Nb and Y composite low-temperature tough soft magnetic stainless steel and soft magnetic stainless steel profile and product prepared from Nb and Y composite low-temperature tough soft magnetic stainless steel

By optimizing chemical composition and preparation process, the problem of insufficient low-temperature impact toughness of soft magnetic stainless steel is solved, and a soft magnetic stainless steel profile with excellent low-temperature toughness and soft magnetic properties is realized, which is suitable for solenoid valve cores in low-temperature media.

CN118895467AActive Publication Date: 2024-11-05UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410930494.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing soft magnetic stainless steel has low low-temperature impact toughness and cannot meet the use needs of solenoid valve cores that are in service in low-temperature media.

Method used

By optimizing the chemical composition design, controlling the content of elements such as Cr, Nb, Y, and annealing during the preparation process, forming soft magnetic stainless steel profiles with excellent low-temperature toughness and soft magnetic properties. The specific steps include providing steel water that meets the element content. Forming, rolling and annealing.

Benefits of technology

The excellent low-temperature toughness and soft magnetic properties of soft magnetic stainless steel profiles are achieved, which are shown as impact work of -40℃ ≥45J, saturated magnetic induction strength ≥1.6T, coercive force ≤130A/m and residual magnetic induction strength ≤0.3T, suitable for low temperatures Solenoid valve core in the medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895467A_ABST
    Figure CN118895467A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of stainless steel. Specifically, the invention relates to soft magnetic stainless steel with excellent low-temperature toughness added with elements Nb and Y, and a soft magnetic stainless steel profile and a product prepared from the soft magnetic stainless steel. According to the soft magnetic stainless steel, a certain amount of Nb element and Y element added into the soft magnetic stainless steel in a composite mode can play a synergistic role, so that the soft magnetic stainless steel can have excellent low-temperature toughness and soft magnetic performance, and the soft magnetic stainless steel can also have good corrosion resistance and low raw material cost. The soft magnetic stainless steel profile can be effectively applied to electromagnetic valves serving in low-temperature media and related products, and has good popularization prospects and application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of stainless steel, and in particular to soft magnetic stainless steel and soft magnetic stainless steel profiles and products prepared therefrom. Background Art

[0002] With the development of intelligent products, devices that use electromagnetic force as switch elements and control units have become indispensable in various fields, such as brakes, relays, solenoid valves, etc. These devices have an increasingly urgent demand for high-quality soft magnetic stainless steel for solenoid valve cores that have high magnetic induction, low coercive force, and mechanical properties such as corrosion resistance, wear resistance, and impact resistance.

[0003] However, the quality of soft magnetic stainless steel currently available on the market cannot meet some specific industrial needs. For example, they generally have poor low-temperature toughness, which may result in a short life of products made from them, especially gas or liquid leakage in solenoid valves made from them.

[0004] Regarding the composition design of soft magnetic stainless steel, the Chinese patent application CN114836684A, entitled "Low chromium soft magnetic stainless steel and its preparation method and application", discloses a low chromium soft magnetic stainless steel, the alloy element composition of which by weight percentage is: C: ≤0.015%, Si: 0.4%-1.0%, Mn: 0.15%-0.30%, P: ≤0.030%, S: ≤0.005%, Cr: 11.0%-13.5%, Ni: ≤0.20%, Ti: 0.12%-0.30%, N: ≤0.020%, and the remainder is Fe and unavoidable impurities. This patent application obtains stainless steel with high saturation magnetic induction intensity by designing the element content and optimizing the preparation process. However, the soft magnetic stainless steel of this patent application has high inclusion and precipitation content, and the soft magnetic properties and low temperature toughness need to be further improved.

[0005] Chinese patent application CN114606440A, entitled "A high-performance soft magnetic stainless steel and its preparation method", discloses a soft magnetic stainless steel, the alloy element composition by weight percentage is: C: ≤0.02%, Si: 1.5-2.5%, Mn: ≤0.8%, P: ≤0.03%, S: 0.15-0.35%, Ni: ≤0.4%, Cr: 13.0-15.0%, N: ≤0.02%, Mo: 0.2-0.8%, Nb: 0.15-0.30%, Re: 0.005-0.012%, and the rest is iron and unavoidable impurities. This patent application obtains stainless steel with excellent soft magnetic properties and cutting performance by adding Nb elements and optimizing metallurgical processes. However, the soft magnetic stainless steel in this patent application has poor plastic toughness, especially low-temperature toughness, which limits its industrial application scenarios.

[0006] Chinese patent application CN114871270A, entitled "A high-speed wire rolling method for soft magnetic stainless steel wire rod", discloses a high-speed wire rolling method for soft magnetic stainless steel wire rod. The patent application improves the rolling yield of soft magnetic stainless steel wire rod by subjecting the billet to multi-stage heating and controlling the temperature nodes during the rolling process of the method. However, the method of the patent application does not include an annealing process, resulting in low low-temperature impact toughness of the final product.

[0007] In summary, the low-temperature impact toughness of the soft magnetic stainless steel in the prior art is still relatively low. Therefore, it is necessary to further research and develop soft magnetic stainless steel profiles with excellent low-temperature toughness and electromagnetic properties to meet the use requirements of electromagnetic valve cores that can serve in low-temperature media. Summary of the invention

[0008] Purpose of the Invention

[0009] In view of the problems existing in the prior art described in the above background technology section, an object of the present invention is to provide a soft magnetic stainless steel having excellent low temperature toughness and electromagnetic properties and a soft magnetic stainless steel profile and product prepared therefrom.

[0010] Technical Solution

[0011] In order to achieve the above-mentioned purpose of the present invention, the present invention provides the following technical solutions:

[0012] Solution 1: A soft magnetic stainless steel, the soft magnetic stainless steel consisting of the following elements:

[0013] Based on the total weight of the soft magnetic stainless steel:

[0014] about 15.0 to about 17.0 wt. %, preferably about 15.5 to about 16.5 wt. % Cr;

[0015] about 0.03 to about 0.30 wt. %, preferably about 0.05 to about 0.20 wt. % Nb;

[0016] about 0.01 to about 0.10 wt %, preferably about 0.015 to about 0.05 wt % of Y;

[0017] and the balance Fe; and

[0018] Unavoidable impurities.

[0019] Solution 2: The soft magnetic stainless steel according to Solution 1, wherein the elements as the unavoidable impurities are based on the total weight of the soft magnetic stainless steel:

[0020] The C content is controlled to be below about 0.015 wt %, preferably below about 0.010 wt %; and / or

[0021] The N content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %; and / or

[0022] The content of O is controlled to be below about 0.002 wt %, preferably below about 0.0015 wt %; and / or

[0023] The S content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %; and / or

[0024] The P content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %.

[0025] Solution 3: A soft magnetic stainless steel profile, preferably a wire, prepared from the soft magnetic stainless steel described in Solution 1 or 2 above.

[0026] Solution 4: The soft magnetic stainless steel profile according to Solution 3 above, wherein the soft magnetic stainless steel profile has any one or more of the following properties:

[0027] The -40°C impact energy KV2 of the soft magnetic stainless steel profile is about ≥45J;

[0028] The saturation magnetic induction intensity B of the soft magnetic stainless steel profile s is about ≥1.6T;

[0029] The coercive force H of the soft magnetic stainless steel profile c About ≤130A / m;

[0030] The residual magnetic induction intensity B of the soft magnetic stainless steel profile r is about ≤0.3T;

[0031] The microstructure of the soft magnetic stainless steel profile contains about 99.99% or more ferrite, preferably pure ferrite, and

[0032] The effective grain size of the microstructure of the soft magnetic stainless steel profile is about ≤30 μm.

[0033] Scheme 5: A method for preparing the soft magnetic stainless steel profile according to Scheme 3 or 4 above, wherein the method comprises the following steps:

[0034] Step 1: providing molten steel, the molten steel containing the element content of the soft magnetic stainless steel as defined in the above scheme 1 or 2;

[0035] Step 2: forming the molten steel obtained in step 1 into a casting billet;

[0036] Step 3: rolling the cast slab obtained in step 2 into a profile, and

[0037] Step 4: The rolled profile obtained in step 3 is annealed to form the soft magnetic stainless steel profile.

[0038] Scheme 6: According to the preparation method described in the above-mentioned Scheme 5, the rolling process in the step 3 includes: first, maintaining the cast billet at a temperature of about 1060 to about 1140°C for about 0.5 to about 1 hour; then rolling the cast billet, wherein the starting rolling temperature is controlled in the range of about 1020 to about 1080°C, and the final rolling temperature is controlled in the range of about 720 to about 780°C; and finally cooling the rolled profile to room temperature at a cooling rate of not less than about 8°C / s.

[0039] Scheme 7: The preparation method according to Scheme 5 or 6 above, wherein the annealing process in step 4 comprises: first maintaining the rolled profile at a temperature of about 900 to about 950°C for about 4 to about 6 minutes, and then cooling the profile to room temperature at a cooling rate of not less than about 20°C / s.

[0040] Scheme 8: A product made from the soft magnetic stainless steel profile according to Scheme 3 or 4 above or the soft magnetic stainless steel profile prepared by the preparation method according to any one of Schemes 5 to 7 above.

[0041] Option 9: The product according to Option 8 above, which is selected from a brake, a relay and a solenoid valve.

[0042] Technical Effects

[0043] Compared with the prior art, the soft magnetic stainless steel and the profiles prepared therefrom of the present invention achieve the following technical effects:

[0044] The soft magnetic stainless steel profile of the present invention has excellent low temperature toughness and also has excellent soft magnetic properties, such as higher saturation magnetic flux density, lower coercive force and lower residual magnetic flux density.

[0045] Specifically, the soft magnetic stainless steel of the present invention adopts a reasonable chemical composition design, optimizes and excludes various alloying elements in other soft magnetic stainless steels, retains the Cr element, strictly controls the content of impurity elements such as C, N, O, S, and P, so as to fully ensure that the steel has excellent soft magnetic properties, and utilizes Nb and Y elements to optimize microalloy precipitation, thereby obtaining a suitable fine grain size, so that the soft magnetic stainless steel of the present invention has excellent low-temperature toughness. The excellent low-temperature impact toughness and soft magnetic properties of the soft magnetic stainless steel of the present invention are specifically embodied in: -40℃ impact energy KV2≥45J, saturation magnetic induction intensity B s ≥1.6T, coercive force Hc ≤130A / m, residual magnetic induction intensity B r ≤0.3T.

[0046] The soft magnetic stainless steel profile of the present invention can be effectively applied to electromagnetic valve cores and related products serving in low-temperature media, and has very good promotion prospects and application value.

[0047] In addition, the soft magnetic stainless steel of the present invention does not use expensive Ni and Mo elements, and the alloy elements are only Cr elements not exceeding about 17% and trace amounts of Nb and Y elements, and the preparation process is simple and conventional, with lower alloy cost and preparation cost.

[0048] In the preparation method of the present invention, Nb and Y elements are added and the annealing process is optimized, so that the soft magnetic stainless steel of the present invention has a uniform structure, thus having good plasticity, which is beneficial to the downstream drawing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0050] Figure 1 This is a metallographic structure photograph of the soft magnetic stainless steel profile of Example 1 of the present invention.

[0051] Figure 2 This is a metallographic structure photograph of the soft magnetic stainless steel profile of Example 2 of the present invention.

[0052] Figure 3 This is a metallographic structure photograph of the soft magnetic stainless steel profile of Example 3 of the present invention. DETAILED DESCRIPTION

[0053] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without paying creative work belong to the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on normal conditions.

[0054] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. The term "about" used in the present invention means that the modified numeral can fluctuate within the range of ±20%, ±15%, ±10%, ±5% or ±2% of the numeral. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in the present invention.

[0055] In a first aspect of the present invention, the present invention provides a soft magnetic stainless steel. According to the first aspect of the present invention, the soft magnetic stainless steel is composed of the following elements:

[0056] Based on the total weight of the soft magnetic stainless steel:

[0057] about 15.0 to about 17.0 wt %, preferably about 15.5 to about 16.5 wt % Cr (chromium);

[0058] About 0.03 to about 0.30 wt. %, preferably about 0.05 to about 0.20 wt. % Nb (niobium);

[0059] About 0.010 to about 0.100 wt %, preferably about 0.015 to about 0.050 wt % Y (yttrium);

[0060] and the balance Fe (iron); and

[0061] Unavoidable impurities.

[0062] In the soft magnetic stainless steel of the first aspect of the present invention, the Cr element is an element that can promote the formation of a ferrite structure and is also the main element that makes stainless steel less prone to rust. In the soft magnetic stainless steel of the present invention, Cr is one of the basic elements. As the Cr content in the stainless steel increases, the pitting potential of the ferritic stainless steel increases and the corrosion resistance also improves. However, as the Cr content increases, the saturation magnetization of the material decreases. Therefore, in the soft magnetic stainless steel of the present invention, the content of the element Cr is controlled within the range of about 15 to about 17 weight %, for example, it can be set to about 15.5 weight %, about 16 weight % or about 16.5 weight %.

[0063] In the soft magnetic stainless steel of the first aspect of the present invention, the Nb element is a strong ferrite forming element, and is also a strong carbide and nitride forming element. The Nb element can form carbides and nitrides with the residual C and N in the stainless steel, inhibiting the precipitation of carbides and nitrides formed by Cr in the stainless steel, and enhancing the intergranular corrosion resistance of the stainless steel. The precipitates of Nb can also pin the grain boundaries, inhibit the growth of grains, and play a role in refining grains and improving impact toughness. However, too much Nb element leads to too fine grains and too high coercivity of the soft magnetic stainless steel. Therefore, in the soft magnetic stainless steel of the present invention, the content of the element Nb should be controlled in the range of about 0.03 to about 0.3 weight %, for example, it can be set to about 0.05 weight %, about 0.10 weight %, about 0.15 weight %, about 0.20 weight % or about 0.25 weight %.

[0064] In the soft magnetic stainless steel of the first aspect of the present invention, the Y element interacts with the possible low melting point harmful impurity elements, inhibits their segregation at the grain boundary, and plays a role in purifying and strengthening the grain boundary. In addition, the Y element can effectively improve the morphology and distribution of inclusions in the steel, reduce the number of irregular large-sized inclusions in the steel, and thus improve the plasticity of the steel. However, the Y element content should not be too high. Excessive Y element will make the inclusions coarse and increase the brittle tendency, so it needs to be controlled within a certain range. Therefore, in the soft magnetic stainless steel of the present invention, the content of the element Y should be controlled within the range of about 0.01 to about 0.1 weight %, for example, it can be set to about 0.015 weight %, about 0.02 weight %, about 0.03 weight %, about 0.04 weight %, about 0.05 weight %, about 0.06 weight %, about 0.07 weight %, about 0.08 weight % or about 0.09 weight %.

[0065] Furthermore, in the soft magnetic stainless steel of the first aspect of the present invention, the composite addition of Nb element and Y element will produce a synergistic effect, optimize the precipitation form of NbC in the stainless steel, increase the number of nucleations of M7C3 type carbides, promote the refinement and dispersion precipitation of Nb precipitation phase in ferrite, enhance the grain refinement and precipitation strengthening effects, thereby synergistically improving the low-temperature impact toughness of the soft magnetic stainless steel.

[0066] In some preferred embodiments of the soft magnetic stainless steel of the first aspect of the present invention, the contents of the elements C (carbon), N (nitrogen), O (oxygen), S (sulfur), and P (phosphorus) as inevitable impurities are preferably strictly controlled.

[0067] The element C is preferably completely absent in the soft magnetic stainless steel of the present invention as an inevitable impurity. The element C is a strong austenite-forming element, which is not conducive to the formation of ferrite. The element C has a strong affinity with the element Cr, and will form cementite-type carbides, which have an adverse effect on the magnetic properties of the stainless steel, and may reduce the magnetic induction intensity and magnetic permeability, and increase the magnetic loss and coercive force. Therefore, in the soft magnetic stainless steel of the first aspect of the present invention, the content of C is usually controlled to be below about 0.015 weight %, preferably below about 0.010 weight %, and more preferably below about 0.005 weight %.

[0068] As an inevitable impurity, the element N is preferably completely absent in the soft magnetic stainless steel of the present invention. The N element is roughly the same as the C element in many properties. The N element is also a strong austenite-forming element, which has an adverse effect on the magnetic properties of ferritic stainless steel. In addition, N has a low solubility and is easy to form nitrides with other alloying elements and then precipitate, causing local distortion inside the stainless steel, forming a stress field, hindering the movement of domain walls, increasing magnetic losses, and weakening magnetic induction intensity and magnetic permeability. Therefore, in the soft magnetic stainless steel of the first aspect of the present invention, the content of the N element is usually controlled to be below about 0.005% by weight, preferably below about 0.003% by weight.

[0069] The element O is preferably completely absent in the soft magnetic stainless steel of the present invention as an inevitable impurity. The element O is generally considered to be a harmful residual element in the soft magnetic stainless steel of the present invention. It may precipitate from the molten steel in the form of oxide inclusions with other alloy elements during the smelting process, greatly weakening almost all properties of the soft magnetic stainless steel of the present invention, including mechanical properties, corrosion resistance, low temperature toughness and soft magnetic properties. Therefore, the content of O in the soft magnetic stainless steel of the first aspect of the present invention is usually controlled to be below about 0.002 weight %, preferably below about 0.0015 weight %, and more preferably below about 0.001 weight %.

[0070] The element S is preferably completely absent in the soft magnetic stainless steel of the present invention as an inevitable impurity. Although the presence of a small amount of S in stainless steel can improve the cutting performance of the stainless steel, in the soft magnetic stainless steel of the present invention, S element causes the precipitation of metal sulfides, which greatly deteriorate the impact toughness and soft magnetic properties of the soft magnetic stainless steel. Therefore, the content of S in the soft magnetic stainless steel of the first aspect of the present invention is usually controlled to be less than about 0.005% by weight, preferably less than about 0.003% by weight.

[0071] The element P is preferably completely absent in the soft magnetic stainless steel of the present invention as an inevitable impurity. The element P is also a harmful residual element in the soft magnetic stainless steel of the present invention, and the element P will have an adverse effect on the corrosion resistance and impact toughness of the soft magnetic stainless steel. Therefore, the content of P in the soft magnetic stainless steel of the first aspect of the present invention is usually controlled to be below about 0.005 weight %, preferably below about 0.003 weight %.

[0072] In a second aspect of the present invention, the present invention provides a soft magnetic stainless steel profile prepared from the soft magnetic stainless steel according to the first aspect of the present invention.

[0073] In some preferred embodiments of the soft magnetic stainless steel profile of the second aspect of the present invention, the shape of the profile is not particularly limited. However, in some preferred embodiments, it can be selected from various forms such as rods, wires, coils, plates and / or blocks.

[0074] In some other preferred embodiments of the soft magnetic stainless steel profile of the second aspect of the present invention, the soft magnetic stainless steel profile of the present invention may have any one or more of the following properties, more preferably all of them:

[0075] The -40°C impact energy KV2 of the soft magnetic stainless steel profile is about ≥45J; and / or

[0076] The saturation magnetic induction intensity B of the soft magnetic stainless steel profile s is about ≥ 1.6 T; and / or

[0077] The coercive force H of the soft magnetic stainless steel profile c is about ≤ 130 A / m; and / or

[0078] The residual magnetic induction intensity B of the soft magnetic stainless steel profile r is about ≤ 0.3 T; and / or

[0079] The microstructure of the soft magnetic stainless steel profile contains more than 99.99% ferrite, preferably pure ferrite, and / or

[0080] The effective grain size of the microstructure of the soft magnetic stainless steel profile is about ≤30 μm.

[0081] In a third aspect of the present invention, the present invention provides a method for preparing the soft magnetic stainless steel profile according to the second aspect of the present invention.

[0082] The preparation method according to the third aspect of the present invention comprises steps 1 to 4.

[0083] The step 1 comprises providing molten steel, wherein the molten steel contains the following elements in accordance with the content of the soft magnetic stainless steel defined in the first aspect of the present invention:

[0084] Based on the total weight of the soft magnetic stainless steel:

[0085] about 15.0 to about 17.0 wt. %, preferably about 15.5 to about 16.5 wt. % Cr;

[0086] about 0.03 to about 0.30 wt. %, preferably about 0.05 to about 0.20 wt. % Nb;

[0087] about 0.010 to about 0.100 wt %, preferably about 0.015 to about 0.050 wt % of Y;

[0088] and the balance Fe; and

[0089] Unavoidable impurities.

[0090] In some preferred embodiments of the method for preparing a soft magnetic stainless steel profile according to the third aspect of the present invention, the contents of the elements C, N, O, S and P as inevitable impurities in the molten steel need to be strictly controlled. For example, based on the total weight of the molten steel, the elements as the inevitable impurities are:

[0091] The C content is controlled to be below about 0.015 wt %, preferably below about 0.010 wt %; and / or

[0092] The N content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %; and / or

[0093] The content of O is controlled to be below about 0.002 wt %, preferably below about 0.0015 wt %; and / or

[0094] The S content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %; and / or

[0095] The P content is controlled to be below about 0.005 wt %, preferably below about 0.003 wt %.

[0096] In step 1 of the method for preparing a soft magnetic stainless steel profile in the third aspect of the present invention, the molten steel can be obtained by any method known in the art. For example, in a preferred embodiment of the present invention, the molten steel can be obtained by the process of (1) converter smelting → (2) LF (Ladle Furnace) furnace refining → (3) VD (Vacuum Degassing) and / or RH (Ruhrstahl-Heraeus) furnace vacuum degassing commonly used in the art. The molten steel thus obtained can meet the required range of element content of the stainless steel in the first aspect of the present invention.

[0097] The step 2 comprises forming the molten steel obtained from the step 1 into a casting ingot.

[0098] In step 2 of the method for preparing a soft magnetic stainless steel profile in the third aspect of the present invention, the molding can be performed by any method known in the art. For example, the molding in step 2 can be performed by die casting or continuous casting, preferably continuous casting. Preferably, the casting temperature during the continuous casting process can be about 1515°C to about 1535°C.

[0099] The shape of the resulting ingot is not particularly limited and can be determined according to the shape of the final product. For example, according to the requirements of the final product specifications, the shape of the continuous casting ingot is preferably a ingot with a cross-section of about 240×240 mm or about 180×180 mm, and the surface of the ingot is required to be flat and free of defects visible to the naked eye.

[0100] In step 2 of the method for preparing a soft magnetic stainless steel profile in the third aspect of the present invention, the temperature of the ingot is preferably maintained at above about 1200° C., more preferably about 1200 to about 1250° C. Such a temperature can ensure that the subsequent rolling process can proceed smoothly and ensure that the final profile has ideal properties.

[0101] The step 3 comprises rolling the cast slab obtained in the step 2 into a profile.

[0102] The rolling process can be carried out by a rolling mill using rollers. The shape of the profile obtained by rolling is not particularly limited, and can be determined according to the shape of the final product, for example, it can be in the form of a plate, block, wire, wire rod and / or bar. In a preferred embodiment of the present invention, the shape of the profile is particularly preferably a wire or wire rod.

[0103] In a preferred embodiment of step 3 of the method for preparing a soft magnetic stainless steel profile described in the third aspect of the present invention, the cast billet is first maintained at a temperature of about 1060 to about 1140°C (for example, about 1070°C, about 1080°C, about 1090°C, about 1100°C, about 1110°C, about 1120°C or about 1130°C) for about 0.5 to about 1 hour (for example, about 0.6 hour, about 0.7 hour, about 0.8 hour or about 0.9 hour); and then the cast billet is rolled, wherein the start rolling temperature is controlled in the range of about 1020 to about 1080°C (for example, about 1025°C, about 1030°C, about 1040°C, about 1050°C, about 1060°C or about 1070°C), and the final rolling temperature is controlled in the range of about 720 to about 780°C (for example, about 740°C, about 760°C or about 770°C).

[0104] Here, since the phase diagram of the steel with the soft magnetic stainless steel composition of the present invention is single-phase ferrite without austenite phase transformation, the settings of the above parameters are set according to the parameters in the prior art on the one hand, and determined by the inventor of the present invention through experiments on the other hand. For example, on the one hand, the insulation temperature of the ingot should preferably not be too high or too low, for example, it should not be higher than about 1140°C, otherwise the original grains in the ingot may be too coarse, and it should not be lower than about 1060°C, otherwise the deformation resistance of the ingot may be too large and rolling cracking may occur; on the other hand, the insulation time of the ingot should preferably not be too long or too short, for example, it should not be longer than about 1 hour, otherwise the original grains in the ingot may be too coarse, and it should not be shorter than about 0.5 hours, otherwise the temperature difference inside and outside the ingot may cause rolling cracking; and On the one hand, the starting rolling temperature should preferably not be too high or too low, for example, it should not be higher than about 1080°C, otherwise the original grains of the ingot during the rolling process may be too coarse and even cause steel piling accidents, and it should not be lower than about 1020°C, otherwise the deformation resistance of the ingot may be too large and rolling cracks may occur; finally, the final rolling temperature should preferably not be too high or too low, for example, it should not be higher than about 780°C, otherwise the grains in the rolled profile may be too large, and it should not be lower than about 720°C, otherwise rolling hot cracks may occur in the profile.

[0105] In addition, the profile obtained after the rolling can be directly subjected to annealing and heating operations without cooling. However, the phase diagram of the steel type having the soft magnetic stainless steel composition of the present invention is full ferrite, without austenite phase transformation, and the ferrite grains have a high tendency to grow at high temperatures. Therefore, in order to avoid coarse grains, it is generally preferred to cool the profile first and then perform recrystallization annealing. For example, in a preferred embodiment of the present invention, in order to cool the profile to room temperature as quickly as possible, it can be air-cooled to room temperature at a cooling rate of not less than 8°C / s, which can also facilitate subsequent operations such as the transfer of the profile. The cooling rate of the profile described here should not be too slow, for example, it should not be less than about 8°C / s, otherwise it may cause the growth of grains and precipitation in the profile.

[0106] The step 4 includes annealing the rolled profile obtained in the step 3 to form the soft magnetic stainless steel profile.

[0107] The specific parameters of the annealing treatment are not particularly limited, as long as the annealing treatment can make the soft magnetic stainless steel profile of the present invention have the advantageous properties described herein. However, in a preferred embodiment, in step 4 of the preparation method described in the third aspect of the present invention, the annealing treatment includes first keeping the rolled profile at a temperature of about 900 to about 950°C (for example, about 910°C, about 920°C, about 930°C or about 940°C) for about 4 to about 6 minutes (for example, about 5 minutes), and then cooling the profile to room temperature as quickly as possible. Here, after the recrystallization annealing, it is preferably necessary to cool the profile quickly to avoid the growth of recrystallized grains, for example, it can be cooled to room temperature at a cooling rate of not less than 20°C / s, for example, it can be cooled to room temperature by spraying water.

[0108] Here, on the one hand, the temperature of the annealing treatment is preferably not too high or too low, for example, it should not be higher than about 950°C, otherwise the recrystallized grains in the profile may be too coarse, and it should not be lower than about 900°C, otherwise the stress relief and recrystallization of the profile may be incomplete; on the other hand, the annealing time is preferably not too long or too short, for example, it should not be longer than about 6 minutes, otherwise the recrystallized grains in the profile may be too coarse, and it should not be shorter than about 4 minutes, otherwise the stress relief and recrystallization of the profile may be incomplete.

[0109] Preferably, after the annealing treatment as described above, the obtained soft magnetic stainless steel profile preferably has one or more of the following advantageous properties:

[0110] The -40°C impact energy KV2 of the soft magnetic stainless steel profile is about ≥45J; and / or

[0111] The saturation magnetic induction intensity B of the soft magnetic stainless steel profile s is about ≥ 1.6 T; and / or

[0112] The coercive force H of the soft magnetic stainless steel profile c is about ≤ 130 A / m; and / or

[0113] The residual magnetic induction intensity B of the soft magnetic stainless steel profile r is about ≤ 0.3 T; and / or

[0114] The microstructure of the soft magnetic stainless steel profile contains more than 99.99% ferrite, preferably pure ferrite, and / or

[0115] The effective grain size of the microstructure of the soft magnetic stainless steel profile is about ≤30 μm.

[0116] In a fourth aspect of the present invention, the present invention provides a soft magnetic stainless steel product, which is prepared from the soft magnetic stainless steel profile according to the second aspect of the present invention.

[0117] Particularly preferably, the soft magnetic stainless steel product according to the fourth aspect of the present invention is a brake, a relay and a solenoid valve comprising a soft magnetic stainless steel profile.

[0118] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0119] In the context of the present invention, room temperature is considered to be about 15 to about 40°C, more preferably about 25°C.

[0120] Examples 1-3 and Comparative Examples 1-5: General preparation process of soft magnetic stainless steel profiles:

[0121] The process of (1) converter smelting → (2) LF furnace refining → (3) VD and / or RH furnace vacuum degassing as described above and known in the art provides molten steel (as shown in Table 1) that meets the required range of soft magnetic stainless steel element content of Examples 1-3 of the present invention and Comparative Examples 1-5 listed in Table 1 below.

[0122] The obtained molten steel was continuously cast into square ingots with specifications of about 180×180×6000 mm. The holding temperature and time of the ingots are shown in Table 2.

[0123] The insulated ingot is rolled into a profile through at least one pair of rotating rollers of a rolling mill, which is a wire with a cross-sectional diameter ranging from about 10 to about 20 mm, wherein the starting rolling temperature and the final rolling temperature of the rolling process are listed in Table 2.

[0124] The rolled wire rod was air-cooled to room temperature, and the cooling rate was as shown in Table 2.

[0125] The cooled wire rod was subjected to an annealing treatment, which included first maintaining the wire rod at a temperature as shown in Table 2 for several minutes and then cooling to room temperature by spraying water to obtain the soft magnetic stainless steel wire rod of each of the Examples and Comparative Examples.

[0126] Table 1 lists the element content ranges (weight %) of the soft magnetic stainless steel profiles of Examples 1-3 and Comparative Examples 1-5 of the present invention, and the remainder is Fe and other unavoidable impurities. Table 2 lists the specific process parameters used in each step of the method for preparing the soft magnetic stainless steel profiles of Examples 1-3 and Comparative Examples 1-5.

[0127] Samples of the soft magnetic stainless steel profiles of Examples 1-3 of the present invention and Comparative Examples 1-5 were taken and their microstructures were observed. Microstructure photos of the soft magnetic stainless steel wires of Examples 1-3 of the present invention are respectively Figure 1-3 Shown in.

[0128] The impact test of the sample was carried out according to the Chinese national standard GB / T 229-2020 "Metallic Material Charpy Pendulum Impact Test Method". Specifically, the sample was processed into a sample with a V-notch size of about 2.5×10×55 mm, the test temperature was controlled to be about -40°C, and the -40°C impact energy KV2 of the soft magnetic stainless steel of Examples 1-3 and Comparative Examples 1-5 was measured.

[0129] The average grain size of the sample was determined according to the Chinese national standard GB / T 6394-2017 "Method for Determining Average Grain Size of Metals". Specifically, the sample was processed into a sample with a size of about 10×10 mm, and the average grain size of the soft magnetic stainless steel of Examples 1-3 and Comparative Examples 1-5 was measured by the intercept method.

[0130] The soft magnetic properties of the samples were tested according to the Chinese national standard GB / T 13012-2008 "Measurement Method for DC Magnetic Properties of Soft Magnetic Materials". Specifically, the samples were processed into samples with a size of about Φ10×200 mm and a circular cross section, the test temperature was set to room temperature, and the saturation magnetic induction intensity B of the soft magnetic stainless steels of Examples 1-3 and Comparative Examples 1-5 was measured. s , coercive force H c and residual magnetic induction intensity B r .

[0131] Table 3 summarizes the properties of the wires prepared from the soft magnetic stainless steels of Examples 1-3 of the present invention and Comparative Examples 1-5.

[0132] Table 1

[0133]

[0134] Table 2

[0135]

[0136] Table 3

[0137]

[0138] The present invention is attached to the specification Figure 1-3 It can be seen from the metallographic structure pictures of the samples of Examples 1 to 3 of the present invention that the microstructures of the soft magnetic stainless steels of Examples 1 to 3 of the present invention are all ferrite of more than 99.99%, and the structure is uniform, and no micron-level precipitation and inclusions are observed, which indicates that the soft magnetic stainless steels of Examples 1 to 3 of the present invention have excellent plasticity and toughness and excellent soft magnetic properties.

[0139] It can be seen from the various performance data of Examples 1 to 3 of the present invention listed in Table 3 that the soft magnetic stainless steel samples of Examples 1 to 3 of the present invention all achieved an impact energy of ≥45J at -40°C, showing very good low-temperature toughness; the average grain size of the samples was ≤30μm, and the saturation magnetic induction intensity B s ≥1.6T, coercive force H c ≤130A / m, residual magnetic induction intensity B r ≤0.3T, so that the soft magnetic stainless steel samples of Examples 1-3 of the present invention have excellent soft magnetic properties and can be used to prepare various types of mechanical equipment and solenoid valve equipment.

[0140] It can be seen from the various parameters and performance data of Comparative Examples 1-5 listed in Tables 1-3 that the main differences between Comparative Examples 1-3 and Examples 1-3 of the present invention are that Nb and / or Y elements are not added, which affects the morphology and distribution of precipitates in stainless steel, weakens the effect of dispersed distribution of precipitates on pinning grain boundaries, and the increased precipitated inclusions and element segregation at grain boundaries not only lead to an increase in grain size and reduce low-temperature toughness, but also affect the rotation of magnetic domains, deteriorate the coercive force and residual magnetic induction intensity of steel, and the effect of single addition of Nb and Y elements on refining grains and precipitates is not as good as that of composite addition; Compared with Examples 1-3 of the present invention, the main difference between Comparative Examples 4-5 is that Al and / or Si elements commonly used in the field of soft magnetic stainless steel are added, which affects the morphology and recovery effect of recrystallized grains in stainless steel, promotes the aggregation and growth of precipitated inclusions in the grains, and the enlarged precipitated inclusions and non-equiaxed coarse grains not only greatly reduce the low-temperature toughness, but also affect the rotation of magnetic domains, deteriorate the coercive force and residual magnetic induction intensity of steel, and the addition of Al and Si as impurity elements of the soft magnetic stainless steel of the present invention will significantly coarsen the grains, and the size of precipitated inclusions is significantly increased, and the low-temperature impact toughness is significantly deteriorated.

[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A soft magnetic stainless steel, characterized in that: The soft magnetic stainless steel is composed of the following elements: Based on the total weight of the soft magnetic stainless steel: 15.0 to 17.0 wt. %, preferably 15.5 to 16.5 wt. % Cr; 0.03 to 0.30 wt. %, preferably 0.05 to 0.20 wt. % Nb; 0.01 to 0.10 wt %, preferably 0.015 to 0.05 wt % of Y; and the balance Fe; and Unavoidable impurities.

2. The soft magnetic stainless steel according to claim 1, characterized in that: Based on the total weight of the soft magnetic stainless steel, the elements that will serve as the inevitable impurities are: The content of C is controlled to be below 0.015 wt %, preferably below 0.010 wt %; and / or The content of N is controlled to be below 0.005 wt %, preferably below 0.003 wt %; and / or The content of O is controlled to be below 0.002 wt %, preferably below 0.0015 wt %; and / or The content of S is controlled to be below 0.005 wt %, preferably below 0.003 wt %; and / or The P content is controlled to be below 0.005 wt %, preferably below 0.003 wt %.

3. A soft magnetic stainless steel profile prepared from the soft magnetic stainless steel according to claim 1 or 2, preferably a wire.

4. The soft magnetic stainless steel profile according to claim 3, characterized in that: The soft magnetic stainless steel profile has any one or more of the following properties: The -40°C impact energy KV2 of the soft magnetic stainless steel profile is ≥45J; The saturation magnetic induction intensity B of the soft magnetic stainless steel profile s ≥1.6T; The coercive force H of the soft magnetic stainless steel profile c ≤130A / m; The residual magnetic induction intensity B of the soft magnetic stainless steel profile r ≤0.3T; The microstructure of the soft magnetic stainless steel profile contains more than 99.99% ferrite, and The effective grain size of the microstructure of the soft magnetic stainless steel profile is ≤30 μm.

5. A method for preparing the soft magnetic stainless steel profile according to claim 3 or 4, characterized in that: The method comprises the following steps: Step 1: providing molten steel, the molten steel containing the element content of the soft magnetic stainless steel as defined in claim 1 or 2; Step 2: forming the molten steel obtained in step 1 into a casting billet; Step 3: rolling the cast slab obtained in step 2 into a profile, and Step 4: The rolled profile obtained in step 3 is annealed to form the soft magnetic stainless steel profile.

6. The preparation method according to claim 5, characterized in that: The rolling process in step 3 includes: first, maintaining the cast billet at a temperature of 1060 to 1140°C for 0.5 to 1 hour; then rolling the cast billet, wherein the start rolling temperature is controlled within the range of 1020 to 1080°C, and the final rolling temperature is controlled within the range of 720 to 780°C; and finally, cooling the rolled profile to room temperature at a cooling rate of not less than 8°C / s.

7. The preparation method according to claim 5 or 6, characterized in that: The annealing process in step 4 includes: firstly keeping the rolled profile at a temperature of 900 to 950° C. for 4 to 6 minutes, and then cooling the profile to room temperature at a cooling rate of not less than 20° C. / s.

8. A product made from the soft magnetic stainless steel profile according to claim 3 or 4 or the soft magnetic stainless steel profile made by the preparation method according to any one of claims 5 to 7.

9. The article of manufacture of claim 8, selected from the group consisting of a brake, a relay, and a solenoid valve.

Citation Information

Patent Citations

  • Composite magnetic material and preparation method thereof

    CN101853723A

  • Cr-based stainless steel having excellent hydrogen embrittlement resistance

    CN113227414A

  • Soft magnetic stainless steel fine wire and method for producing the same

    JP2013185183A

Cited By

  • Soft magnetic stainless steel and soft magnetic stainless steel profile and product prepared from same

    CN120006168A

  • A soft magnetic stainless steel and a soft magnetic stainless steel profile and article made therefrom

    CN120006168B

  • Soft magnetic stainless steel wire rod suitable for cold heading machining and preparation method of soft magnetic stainless steel wire rod