, it is necessary to perform:
[0223] (k) A step of removing the temporary bonding agent remaining on the wafer surface.
[0224] As a method for removing the temporary fixing agent, there are the following methods: a method in which an adhesive tape such as a dicing tape is attached to the entire surface of the other side where the temporary fixing agent remains, while the thinned surface is vacuum-adsorbed on the adsorption surface, and the temporary fixing agent is peeled off together with the tape; and a method in which the wafer is immersed in a solvent (for example, aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) to swell the adhesive layer and then peel it off. Among the above methods, the tape peeling method is preferred in terms of the small number of steps and the short time required.
[0225] After the temporary fixative is removed, the wafer can also be directly processed into the next step without cleaning the surface. In the case of cleaning, it is preferred to also perform:
[0226] (l) A process of cleaning the chip from which the support and temporary fixing agent have been removed, with the circuit forming surface facing upward, using a solvent (for example, aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.).
[0227] On the circuit forming surface of the wafer from which the temporary fixing agent has been removed by step (k), a portion of the adhesive (temporary fixing agent) may remain. In addition, the peeled support is preferably reused after cleaning, but sometimes adhesive residues are also fixed on the surface of the support. As a method for removing these adhesive residues, there can be cited a method of immersing the support in a solvent (for example, aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) to make it swell and then peel it off.
[0228] In one embodiment, when the above composition is cured to obtain a cured product, various methods as described below can be employed.
[0229] First, as a first method, a layer formed of a temporary fixing composition containing components (A) to (D) can be cured to obtain a single-layer cured body.
[0230] In addition, as a second method, the following method can be cited: prepare a first layer formed by a temporary fixing composition containing components (A-1), (A-2), (B), and (C) and excluding component (D), and a second layer formed by a temporary fixing composition containing components (A) to (D), and cure them to obtain an integrated solidified body having a single layer or multiple layers (plural layers). In the solidified body, it is preferred that the concentration distribution of the components is different in the thickness direction; or the concentration distribution of the components is different on the upper surface and the lower surface in the thickness direction of the solidified body. The different concentration distribution of the components can be confirmed by the following method: using the above-mentioned reflectivity measurement spectrometry, the UV transmittance is quantified for both sides of the solidified body. Using this method, layers with different light transmittance are combined, thereby achieving the best curing effect. In addition, during the above-mentioned curing, a black light lamp or UV-LED can be used as a light source (the same applies to the following method). An example of a black light lamp is TUV-8271 (central wavelength 365 nm, illuminance 10 mW / cm 2 In addition, as UV-LED, there is H-4MLH200-V2-1S19+special design mirror unit (wavelength 385±5nm, illumination 350mW / cm 2 , conditions: scanning distance from the front end of the mirror unit 20mm), HOYA Corporation H-4MLH200-V3-1S19 + dedicated design mirror unit (wavelength 395±5nm, illumination 375mW / cm 2 , conditions: working distance from the front end of the mirror unit 20mm), HOYA Corporation H-4MLH200-V4-1S19 + dedicated design mirror unit (wavelength 405±5nm, illumination 400mW / cm 2, condition: working distance from the front end of the mirror unit is 20mm) such a lamp.
[0231] In addition, as the third method, the following method can also be used: on a solidified layer formed by a temporary fixing composition comprising (A-1) component, (A-2) component, (B) component, and (C) component, coating (e.g., coating by spin coating) (D) component is applied to obtain a solidified body with a monolayer that is at least partially integrated. In this case, the concentration distribution of the components of the solidified body is different in the thickness direction. With regard to the concentration distribution of the components, as mentioned above, it can be quantitatively measured by spectrometry of the reflectivity of each object layer. Utilizing this method, an effect that can accurately control the UV absorption characteristics can be obtained.
[0232] In addition, as a fourth method, a layer of a commercially available LTHC agent (light-to-heat conversion agent) may be placed on a layer formed of the temporary fixing composition comprising the components (A-1), (A-2), (B), and (C) and cured to obtain a multilayer cured product. This can easily obtain a cured product.
[0233] The cured product obtained by the above-mentioned method can be combined with an adherend to provide a structure.
[0234] Various examples can be given as methods for manufacturing the above-mentioned structure. For example, the first manufacturing method may include: a step of applying a first temporary fixing composition containing components (A-1), (A-2), (B), and (C) and excluding component (D) on a wafer and partially curing the composition; a step of applying a second temporary fixing composition containing components (A) to (D) on the partially cured temporary fixing composition; and a step of further placing a transparent substrate on the applied second temporary fixing composition and photocuring the composition.
[0235] In addition, as a second method for manufacturing a structure, there may be a method comprising the following steps: a step of applying a first temporary fixing composition containing components (A-1), (A-2), (B), and (C) and excluding component (D) on a chip and partially curing it as needed; a step of applying a second temporary fixing composition containing components (A) to (D) on a transparent substrate and partially curing it as needed; and a step of bringing the surfaces of the chip and the transparent substrate coated with the temporary fixing composition into close contact with each other and then bonding them by photocuring.
[0236] In addition, as a third method for manufacturing a structure, there may be a method comprising the following steps: a step of coating a temporary fixing composition containing components (A-1), (A-2), (B), and (C) but excluding component (D) on a chip and partially curing it as needed; a step of coating an LTHC layer on a transparent substrate, drying it, and curing it; and a step of bringing the surface of the chip coated with the temporary fixing composition into close contact with the surface of the transparent substrate coated with the LTHC layer and then bonding them by photocuring.
[0237] In addition to the temporary fixing composition described above, the same composition as that used in the temporary fixing composition of the present invention can also be used as a raw material for a light-to-heat conversion (LTHC) layer that absorbs IR laser light and converts it into heat as described in Japanese Patent No. 4565804. By adding the composition as a component of the light-to-heat conversion (LTHC) layer, its heat resistance can be improved.
[0238] As another aspect of the present invention, a method for manufacturing a semiconductor wafer can be provided, which includes: applying a temporary fixing adhesive to a semiconductor wafer substrate and / or a supporting member to bond the semiconductor wafer substrate to the supporting member; curing the temporary fixing adhesive by irradiating light with a wavelength of 350 to 700 nm (preferably 365 to 500 nm or 385 to 700 nm, more preferably 385 to 450 nm) to obtain an adhesive body; and irradiating the adhesive body with a laser with a wavelength less than 385 nm (preferably a laser with a wavelength of 200 nm or more and less than 385 nm) to peel off the semiconductor wafer substrate. The curing and peeling steps of this manufacturing method are both processes at room temperature, and there is no need to heat or cool the parts, and usually no need to use solvents, etc., and it has the advantages of being simple and having a short cycle time.
[0239] In addition, the cured temporary fixing adhesive may constitute a single layer in the above-mentioned adhesive body. In this way, the process can be simplified and the cycle time can be shortened.
[0240] As a temporary fixing adhesive preferably used in this manufacturing method, a temporary fixing agent containing a UV curable monomer, a (C) photo radical polymerization initiator component selected according to the above absorbance, and a (D) UV absorber component selected according to the UV transmittance can be used. Here, as the UV curable monomer, a monofunctional (meth)acrylate or a multifunctional (meth)acrylate is preferred, and the above components (A-1) and (A-2) are most preferred. It can also contain the above-mentioned (B) polyisobutylene homopolymer and / or polyisobutylene copolymer, or a known resin component used in a temporary fixing adhesive in the past.
[0241] In a preferred embodiment, by making the composition contain the above-mentioned preferred (C) photoradical polymerization initiator component and (D) UV absorber component, even if it is a single-layer temporary fixing adhesive, it is possible to achieve both a fast curing speed and a fast peeling speed. In addition, the uncured UV curable monomer components remaining in the cured body when the temporary fixing adhesive is UV cured can be significantly reduced, the heat resistance of the cured body can be improved, and the volatile components under vacuum can be reduced. That is, for example, the 2% heating mass reduction temperature in the Tg / DTA measurement of the cured body can be increased. Temporary fixing adhesives with high heat resistance of the cured body and reduced volatile components under vacuum are extremely useful for recent semiconductor manufacturing processes.
[0242] Example
[0243] Hereinafter, the present invention will be described in more detail with reference to experimental examples, but the present invention is not limited to these.
[0244] (Experimental example)
[0245] Unless otherwise specified, the experiment was conducted at 23°C and 50% humidity. Curable resin compositions (hereinafter sometimes referred to as liquid resin compositions) having the compositions (unit: parts by mass) shown in Tables 1, 2, and 4 were prepared and evaluated. The following compounds were selected as the components in the curable resin compositions described in the experimental examples.
[0246] (composition)
[0247] As the monofunctional acrylate having a homopolymer Tg of -100°C to 60°C (A-1), the following compounds were selected.
[0248] Isostearyl acrylate ("ISTA" manufactured by Osaka Organic Chemical Industry Co., Ltd., glass transition temperature of homopolymer: -18°C, molecular weight 325)
[0249] 2-Dodecyl-1-hexadecyl acrylate ("Light Acrylate DHD-A (DHD-A)" manufactured by Kyoeisha Chemical Co., Ltd., glass transition temperature of homopolymer: -23°C, molecular weight 465)
[0250] 2-Tetradecyl-1-octadecyl acrylate ("Light Acrylate DOD-A (DOD-A)" manufactured by Kyoeisha Chemical Co., Ltd., glass transition temperature of homopolymer: -8°C, molecular weight 521)
[0251] 2-Decyl-1-tetradecyl acrylate ("Light Acrylate DTD-A (DTD-A)" manufactured by Kyoeisha Chemical Co., Ltd., glass transition temperature of homopolymer: -36°C, molecular weight 409)
[0252] As the (A-2) multifunctional acrylate, the following compounds were selected.
[0253] Tricyclodecane dimethanol diacrylate ("NK ESTER A-DCP (A-DCP)" manufactured by Shin-Nakamura Chemical Co., Ltd., molecular weight 304)
[0254] As (B) the polyisobutylene homopolymer and / or the polyisobutylene copolymer, the following compounds are selected.
[0255] As the polyisobutylene homopolymer, the following compounds were selected.
[0256] Oppanol N 50SF (manufactured by BASF, weight average molecular weight (Mw) based on PS conversion: 565,000, molecular weight distribution 2.4)
[0257] As the polyisobutylene-polystyrene block copolymer, the following compounds were selected.
[0258] SIBSTAR 103T (manufactured by Kaneka Corporation, polystyrene-polyisobutylene-polystyrene triblock copolymer, weight average molecular weight (Mw) in terms of PS: 100,000, molecular weight distribution 2.0, total mass ratio of polystyrene segments 30%)
[0259] Epyon EP400V (manufactured by Kaneka Corporation, polyisobutylene modified with acrylic acid at both ends, weight average molecular weight (Mw) in terms of PS: 17,000, molecular weight distribution 1.2)
[0260] As (C) the photoradical polymerization initiator, the following compounds were selected.
[0261] Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide ("Irgacure 819" manufactured by BASF)
[0262] As the (D) UV absorber, the following compounds were selected.
[0263] 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (Tinuvin 900 manufactured by BASF, Adekastab LA-24 manufactured by Adeka Corporation, EVERSORB 76 / EVERSORB 234 manufactured by Everlight Chemical Co., Ltd., molecular weight 447)
[0264] 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinuvin 928 manufactured by BASF, EVERSORB 89 / 89FD manufactured by Everlight Chemical, molecular weight 442)
[0265] 2-[2-Hydroxy-3-(3,4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl]benzotriazole (Sumisorb 250 manufactured by Sumika Chemtex Co., Ltd., molecular weight 389)
[0266] 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (Tinuvin 405 manufactured by BASF, molecular weight 584)
[0267] 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bisbutoxyphenyl)-1,3,5-triazine (Tinuvin 460 manufactured by BASF, molecular weight 630)
[0268] As the antioxidant, the following compounds were selected.
[0269] 4-((4,6-bis(octylthio)-1,3,5-triazin-2-yl)amino)-2,6-di-tert-butylphenol ("IRGANOX 565" manufactured by BASF)
[0270] (Liquid sample preparation)
[0271] The materials were mixed with heating at 80°C, thereby preparing a uniform mixture.
[0272] (Preparation of curing samples using black light)
[0273] The liquid resin composition homogenized by heating and mixing was sandwiched between PET films and spread to a thickness of 50 μm (0.5 mm for the sample for elastic modulus measurement described later). 2 The solidified body was prepared by curing it under the conditions of . A black light lamp (central wavelength 365nm, illumination 10mW / cm 2 , TUV-8271 manufactured by Toyoadtechno Co., Ltd.).
[0274] (Curing sample made using 405nm UV-LED)
[0275] The liquid resin composition homogenized by heating and mixing was sandwiched between PET films and spread to a thickness of 50 μm (0.5 mm for the sample for elastic modulus measurement described later). 2 The cured product was prepared by curing with UV-LED (central wavelength 405nm, illumination 100mW / cm 2 , HLDL-120V0-NWPSC made by CCS Company).
[0276] Preparation process of test body for evaluating suitability of UV laser stripping process: In an automatic wafer bonding machine, the prepared liquid resin composition is spin-coated on an 8-inch silicon wafer (diameter 200mm×thickness 0.725mm) with a thickness of 50μm, and then bonded with an 8-inch glass wafer (diameter 201mm×thickness 0.7mm) under a reduced pressure of 10Pa in the device. After bonding, the liquid resin compound is cured from the glass wafer side using any of the above-mentioned UV light sources to obtain a bonded body. Next, the silicon wafer surface of the obtained bonded body is ground and polished, and after being thinned to a thickness of 50μm, it is heated for 1 hour at a high temperature and reduced pressure of 250℃·13Pa.
[0277] Preparation process of the test body for evaluating the suitability of the IR laser peeling / mechanical peeling process: Use the prepared liquid resin composition to bond a 4-inch silicon wafer (100 mm in diameter × 0.47 mm in thickness) to a 4-inch glass wafer (100 mm in diameter × 0.7 mm in thickness), spread the liquid resin composition until it is spread over the entire surface between the substrates with a thickness of 50 μm, and use any of the above light sources at a cumulative light intensity of 5000 to 10000 mJ / cm 2 The film was cured under the conditions of , and a peeling / disassembly test piece was prepared. The light for curing was irradiated from the surface of a 4-inch glass wafer.
[0278] (evaluate)
[0279] Compatibility of materials of liquid resin composition ("Compatibility of materials", "Absorbance" in Tables 1, 2 and 4): The temporary fixing composition homogenized by heating and mixing is cooled to 23°C to confirm whether the uniform state is maintained. The absorbance (OD660) of the sample placed in a cuvette with a width of 10 mm in the direction of the optical path length is measured at a wavelength of 660 nm using a UV-visible spectrophotometer V-650 manufactured by JASCO Corporation. When the absorbance is less than 0.1, it is compatible and recorded as acceptable. When the absorbance is greater than 0.1 and when inhomogeneities such as phase separation are visually confirmed, it is incompatible and recorded as unacceptable. From the perspective of compatibility, the absorbance is preferably less than 0.1. It should be noted that for examples of "unacceptable", subsequent evaluations are omitted. The same applies to the following.
[0280] Viscosity ("Suitability of Spin Coating Process", "Viscosity" in Tables 1, 2, and 4): The viscosity of the liquid resin composition maintained in a uniform state at 23°C in the above "Material Compatibility" was measured to evaluate the suitability of spin coating on the upper surface of the substrate in the actual process. The viscosity was measured at 23°C using a rheometer MCR302 manufactured by Anton-Paar and a cone-plate CP50-2. The shear rate was set to 1s -1 The case where the shear viscosity is 1000mPa·s or more and less than 4000mPa·s is considered excellent, the case where it is 4000mPa·s or more than 1000mPa·s or less than 100mPa·s is considered acceptable, and the case where it exceeds 10000mPa·s or is less than 100mPa·s is considered unacceptable. From the perspective of suitability for the spin coating process, the viscosity is preferably 100 to 10000mPa·s. It should be noted that the subsequent evaluation is omitted for the example of being "unacceptable". The same applies to the following.
[0281] Heating mass reduction rate of the cured product (“Heat resistance 1”, “2% heating mass reduction temperature of the cured product” in Tables 1, 2, and 4):
[0282] For the obtained solidified body 10mg, the temperature was raised from 30°C to 350°C at a heating rate of 10°C / min under a nitrogen flow, and then continued to rise from 350°C to 800°C at a heating rate of 20°C / min under an air flow, using the differential thermal and thermal mass simultaneous measurement device "TG-DTA2000SA" manufactured by Bruker-AXS Co., Ltd. The heating mass reduction rate of the obtained solidified body was measured. The 2% heating mass reduction temperature of the solidified body is displayed. The case where a value of 250°C or more is displayed is excellent, the case where a value of 200°C or more and less than 250°C is displayed is good, the case where a value of 150°C or more and less than 200°C is displayed is acceptable, and the case where a value of less than 150°C is displayed is unacceptable. From the perspective of suitability for high-temperature processes in semiconductor manufacturing, the temperature at which the heating mass reduction rate becomes 2% is preferably 150°C or more, and more preferably 250°C or more. It should be noted that for the example of becoming "unacceptable", subsequent evaluations are omitted. The same is true below.
[0283] Elastic modulus range of the solidified body (“Heat resistance 2” and “Storage elastic modulus at -50 to 250°C” in Tables 1, 2, and 4): The dynamic viscoelasticity of the solidified body sample was measured using the viscoelasticity measuring device RSA-G2 manufactured by TA Instrument Japan Co., Ltd. The measurement was carried out under the conditions of a chuck distance of 10 mm, a sample width of 8 mm, a sample thickness of 0.5 mm, a strain of 0.1%, a tensile frequency of 1 Hz, a heating rate of 3°C / min, and a temperature range of -50 to 250°C. Under these conditions, samples whose storage elastic modulus E' is greater than 10 kPa in the entire temperature range are considered acceptable, and samples whose storage elastic modulus E' is less than 10 kPa in any temperature range are considered unacceptable. The elastic modulus is preferably greater than 10 kPa. It should be noted that for examples of being "unacceptable", subsequent evaluations are omitted. The same applies to the following.
[0284] Adhesion at high temperature ("Adhesion under high temperature conditions (250°C 1h 30Pa reduced pressure)", "Width of discoloration at the outer edge", "Peeling by heating" in Tables 1, 2, and 4): A 4-inch silicon wafer (10 cm in diameter × 0.47 mm in thickness) was bonded to a 4-inch glass wafer (10 cm in diameter × 0.7 mm in thickness) using the prepared liquid resin composition. During bonding, the thickness of the resin composition was adjusted by adding 0.1% by mass of silica particles (trade name Hipresica TS N3N, average particle size 50 μm) manufactured by UbeExsymo to a temporary fixing agent and mixing the mixture. After bonding, at a cumulative light intensity of 10,000 mJ / cm 2 The adhesive was cured under the conditions of , and a test piece for evaluating the adhesion under high temperature and reduced pressure was prepared. The adhesive was applied to the entire surface of the bonding surface. The black light was irradiated from the surface of a 4-inch glass wafer. The completed test piece was placed on a heating plate preheated to a specified temperature with the 4-inch silicon wafer side facing down, and the width of the discolored area at the outer edge toward the center of the wafer and the presence or absence of peeling that could be visually confirmed from the glass side were observed. Under a reduced pressure of 30Pa, the temperature of the heating plate was set to 250°C, and the heating duration was set to 1 hour. In the "Adhesion under high temperature conditions (250°C·1h·reduced pressure 30Pa)" of the table, the case where the width extending from the outer edge of the discolored area to the center under each temperature condition is less than 5mm and no peeling is observed (the "peeling based on heating" in the table is "none") is considered acceptable, and the case where the width exceeds 5mm and peeling is observed is considered unacceptable. The width extending from the outer edge of the discolored area to the center is preferably less than 5mm. The color change indicated here refers to a color change confirmed due to a change caused by the temporary fixing agent peeling off from any of the glass and silicon substrates.
[0285] (1)Suitability of UV curing process and UV laser stripping process (“light transmittance” in Tables 1 and 2):
[0286] The light transmittance of the obtained cured film having a thickness of 50 μm was measured in the wavelength range of 200 nm to 450 nm. The case where all the following conditions were satisfied was deemed acceptable, and the case where only two or less of the conditions were satisfied was deemed unacceptable.
[0287] [1] The light transmittance in the wavelength range above 395nm is 70% or more
[0288] [2] The light transmittance in the wavelength range of 385nm to less than 395nm is 20% or more
[0289] [3] Transmittance at a wavelength of 355nm is less than 1%
[0290] (1) Suitability of UV laser peeling process ("UV laser peeling performance", "minimum time required to achieve complete peeling" in Tables 1, 2, and 4, and "UV laser irradiation conditions" in Table 3): The entire surface of the obtained 8-inch test body is scanned from the glass support side of the test body, and the 210 mm square area with the test body fixed in the center is irradiated with UV laser. As UV laser irradiation conditions, the conditions shown in Table 3 were applied to the embodiments of Table 1 in turn and evaluated. For UV laser, the output power was 9.3 W, the pulse energy was 235 μJ, and the energy density was 11968 mJ / cm 2 QLA-355 (wavelength 355 nm) manufactured by Quark Technology Co., Ltd. was used under the conditions shown in condition number 9 of Table 3, such as frequency 40 kHz, beam diameter (spot diameter) 50 μm, scanning pitch 500 μm, and scanning speed 20 m / s (Table 3 records the attempt to study the optimal conditions). As for the peelability after irradiation, the situation where the adhesive force is completely lost and the glass support body is in a state of free sliding (or moving) on the silicon wafer (adhesion = 0) is defined as complete peeling, and the suitability of the UV laser peeling process is evaluated by the minimum value of the required time of the UV laser irradiation process required to obtain the complete peeling state. The situation where the minimum value of the required time is less than 15 seconds is excellent, the situation where it is more than 15 seconds and less than 30 seconds is good, the situation where it is more than 30 seconds and less than 60 seconds is acceptable, and the situation where it is more than 60 seconds is unacceptable.
[0291] (2) Evaluation of suitability of IR laser lift-off process: This method can use, for example, the method described in Japanese Patent Gazette No. 4565804. Japanese Patent Gazette No. 4565804 describes a method of using a light-to-heat conversion layer (LTHC layer) that absorbs light and converts it into heat, such as described in Japanese Patent Gazette No. 4405246, together with a liquid resin composition. The LTHC layer is formed by coating on the surface of a support and curing. Japanese Patent Gazette No. 4565804 describes the following method: the LTHC layer-forming surface side of a support having an LTHC layer formed on the surface is joined to the liquid resin composition-coated surface of a silicon wafer spin-coated with a liquid resin composition, UV irradiation is performed from the support side to cure it, the laminate produced by this method is fixed to a fixing device in such a way that the support is the upper surface, and YAG laser or semiconductor laser is irradiated from the upper surface to disintegrate it. The disintegration is carried out in the following manner: the LTHC layer absorbs the light energy of the IR laser and converts it into heat, and the heat decomposes and vaporizes the adjacent resin layer, and the gas layer generated by the vaporization eliminates the adhesive force between the support and the resin layer. The peelability after IR laser irradiation can be evaluated by the same method as the evaluation of the peelability after UV laser irradiation.
[0292] (3) Mechanical peeling process suitability ("Mechanical peeling (possible / unacceptable)" in Tables 1 and 2): A PET sheet was inserted between the two substrates of a test body similar to the sample for evaluating adhesion at high temperature described above, and the test body was attached to a dicing tape (ERK-3580 manufactured by Denka Co., Ltd.) with the silicon wafer facing downward. While the attached object was placed on a vacuum chuck and fixed, a suction cup with a diameter of 50 mm was attached to the end of the test body, and the measuring part of an electronic spring balance was installed in the center of the suction cup. The balance was lifted vertically upward, and the peeling property was evaluated by this method. The case where the force required for peeling (adhesive force) exceeded 50 N, or the case where the PET sheet could not be inserted was regarded as unacceptable.
[0293] [Table 1]
[0294]
[0295] [Table 2]
[0296]
[0297] [Table 3]
[0298] UV laser irradiation conditions Equipment: QLA-355 GAUSSIAN BEAM manufactured by Quark Technology
[0299] Condition Number 1 2 3 4 5 6 7 8 9 Working distance (mm) 692 692 692 692 692 692 692 692 692 Output power(W) 9.3 9.3 9.3 9.3 9.3 9.3 9.3 9.3 9.3 Pulse energy (μJ) 235 235 235 235 235 235 235 235 235 Energy density (mJ / cm2) 11968 11968 11968 11968 11968 11968 11968 11968 11968 Spot diameter(um) 50 50 50 50 50 50 50 50 50 Frequency (kHz) 40 40 40 40 40 40 40 40 40 Scanning pitch (μm) 100 150 200 250 300 350 400 450 500 Scanning speed (m / s) 4 6 8 10 12 14 16 18 20 Time required to scan a 210mm square (s) 110.8 49.2 27.7 17.7 12.3 9.0 6.9 5.5 4.4 determination No Can good good excellent excellent excellent excellent excellent
[0300] [Table 4]
[0301]
[0302] ※The values of component amounts are expressed in parts by mass.
[0303] The results of the Examples in Tables 1 and 2 and the Comparative Examples in Table 4 show that the resin composition of the present invention is a composition having excellent compatibility, suitability for a spin coating process, and heat resistance.
[0304] When (A-1) was not used and all monomers were (A-2), (B) was precipitated and there was no compatibility (Comparative Examples 1 and 2).
[0305] When (A-2) was not used and all monomers were (A-1), the required heat resistance (2% heating mass loss temperature, elastic modulus) was not obtained (Comparative Examples 3 and 4).
[0306] If (B) is not used, the viscosity does not reach the required minimum value (Comparative Example 5).
[0307] In addition, as can be seen from the results in Tables 1 and 2, the composition of the present invention is excellent in UV laser peelability.
[0308] The resin composition of the present invention can ensure the compatibility of materials and the minimum viscosity required during spin coating, and has excellent adhesion, heat resistance and peeling properties under room temperature and high temperature conditions.
[0309] The resin composition involved in this embodiment has suitability for UV laser stripping process and suitability for mechanical stripping process. Stripping can be performed in the following manner: a thin and sharp metal blade for generating cracks is inserted into the substrate interface at the end of the silicon wafer / glass support laminate produced by the method described in the above embodiment, and then the glass support is fixed horizontally with the glass support as the upper side in advance. After the blade is inserted, an upward stress is applied to the upper support to develop the above cracks and peel the wafer and support.
[0310] In addition, as a method for evaluating the energy required for peeling, a method such as the Maszara test is used, in which a thin and sharp blade is inserted a certain distance in the same manner as above, and the distance of crack development at this time is measured. In this test, the sample obtained by bonding using the liquid resin of the composition of Example 1 also showed a sufficiently low value.
[0311] The resin composition involved in this embodiment has suitability for UV laser stripping process. For the silicon wafer / glass support body laminated body produced by the method described in the above embodiment, the silicon wafer is fixed to the fixing device on the lower side, and the UV laser QLA-355 manufactured by Quark Technology Co., Ltd. is irradiated from the glass support body side under the conditions of output power 9.3W, frequency 40kHz, scanning interval 200μm, and beam diameter 50μm. The peeling force is measured by the same procedure as the above (3) mechanical stripping process suitability evaluation. As a result, the peeling force is reduced from 3N before UV irradiation to 0N.
[0312] Industrial Applicability
[0313] The composition provided by the present invention is excellent in heat resistance, low outgassing and peeling properties.
[0314] The composition of the present invention can easily exhibit strong adhesion in the manufacture of various electronic components, optical components, and optical devices by irradiating ultraviolet rays or visible light, so it is excellent in operability and productivity. In addition, the cured body of the composition of the present invention has very little outgassing even at a high temperature of 250°C. The composition of the present invention is easy to peel off after processing. Therefore, various electronic components, optical components, and optical devices bonded using the composition of the present invention can be applied even when subjected to vapor deposition treatment at a high temperature of more than 200°C or sintering coating at a high temperature.
[0315] In addition to electronic components such as IC, resistors, inductors, optical components such as image sensors are also gradually applied to the surface packaging of circuit substrates. In this case, high temperature reflow soldering is experienced. In recent years, especially with the lead-free of solder, the temperature conditions of reflow soldering have gradually become harsh. In such a production process, in order to improve the quality of optical components and optical equipment, or in order to improve productivity and production yield, the use position of the composition of the present invention requires that it can fully withstand high temperature heating treatment. Optical components and optical equipment manufactured using the composition of the present invention are very useful in industry because they can fully withstand the above-mentioned high temperature heating treatment.
Claims
1. Temporary fixing adhesives that meet all of the following conditions: The light transmittance of the cured body of the temporary fixing composition having a thickness of 50 μm is 70% or more in the wavelength region of 395 nm or more of the wavelength of the light source used for curing; The light transmittance of the cured body of the temporary fixing composition having a thickness of 50 μm is 20% or more in the wavelength region of 385 nm or more and less than 395 nm of the wavelength of the light source used for curing; The light transmittance of the cured product of the temporary fixing composition having a thickness of 50 μm is 1% or less at the wavelength (355 nm) of UV laser used for UV laser lift-off.
2. The temporary fixing adhesive according to claim 1, comprising (C) a photoradical polymerization initiator and (D) a UV absorber, The (C) photoradical polymerization initiator comprises at least one selected from the group consisting of acylphosphine oxide compounds, titanocene compounds, α-aminoalkylphenone compounds, and oxime ester compounds. The (D) UV absorber includes at least one selected from the group consisting of benzotriazole compounds and hydroxyphenyltriazine compounds.
3. The temporary fixing adhesive according to claim 2, wherein: (C) The photoradical polymerization initiator comprises a compound satisfying any one or more of the following conditions: When dissolved at a concentration of 0.1% by mass in a solvent having no maximum absorption in the wavelength region of 300 nm to 500 nm, the absorbance at a wavelength of 365 nm is 0.5 or more; The absorbance at a wavelength of 385 nm is greater than 0.5; and The absorbance at a wavelength of 405 nm is greater than 0.
5. 4 . The temporary fixing adhesive according to claim 1 , which has a viscosity of 100 mPa·s or more and 10000 mPa·s or less at 23° C. and atmospheric pressure.
5. The temporary fixing adhesive according to any one of claims 1 to 4, further comprising at least one of (A-1) a monofunctional (meth)acrylate having an alkyl group with 18 or more carbon atoms in its side chain and a homopolymer having a Tg of -100°C to 60°C, and (A-2) a polyfunctional (meth)acrylate. 6 . A cured product of the temporary fixing adhesive according to claim 1 .
7. A method for manufacturing a semiconductor wafer, characterized in that: include: A step of applying a temporary fixing adhesive to a semiconductor wafer substrate and / or a supporting member to bond the semiconductor wafer substrate to the supporting member; A step of curing the temporary fixing adhesive by irradiating light with a wavelength of 350nm to 700nm to obtain an adhesive body; and The step of irradiating the adhesive with a laser having a wavelength less than 385 nm to peel off the semiconductor wafer substrate, Wherein, the temporary fixing adhesive meets all of the following conditions: The light transmittance of the cured body of the temporary fixing composition having a thickness of 50 μm is 70% or more in the wavelength region of 395 nm or more of the wavelength of the light source used for curing; The light transmittance of the cured body of the temporary fixing composition having a thickness of 50 μm is 20% or more in the wavelength region of 385 nm or more and less than 395 nm of the wavelength of the light source used for curing; The light transmittance of the cured product of the temporary fixing composition having a thickness of 50 μm is 1% or less at the wavelength (355 nm) of UV laser used for UV laser lift-off.
8. The manufacturing method according to claim 7, wherein: The cured temporary fixing adhesive forms a single layer in the bonded body.
9. The manufacturing method according to claim 7 or 8, wherein: The temporary fixing adhesive has a viscosity of 100 mPa·s or more and 10000 mPa·s or less at 23° C. and atmospheric pressure.
10. The production method according to any one of claims 7 to 9, wherein The temporary fixing adhesive comprises at least one of (A-1) a monofunctional (meth)acrylate having an alkyl group having 18 or more carbon atoms in its side chain and a homopolymer having a Tg of -100°C to 60°C, and (A-2) a polyfunctional (meth)acrylate.
11. The production method according to any one of claims 7 to 10, wherein The temporary fixing adhesive contains (C) a photoradical polymerization initiator and (D) a UV absorber. The (C) photoradical polymerization initiator comprises at least one selected from the group consisting of acylphosphine oxide compounds, titanocene compounds, α-aminoalkylphenone compounds, and oxime ester compounds. The (D) UV absorber includes at least one selected from the group consisting of benzotriazole compounds and hydroxyphenyltriazine compounds.
12. A semiconductor wafer obtained by the production method according to any one of claims 7 to 11.