Porous paper-based facing material and preparation method thereof

By adding hollow silica particles, chitosan and sodium alginate to the porous paper base layer, anti-mold coating and decorative coating, and forming anti-mold and decorative layers through heat treatment, the mechanical strength of porous paper-based finish materials and the mechanical strength of porous paper-based finish materials and the decorative coating are solved. The problem of insufficient anti-mildew and moisture resistance effect has achieved high mechanical strength, good anti-mildew and moisture resistance and fire and heat insulation properties of the material.

CN118895685AActive Publication Date: 2024-11-05ZHEJIANG GRANDRICH PAPER
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411066772.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-05
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing porous paper-based finishing materials have shortcomings in terms of mechanical strength and anti-mildew and moisture effects, and it is difficult to meet the high requirements of decorative materials.

Method used

The method of preparing porous paper base layer, anti-mold coating and decorative coating is adopted, where the porous paper base layer contains hollow silica particles, anti-mold coating contains chitosan, and decorative coating contains sodium alginate. The anti-mold layer and decorative layer are formed by heat treatment. , improve the mechanical strength of the material and anti-mildew resistance.

Benefits of technology

It significantly improves the mechanical strength, anti-mildew and moisture effect of porous paper-based finishing materials, and enhances fire and heat insulation properties, making the material thickness uniform and the paper surface smooth and bright.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a porous paper-based facing material and a preparation method thereof. The preparation method comprises the following steps: S100, respectively preparing a porous paper-based layer, a mildew-proof coating and a decorative coating; s200, applying the mildew-proof coating to the paper base layer, and performing first heat treatment to form a mildew-proof layer on the porous paper base layer; and S300, the decorative coating is applied to the mildew-proof layer, second heat treatment is carried out, so that a decorative layer is formed on the mildew-proof layer, and the porous paper-based facing material is obtained, wherein the porous paper base layer comprises hollow silicon dioxide particles, the mildew-proof coating comprises chitosan, the decorative coating comprises sodium alginate, the temperature of the first heat treatment is 80-90 DEG C, and the temperature of the second heat treatment is 100-110 DEG C. The porous paper-based facing material which is good in mechanical strength and not prone to mildewing can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking, and in particular to a porous paper-based finishing material and a preparation method thereof. Background Art

[0002] In interior decoration projects, paper-based finishing materials are important decoration substrates, which can be used in a variety of scenarios such as wall decoration and furniture veneer. In addition to being used as wallpaper, low-pressure boards and high-pressure boards used in furniture and cabinets, as well as fireproof boards and floors, all require decorative paper to enhance the aesthetic effect of the product.

[0003] Porous paper-based facing materials are usually manufactured through pulping, papermaking, pressing and other processes. The two most important performance indicators of porous paper-based facing materials in the industry are their mechanical strength and mildew and moisture resistance. How to improve the mechanical strength and mildew and moisture resistance of porous paper-based facing materials has always been a technical problem that technicians in this field have been committed to solving. Summary of the invention

[0004] One of the problems solved by the present invention is how to provide a porous paper-based facing material with high mechanical strength and good mildew and moisture resistance effects.

[0005] In order to solve at least one of the above problems, the present invention provides a method for preparing a porous paper-based facing material, the preparation method comprising:

[0006] S100, preparing a porous paper base, an anti-mildew coating, and a decorative coating respectively;

[0007] S200, applying the anti-mildew coating to the paper base layer, and performing a first heat treatment to form an anti-mildew layer on the porous paper base layer;

[0008] S300, applying the decorative coating to the anti-mildew layer, and performing a second heat treatment to form a decorative layer on the anti-mildew layer, and obtaining the porous paper-based facing material;

[0009] Wherein, the porous paper base layer comprises hollow silica particles, the anti-mildew coating comprises chitosan, and the decorative coating comprises sodium alginate.

[0010] In any of the above technical solutions, the porous paper substrate is prepared by the following steps:

[0011] S111, mixing raw materials including a wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous wood pulp and bleached hardwood wood pulp to obtain pulp;

[0012] S112, placing the slurry on a screen to make paper sheets to obtain wet paper sheets;

[0013] S113, pressing, drying and calendering the wet paper sheet to obtain the porous paper base layer.

[0014] In any of the above technical solutions, in S111, by mass ratio, wet strength agent: aluminum sulfate: cationic polyacrylamide: hollow silica particles: bleached coniferous wood pulp: bleached hardwood wood pulp = (3-4): (4-5): (5-6): (12-16): (15-25): 100.

[0015] In any of the above technical solutions, in S111, the beating degree of the slurry is 30°SR to 45°SR, and the wet weight is 2.0g to 3.0g.

[0016] In any of the above technical solutions, the anti-mildew coating is prepared by the following steps:

[0017] S121, mixing raw materials including a surfactant, an emulsifier, a wetting agent, a defoaming agent, oxalic acid, chitosan, potassium sorbate, polyethylene glycol, a water-soluble acrylate and water to obtain a first mixture;

[0018] S122, heating the first mixture to 45° C. to 55° C., and ultrasonically dispersing the mixture for 20 min to 30 min under heat preservation conditions to obtain the anti-mildew coating.

[0019] In any of the above technical schemes, in S121, in terms of mass ratio, surfactant: emulsifier: wetting agent: defoaming agent: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = (0.2-1): (0.5-1.5): (0.5-1.5): (0.5-1.5): (2-4): (6-8): (8-10): (10-12): (20-30): 100.

[0020] In any of the above technical solutions, the decorative coating is prepared by the following steps:

[0021] S131, mixing raw materials including a color regulator, a gloss regulator, sodium alginate, polyacrylamide, a water-soluble acrylate and water to obtain a second mixture;

[0022] S132, ultrasonically dispersing the second mixture for 20 to 30 minutes to obtain the decorative coating.

[0023] In any of the above technical solutions, in S131, the mass ratio of color regulator: glossiness regulator: sodium alginate: polyacrylamide: water-soluble acrylate: water = (2-8): (2-8): (4-6): (16-20): (20-30): 100.

[0024] In any of the above technical solutions, the temperature of the first heat treatment is 80°C to 90°C, and the temperature of the second heat treatment is 100°C to 110°C.

[0025] The present invention also provides a porous paper-based facing material, and the porous paper-based facing material is obtained by using the preparation method described in any of the above technical solutions.

[0026] Beneficial Effects

[0027] The present invention provides a method for preparing a porous paper-based finishing material, which prepares a porous paper base, an anti-mildew coating, and a decorative coating respectively; then the anti-mildew coating is applied to the paper base, and a first heat treatment is performed to form an anti-mildew layer on the porous paper base; finally, the decorative coating is applied to the anti-mildew layer, and a second heat treatment is performed to form a decorative layer on the anti-mildew layer, and the porous paper-based finishing material is obtained. It should be noted that the porous paper base of the present invention includes hollow silica particles, the anti-mildew coating includes chitosan, and the decorative coating includes sodium alginate. The hollow silica particles can improve the mechanical strength and fireproof and heat-insulating properties of the porous paper base, and the electrostatic effect between chitosan and sodium alginate can make the anti-mildew coating and the decorative coating be evenly coated to form a uniform, dense, and uniformly thick anti-mildew layer and decorative layer. As a result, the porous paper-based finishing material obtained by the present invention has good mechanical strength, good anti-mildew and moisture-resistant effects, and also has good fireproof and heat-insulating properties, uniform thickness, and a smooth and bright paper surface. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.

[0029] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0030] Paper-based facing materials are important decoration substrates, which can be used in a variety of scenarios such as wall decoration and furniture veneer. The two most important performance indicators of porous paper-based facing materials in this field are their mechanical strength and mildew and moisture resistance. Take wallpaper as an example. As a decorative material widely used in modern interior decoration, compared with traditional interior decoration materials such as paint and wall paint, wallpaper has the advantages of safety, environmental protection, easy construction, and rich and diverse colors and patterns. However, wallpaper itself is not wear-resistant, easy to scratch and break, easy to get damp and moldy, and easy to breed bacteria. Therefore, the present invention is committed to providing a paper-based facing material with high mechanical strength and good mildew and moisture resistance, which is particularly suitable as wallpaper and other interior decoration materials.

[0031] An embodiment of the present invention provides a method for preparing a porous paper-based facing material, the method comprising:

[0032] S100, preparing a porous paper base, an anti-mildew coating, and a decorative coating respectively;

[0033] S200, applying the anti-mildew coating to the paper base layer, and performing a first heat treatment to form an anti-mildew layer on the porous paper base layer;

[0034] S300, applying the decorative coating to the anti-mildew layer, and performing a second heat treatment to form a decorative layer on the anti-mildew layer, and obtaining the porous paper-based facing material;

[0035] Wherein, the porous paper base layer comprises hollow silica particles, the anti-mildew coating comprises chitosan, and the decorative coating comprises sodium alginate.

[0036] The porous paper base is mainly manufactured by pulping, papermaking, pressing, etc. Those skilled in the art can select and adjust the equipment, raw materials and process parameters used in pulping, papermaking and pressing according to actual needs.

[0037] Among them, pulping is a key process in the papermaking industry. This step separates the fibers from the plant fiber raw materials to obtain paper pulp. The pulping step of the present invention can be carried out by mechanical method, chemical method or chemical mechanical method. The papermaking step uses a bamboo curtain type mesh trough specially used for papermaking to scoop a certain amount of paper pulp, and then swings the mesh trough back and forth or left and right to arrange the pulp fibers in a certain direction to form a paper layer of uniform thickness, i.e., wet paper sheet. The pressing process squeezes the wet paper through a press, and its function is to remove excess water in the paper layer and increase the dryness of the paper. The pressure and speed in the pressing process can be selected and adjusted by those skilled in the art according to actual needs.

[0038] In some embodiments of the present invention, the porous paper substrate is prepared by the following steps:

[0039] S111, mixing raw materials including a wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous wood pulp and bleached hardwood wood pulp to obtain pulp;

[0040] S112, placing the slurry on a screen to make paper sheets to obtain wet paper sheets;

[0041] S113, pressing, drying and calendering the wet paper sheet to obtain the porous paper base layer.

[0042] Among them, the role of the wet strength agent is to significantly improve the wet strength of the paper without changing the dry strength of the paper, so that the paper can still maintain good physical properties in a humid environment. Preferably, the present invention can select PAE wet strength agent. The addition of aluminum sulfate can significantly improve the hardness and strength of the paper, enhance the water resistance of cellulose, and thus improve the quality and durability of the paper. In addition, the use of aluminum sulfate can improve the gloss and smoothness of the paper. Cationic polyacrylamide reduces surface tension through the carboxyl group in its molecular chain, so that the fiber or filler is better dispersed in water, thereby improving the uniformity and quality of the paper. Hollow silica particles are used as fillers, which can improve the mechanical strength and fireproof and heat-insulating effects of paper.

[0043] Preferably, in S111, the mass ratio of wet strength agent: aluminum sulfate: cationic polyacrylamide: hollow silica particles: bleached coniferous wood pulp: bleached hardwood wood pulp is (3-4): (4-5): (5-6): (12-16): (15-25): 100.

[0044] Further preferably, in S111, the mass ratio of wet strength agent: aluminum sulfate: cationic polyacrylamide: hollow silica particles: bleached coniferous wood pulp: bleached hardwood wood pulp is 3:4:6:15:25:100.

[0045] Preferably, in S111, the slurry has a beating degree of 30°SR to 45°SR, and a wet weight of 2.0 g to 3.0 g.

[0046] Further preferably, in S111, the beating degree of the slurry is 35°SR to 40°SR, and the wet weight is 2.4g to 2.8g.

[0047] Preferably, the hollow silica particles are prepared by the following steps:

[0048] S111a, mixing the chitosan in ethanol and water at a mass ratio of chitosan: ethanol: water = (8-12): (25-30): 100, adding acid to adjust the pH value to 3-4, to obtain liquid A;

[0049] S111b, according to the mass ratio of silicon tetrachloride: water = (4-8): 100, according to the amount of water added in S111a, silicon tetrachloride is added dropwise to the A solution and stirred simultaneously, and after the addition is completed, stirring is continued for 1h to 1.5h, alkali is added to adjust the pH value to 11-12, and the solution is allowed to stand for 12h to 15h to obtain a silica sol containing chitosan;

[0050] S111c, immersing the silica sol in ethanol and aging it for 24 to 48 hours, taking it out and sending it into a vacuum reactor filled with ethanol, and treating it at a temperature of 260°C to 270°C and a pressure of 6.7MPa to 7.0MPa for 2 to 3 hours. After the treatment, cool down and release the pressure, separate, wash with water, and dry to obtain the hollow silica particles.

[0051] The purpose of adopting the above steps is to prepare loose and porous, hollow inside, small particle size and uniform particle size distribution of silicon dioxide particles. In general, the above steps adopt the sol-gel method to prepare nano silicon dioxide. The improvement made on the basis of the existing sol-gel method is that chitosan is added to the water-alcohol liquid used to prepare the sol solution. The water-alcohol liquid of nano silicon dioxide prepared by the sol-gel method needs to add an acid catalyst, and chitosan has low solubility in water under acidic conditions and exists almost in a particle state. Subsequently, in order to prepare nano silicon dioxide, it is also necessary to add an alkaline catalyst, and chitosan has increased solubility in water under alkaline conditions, so in the process of adding silicon tetrachloride to the A liquid, stirring and adding alkali to adjust the pH value, a silicon dioxide sol containing chitosan can be formed, and chitosan is evenly distributed in the silicon dioxide sol. Subsequently, ethanol is used as a solvent, and aerogel-shaped silicon dioxide can be prepared by supercritical drying. Moreover, chitosan evenly distributed in the silica sol is thermally decomposed at a temperature of 260°C to 270°C, and the decomposed organic matter and water are extracted by supercritical ethanol, thereby forming loose and porous hollow silica particles with small particle size and uniform particle size distribution. The three-dimensional porous hollow properties of the hollow silica particles can be used to improve the fireproof and heat-insulating properties of the porous paper base.

[0052] In some embodiments of the present invention, the anti-mildew coating is prepared by the following steps:

[0053] S121, mixing raw materials including a surfactant, an emulsifier, a wetting agent, a defoaming agent, oxalic acid, chitosan, potassium sorbate, polyethylene glycol, a water-soluble acrylate and water to obtain a first mixture;

[0054] S122, heating the first mixture to 45° C. to 55° C., and ultrasonically dispersing the mixture for 20 min to 30 min under heat preservation conditions to obtain the anti-mildew coating.

[0055] Preferably, in some embodiments of the present invention, in S121, in terms of mass ratio, surfactant: emulsifier: wetting agent: defoaming agent: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = (0.2-1): (0.5-1.5): (0.5-1.5): (0.5-1.5): (2-4): (6-8): (8-10): (10-12): (20-30): 100.

[0056] Further preferably, in some embodiments of the present invention, in S121, the mass ratio of surfactant: emulsifier: wetting agent: defoaming agent: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = 0.5:0.5:1:1:3:8:10:12:25:100.

[0057] In some embodiments of the present invention, the decorative coating is prepared by the following steps:

[0058] S131, mixing raw materials including a color regulator, a gloss regulator, sodium alginate, polyacrylamide, a water-soluble acrylate and water to obtain a second mixture;

[0059] S132, ultrasonically dispersing the second mixture for 20 to 30 minutes to obtain the decorative coating.

[0060] Preferably, in some embodiments of the present invention, in S131, the mass ratio of color regulator: glossiness regulator: sodium alginate: polyacrylamide: water-soluble acrylate: water = (2-8): (2-8): (4-6): (16-20): (20-30): 100.

[0061] Further preferably, in some embodiments of the present invention, in S131, the mass ratio of color regulator: glossiness regulator: sodium alginate: polyacrylamide: water-soluble acrylate: water is 6:2:4:16:22:100.

[0062] The temperature of the first heat treatment is 80°C to 90°C, and the temperature of the second heat treatment is 100°C to 110°C.

[0063] In the present invention, the types and models of auxiliary materials have no effect on the realization of the purpose of the invention, and those skilled in the art can freely select them. In the present invention, the surfactant is specifically sodium dodecylbenzene sulfonate, the emulsifier is specifically a silicone oil emulsifier, the wetting agent is specifically a dioctyl sodium salt of sulfosuccinate wetting agent, and the defoamer is specifically a polyether defoamer. The glossiness regulator is specifically mica powder.

[0064] The reason for adopting the above steps is that chitosan and potassium sorbate have good antibacterial and mildew-proof effects. Polyacrylamide and / or water-soluble acrylate are used as polymer resin materials, which have good wear resistance and waterproof and moisture-proof properties. In addition, the temperature of the indoor environment where the wallpaper is located will change greatly with the change of seasons, and the air permeability of the resin glue surface layer is extremely poor, which makes it easy for local areas of the wallpaper to bubble, affecting the decorative effect. When bubbles appear on the surface of the wallpaper, it will also affect the waterproof and moisture-proof effect of the wallpaper. In order to reduce the possibility of bubbling, it is key to increase the tightness and uniformity of the combination between the mildew-proof layer and the decorative layer. In order to ensure that the anti-mildew layer and the decorative layer are tightly and evenly combined, the present invention utilizes the electrostatic effect between chitosan and sodium alginate, adds chitosan to the anti-mildew layer, and after a first heat treatment at 80°C to 90°C, the anti-mildew layer is in a semi-dried but not completely dried state, and then sodium alginate is added to the decorative layer applied subsequently. The electrostatic effect of the positive and negative charges between chitosan and sodium alginate enables the decorative layer to be more evenly applied on the anti-mildew layer, and then the porous paper-based facing material is completely dried through a second heat treatment at 100°C to 110°C.

[0065] Example 1

[0066] This embodiment provides a porous paper-based facing material, which is prepared by the following steps:

[0067] S1. Mix chitosan in ethanol and water at a mass ratio of chitosan: ethanol: water = 10:25:100, add acid to adjust the pH value to 3-4, and obtain liquid A;

[0068] S2, according to the mass ratio of silicon tetrachloride: water = 8:100, according to the amount of water added in S1, silicon tetrachloride was added to liquid A and stirred simultaneously, and after the addition was completed, stirring was continued for 1.5 hours, and alkali was added to adjust the pH value to 11-12, and the mixture was allowed to stand for 15 hours to obtain a silica sol containing chitosan;

[0069] S3, immersing the silica sol in ethanol and aging it for 48 hours, taking it out and sending it into a vacuum reactor filled with ethanol, keeping it warm and pressurized for 2 hours at a temperature of 260° C. to 270° C. and a pressure of 6.7 MPa to 7.0 MPa, cooling and releasing the pressure after the treatment, separating, washing with water, and drying to obtain hollow silica particles;

[0070] S4. Mix the raw materials including surfactant, emulsifier, wetting agent, defoamer, oxalic acid, chitosan, potassium sorbate, polyethylene glycol, water-soluble acrylate and water according to the mass ratio of surfactant: emulsifier: wetting agent: defoamer: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = 0.5:0.5:1:1:3:8:10:12:25:100 to obtain a first mixture; heat the first mixture to 50° C., and ultrasonically disperse it for 20 minutes under heat preservation conditions to obtain an anti-mildew coating;

[0071] S6. Mixing raw materials including a color regulator, a gloss regulator, sodium alginate, polyacrylamide, a water-soluble acrylate and water in a mass ratio of color regulator: gloss regulator: sodium alginate: polyacrylamide: water-soluble acrylate: water = 6:2:4:16:22:100 to obtain a second mixture; ultrasonically dispersing the second mixture for 20 minutes to obtain a decorative coating;

[0072] S7. Mixing raw materials including wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of 3:4:6:15:25:100 to obtain pulp; the pulp has a beating degree of 35°SR and a wet weight of 2.4 g; placing the pulp on a screen to obtain wet paper sheets; pressing, drying and calendering the wet paper sheets to obtain a porous paper base;

[0073] S8. Apply a thin coat of the anti-mildew paint to the paper base layer at a mass ratio of anti-mildew paint: decorative paint = 1:1, and perform a first heat treatment at a temperature of 80°C to 90°C until the anti-mildew layer is in a semi-dry but not completely dry state, so as to form an anti-mildew layer on the porous paper base layer; apply the decorative paint to the anti-mildew layer, and perform a second heat treatment at a temperature of 100°C to 110°C until the anti-mildew layer and the decorative layer are completely dry, so as to form a decorative layer on the anti-mildew layer, and obtain a porous paper-based facing material.

[0074] Example 2

[0075] This embodiment provides a porous paper-based facing material, which is prepared by the following steps:

[0076] S1. According to the mass ratio of surfactant: emulsifier: wetting agent: defoaming agent: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = 0.5:0.5:1:1:3:8:10:12:25:100, raw materials including surfactant, emulsifier, wetting agent, defoaming agent, oxalic acid, chitosan, potassium sorbate, polyethylene glycol, water-soluble acrylate and water are mixed to obtain a first mixture; the first mixture is heated to 50° C. and ultrasonically dispersed for 20 minutes under heat preservation conditions to obtain an anti-mildew coating;

[0077] S2. Mixing raw materials including a color regulator, a gloss regulator, sodium alginate, polyacrylamide, a water-soluble acrylate and water in a mass ratio of color regulator: gloss regulator: sodium alginate: polyacrylamide: water-soluble acrylate: water = 6:2:4:16:22:100 to obtain a second mixture; ultrasonically dispersing the second mixture for 20 minutes to obtain a decorative coating;

[0078] S3. Mix raw materials including wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous pulp and bleached broadleaf pulp according to the mass ratio of wet strength agent: aluminum sulfate: cationic polyacrylamide: silica particles: bleached coniferous pulp: bleached broadleaf pulp = 3:4:6:15:25:100 to obtain pulp; the pulp has a beating degree of 35°SR and a wet weight of 2.4 g; the pulp is placed on a screen to obtain wet paper sheets; the wet paper sheets are pressed, dried and calendered to obtain a porous paper base; wherein the silica particles are nano silica particles purchased from commercial channels;

[0079] S8. Apply a thin coat of the anti-mildew paint to the paper base layer at a mass ratio of anti-mildew paint: decorative paint = 1:1, and perform a first heat treatment at a temperature of 80°C to 90°C until the anti-mildew layer is in a semi-dry but not completely dry state, so as to form an anti-mildew layer on the porous paper base layer; apply the decorative paint to the anti-mildew layer, and perform a second heat treatment at a temperature of 100°C to 110°C until the anti-mildew layer and the decorative layer are completely dry, so as to form a decorative layer on the anti-mildew layer, and obtain a porous paper-based facing material.

[0080] Example 3

[0081] This embodiment provides a porous paper-based facing material, which is prepared by the following steps:

[0082] S1. Mix chitosan in ethanol and water at a mass ratio of chitosan: ethanol: water = 10:25:100, add acid to adjust the pH value to 3-4, and obtain liquid A;

[0083] S2, according to the mass ratio of silicon tetrachloride: water = 8:100, according to the amount of water added in S1, silicon tetrachloride was added to liquid A and stirred simultaneously, and after the addition was completed, stirring was continued for 1.5 hours, and alkali was added to adjust the pH value to 11-12, and the mixture was allowed to stand for 15 hours to obtain a silica sol containing chitosan;

[0084] S3, immersing the silica sol in ethanol and aging it for 48 hours, taking it out and sending it into a vacuum reactor filled with ethanol, keeping it warm and pressurized for 2 hours at a temperature of 260° C. to 270° C. and a pressure of 6.7 MPa to 7.0 MPa, cooling and releasing the pressure after the treatment, separating, washing with water, and drying to obtain hollow silica particles;

[0085] S4. Mixing raw materials including surfactant, emulsifier, wetting agent, defoamer, oxalic acid, potassium sorbate, polyethylene glycol, water-soluble acrylate and water according to the mass ratio of surfactant: emulsifier: wetting agent: defoamer: oxalic acid: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = 0.5:0.5:1:1:3:8:10:22:25:100 to obtain a first mixture; heating the first mixture to 50° C., and ultrasonically dispersing it for 20 minutes under heat preservation conditions to obtain a first coating;

[0086] S6, mixing the raw materials including the color regulator, the gloss regulator, the polyacrylamide, the water-soluble acrylate and water in a mass ratio of the color regulator: the gloss regulator: the polyacrylamide: the water-soluble acrylate: the water = 6:2:20:22:100 to obtain a second mixture; ultrasonically dispersing the second mixture for 20 minutes to obtain a second coating;

[0087] S7. Mixing raw materials including wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of 3:4:6:15:25:100 to obtain pulp; the pulp has a beating degree of 35°SR and a wet weight of 2.4 g; placing the pulp on a screen to obtain wet paper sheets; pressing, drying and calendering the wet paper sheets to obtain a porous paper base;

[0088] S8. Apply a thin coat of the first coating to the paper base layer at a mass ratio of first coating: second coating = 1:1, and perform a first heat treatment at a temperature of 80°C to 90°C until the first layer is in a semi-dry but not completely dry state, so as to form a first layer on the porous paper base layer; apply the second coating to the first layer, and perform a second heat treatment at a temperature of 100°C to 110°C until the first layer and the second layer are completely dry, so as to obtain a porous paper-based finishing material.

[0089] Performance Testing

[0090] The tensile strength of the paper obtained in Examples 1-3 was tested with reference to GB / T 12914-2008. The longitudinal tensile strength of the paper obtained in Examples 1-3 was 33.5N / 15mm, 32.9N / 15mm and 33.1N / 15mm, respectively. The wear rate of the paper obtained in Examples 1-3 was tested using a material surface performance comprehensive tester. The wear rate of the paper obtained in Examples 1-3 was 2.04mm 3 / J, 2.76mm 3 / J, 2.69mm 3 / J. The thermal conductivity of the papers obtained in Examples 1-3 was tested by the hot box method of GB / T13475-2008. The thermal conductivity of the papers obtained in Examples 1-3 was 0.029W / (m·K), 0.051W / (m·K), and 0.032W / (m·K), respectively. The antibacterial properties and anti-mildew effects of the papers obtained in Examples 1-3 were tested according to GB / T 21866-2008. The tested fungi included Aspergillus flavus, Aspergillus niger, Penicillium, and Soil mold. The papers obtained in Examples 1 and 2 had no mold growth within 6 months. The mold growth area of ​​the paper obtained in Example 3 was 0.4% within 6 months.

Claims

1. A method for preparing a porous paper-based facing material, It is characterized in that The preparation method comprises: S100, preparing a porous paper base, an anti-mildew coating, and a decorative coating respectively; S200, applying the anti-mildew coating to the paper base layer, and performing a first heat treatment to form an anti-mildew layer on the porous paper base layer; S300, applying the decorative coating to the anti-mildew layer, and performing a second heat treatment to form a decorative layer on the anti-mildew layer, and obtaining the porous paper-based facing material; Wherein, the porous paper base layer comprises hollow silica particles, the anti-mildew coating comprises chitosan, and the decorative coating comprises sodium alginate.

2. The preparation method according to claim 1, It is characterized in that The porous paper substrate is prepared by the following steps: S111, mixing raw materials including a wet strength agent, aluminum sulfate, cationic polyacrylamide, hollow silica particles, bleached coniferous wood pulp and bleached hardwood wood pulp to obtain pulp; S112, placing the slurry on a screen to make paper sheets to obtain wet paper sheets; S113, pressing, drying and calendering the wet paper sheet to obtain the porous paper base layer.

3. The preparation method according to claim 2, It is characterized in that In S111, by mass ratio, wet strength agent: aluminum sulfate: cationic polyacrylamide: hollow silica particles: bleached coniferous wood pulp: bleached hardwood wood pulp = (3-4): (4-5): (5-6): (12-16): (15-25):

100.

4. The preparation method according to claim 2, It is characterized in that In S111, the slurry has a beating degree of 30°SR to 45°SR and a wet weight of 2.0 g to 3.0 g.

5. The preparation method according to claim 1, It is characterized in that The anti-mildew coating is prepared by the following steps: S121, mixing raw materials including a surfactant, an emulsifier, a wetting agent, a defoaming agent, oxalic acid, chitosan, potassium sorbate, polyethylene glycol, a water-soluble acrylate and water to obtain a first mixture; S122, heating the first mixture to 45° C. to 55° C., and ultrasonically dispersing the mixture for 20 min to 30 min under heat preservation conditions to obtain the anti-mildew coating.

6. The preparation method according to claim 5, It is characterized in that In S121, in terms of mass ratio, surfactant: emulsifier: wetting agent: defoaming agent: oxalic acid: chitosan: potassium sorbate: polyethylene glycol: water-soluble acrylate: water = (0.2-1): (0.5-1.5): (0.5-1.5): (0.5-1.5): (2-4): (6-8): (8-10): (10-12): (20-30):

100.

7. The preparation method according to claim 1, It is characterized in that The decorative coating is prepared by the following steps: S131, mixing raw materials including a color regulator, a gloss regulator, sodium alginate, polyacrylamide, a water-soluble acrylate and water to obtain a second mixture; S132, ultrasonically dispersing the second mixture for 20 to 30 minutes to obtain the decorative coating.

8. The preparation method according to claim 7, It is characterized in that In S131, the mass ratio of color adjuster: glossiness adjuster: sodium alginate: polyacrylamide: water-soluble acrylate: water = (2-8): (2-8): (4-6): (16-20): (20-30):

100.

9. The preparation method according to any one of claims 1 to 8, It is characterized in that The temperature of the first heat treatment is 80°C to 90°C, and the temperature of the second heat treatment is 100°C to 110°C.

10. A porous paper-based facing material, It is characterized in that The porous paper-based facing material is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Mildew-proof preservative paper and preparation method and preparation device thereof

    CN106638157A

  • Mildew-proof and fresh-keeping paper and preparation method thereof

    CN108060610A

  • Antibacterial and mildew-proof wallpaper and preparation method thereof

    CN112176776A

  • Anti-condensation mildew-proof coating and preparation method thereof

    CN112266665A

  • Environment-friendly plastic-replacing glazing oil and application thereof in paper product packaging

    CN114592381A