Printing reflective material and preparation method thereof
By setting up a directional quaternary ammonium salt ion film and adding color base layer on the glass microbead surface of the bead planting film, combining electronic inkjet printing and hot pressing composite processes, the problem of difficult to take into account the color and brightness of color reflective materials in the prior art. The preparation of printed reflective materials with high retroreflection coefficient and water washing fastness is achieved, which improves production efficiency and accuracy.
Patent Information
- Application Number
- CN202410942617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
It is difficult to achieve high retroreflective coefficient and water-washing color fastness when existing color reflective materials ensure bright colors, and the processing technology is complex, the operation accuracy is high, and the output is difficult to control.
The surface of the glass microbeads of the bead planting film is arranged, and a color bottom layer and a metal evaporation layer are added under the ink layer. The electronic inkjet printing and hot pressing composite process are used to control the thickness of the ink and glue layer. Improve printing performance and washing fastness.
The color is bright and the retroreflection coefficient reaches 200-520, the brightness remains 250-350 after washing, and the color fastness is above 4 levels, which has high production efficiency and is simple and fast.
Smart Images

Figure BDA0004944637180000091 
Figure BDA0004944637180000101 
Figure BDA0004944637180000102
Abstract
Description
Technical Field
[0001] The invention relates to a printed reflective material and a preparation method thereof, and relates to G02B, and in particular to the field of optical elements and systems. Background Art
[0002] As people's requirements for fashion and aesthetics of materials increase, printed reflective materials can better meet people's aesthetic requirements, but the processing technology is limited and it is difficult to achieve good effects of printing color and brightness at the same time. There are two existing methods for preparing colored reflective printed materials. One is to add pigments to the composite adhesive layer to give color, and the other is to use a digital printing machine to print on the surface of the reflective material to produce colored printed materials with reflective properties. However, adding pigments to the composite adhesive layer will reduce the bonding effect of the composite adhesive layer. At the same time, the color of the obtained color print is relatively single. The color of the digital printing technology has a large deviation from different production batches, which requires high operating accuracy of workers, and the production volume is difficult to control. The stability of water-based ink products is poor, and it is difficult to achieve both color and brightness. Therefore, it is very important to develop a reflective product that has a high retroreflection coefficient and excellent water washing color fastness while ensuring bright colors.
[0003] Chinese invention patent CN202021636926.7 discloses a fantasy reflective film, by adding an ink layer and a transparent resin layer on the upper and lower surfaces of the luminous layer inside the fantasy reflective film, the color and built-in pattern of the first ink layer and the second ink layer can use different colors and patterns according to the required situation, thereby improving the practicality of the fantasy reflective film. However, the glass beads of the fantasy reflective film are located in the middle of the film, and the degree of reflection is weak. Chinese invention patent CN202111080987.9 discloses a production process for a fancy reflective beaded film, by printing a pattern layer with a washable first medium on the surface of the glass bead layer, then vapor-depositing the second medium, and washing away the pattern layer of the first medium, a colorful reflective pattern and a transparent reflective pattern are obtained, but the pattern color of the vapor-deposited metal is single, and the diversity of ink colors cannot be achieved. Summary of the invention
[0004] In order to prepare a reflective material having both color saturation and reflective properties and excellent washing color fastness, the first aspect of the present invention provides a printed reflective material, which comprises, from bottom to top, a substrate layer, a glue layer, a color base layer, an ink layer, and glass beads.
[0005] As a preferred embodiment, a directional quaternary ammonium salt ion membrane is arranged on the surface of the glass microspheres, and the particle size of the glass microspheres is 15-110 μm.
[0006] As a preferred embodiment, the particle size of the glass microbeads is 40-75 μm. Preferably, the particle size of the glass microbeads is 50-75 μm. Preferably, the particle size of the glass microbeads is 42-50 μm.
[0007] As a preferred embodiment, the quaternary ammonium salt ion membrane is obtained by immersing glass microbeads in a cationic solution, wherein the cationic solution is a combination of a cationic substance and a coupling agent. Preferably, the weight ratio of the cationic substance to the coupling agent is (1-3): (1-3).
[0008] As a preferred embodiment, the weight ratio of the cationic substance to the coupling agent is 1:1.
[0009] As a preferred embodiment, the cationic substance is selected from one or a combination of stearyl trimethyl ammonium chloride, stearyl dimethyl amyl ammonium chloride, octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, trihydroxyethyl methyl quaternary ammonium methyl sulfate, and N,N-hexadecyl ethyl morpholine ethyl sulfate.
[0010] As a preferred embodiment, the coupling agent is a silane coupling agent containing an epoxy group. Preferably, the coupling agent is silane coupling agent KH-560.
[0011] As a preferred embodiment, the processing method of the glass microspheres includes the following steps:
[0012] Mix the cationic substance and coupling agent, heat to 60-100℃, add glass beads and stir at 1000rps for 1-5min, take out and dry at 80-150℃ for 30-90min.
[0013] During the experiment, the applicant found that when printing ink onto the surface of the glass microbeads of the implanted bead membrane, problems such as poor ink drying and uneven ink spraying would occur. After a large number of experimental studies, the applicant found that when the ink flows on the printing press, the friction between the ink molecules and the movement of ions cause charge separation, and the friction between the ink surface and the glass microbeads causes the movement of electrostatic particles, resulting in the accumulation of electrostatic charge, which causes the problems of poor ink drying and uneven ink spraying. The applicant found that by providing a layer of directional quaternary ammonium salt ion membrane on the surface of the glass microbeads of the implanted bead membrane, the electrostatic effect between the ink printing and the glass microbeads can be avoided, and the printing performance of the ink can be improved. It is speculated that the possible reason is: the glass microbeads of the implanted bead membrane are immersed in a quaternary ammonium salt solution, and the quaternary ammonium salt solution with cations can form a directional cationic membrane on the surface of the glass microbeads to eliminate the electrostatic attraction between the glass microbeads and the ink, and between the inks.
[0014] The applicant further discovered that the surface tension of the quaternary ammonium salt solution is relatively large and it is not easy to form a film on the surface of the glass beads. By introducing a silane coupling agent, the surface tension between the interfaces can be reduced, thereby reducing the difficulty of the quaternary ammonium salt ion film adsorbing onto the surface of the glass beads, thereby achieving the technical effect of improving ink printing.
[0015] As a preferred embodiment, the ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 1-5 μm.
[0016] As a preferred embodiment, the ink layer has a thickness of 2-3 μm.
[0017] As a preferred implementation, the thickness of the ink layer is 3 μm.
[0018] As a preferred embodiment, the ink of the ink layer includes a colorant, a color fixing agent and a dispersant, and the weight ratio of the colorant, the color fixing agent and the dispersant is (0.2-2): (1-10): (0-5).
[0019] As a preferred embodiment, the ink is selected from one or a combination of the series such as Konica 512i-PL, Starlight 1024-10PL, Starlight 1024-25PL, Hongyin ECO-AP3200, Decai Digital DC-A-HS, and Honghua Digital CPK00060.
[0020] As a preferred embodiment, the color base layer is a metal vapor deposition layer or a white ink layer, and the thickness of the white ink layer is 0-10 μm. Preferably, the thickness of the white ink layer is 0.5-3 μm. More preferably, the thickness of the white ink layer is 2 μm.
[0021] As a preferred embodiment, the white ink in the white ink layer is selected from one or a combination of the series such as Konica 512i-PL, Starlight 1024-10PL, Starlight 1024-25PL, Hongyin ECO-AP3200, and Honghua Digital CPK00060.
[0022] As a preferred implementation, the white ink in the white ink layer is a mixed color of Konica 512i series inks of Flora.
[0023] The Starlight 1024-10PL and Starlight 1024-25PL were purchased from Cyber Starlight, and the Hongyin ECO-AP3200 was purchased from Zhejiang Hongyin Digital.
[0024] As a preferred embodiment, the thickness of the metal vapor-deposited layer is 50-200nm, preferably, the thickness of the metal vapor-deposited layer is 100-200nm, and further preferably, the thickness of the metal vapor-deposited layer is 200nm; the raw material for preparing the metal vapor-deposited layer is selected from one or a combination of Al, Ag, ZnS, aluminum oxide, aluminum hydroxide, and silver oxide.
[0025] The raw material for preparing the metal vapor deposition layer is Al.
[0026] As a preferred embodiment, the adhesive layer is a polyurethane adhesive layer or an acrylate adhesive layer, and the thickness of the adhesive layer is 50-300 μm. Preferably, the thickness of the adhesive layer is 160-200 μm. More preferably, the thickness of the adhesive layer is 200 μm.
[0027] As a preferred implementation, the number average molecular weight of the polyurethane in the polyurethane adhesive layer is 3000-4000 kg / mol, and the number average molecular weight of the acrylate in the acrylate adhesive layer is 220000-230000 kg / mol.
[0028] As a preferred embodiment, the substrate layer is selected from one or a combination of knitted fabric, woven fabric, non-woven fabric, TPU, and PES.
[0029] A second aspect of the present invention provides a method for preparing a printed reflective material, comprising the following steps:
[0030] S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it;
[0031] S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer;
[0032] S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer;
[0033] S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
[0034] As a preferred implementation, the drying temperature in step S1 is 50-70° C., and the drying time is 1-2 min.
[0035] As a preferred embodiment, the drying procedure in step S4 is a gradient heating and cooling process. The product continuously passes through 60°C, 80°C, and 100°C, and then passes through a cooling zone of 80°C and a 60°C oven. The product is continuously processed at a speed of 2-5min / m, and each temperature interval is 1-2min.
[0036] As a preferred implementation, the hot pressing temperature in step S4 is 60-130° C., and the hot pressing pressure is 0.2-3 MPa.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The printed reflective material of the present invention can avoid the electrostatic interaction between the ink printing and the glass microbeads by arranging a layer of oriented quaternary ammonium salt ion membrane on the surface of the glass microbeads of the implanted bead membrane, thereby improving the printing performance and drying performance of the ink.
[0039] (2) The printed reflective material of the present invention has a color base layer arranged under the ink layer, and the color base layer is controlled to be a 0.5-3 μm white ink layer or a 100-200 nm metal vapor deposition layer, so that the product can have a retroreflection coefficient of 200-520 while ensuring bright colors, while ensuring high quality and high precision of colors or patterns.
[0040] (3) The printed reflective material of the present invention adopts a digital inkjet printing method and controls the thickness of the adhesive layer, which can improve the water washing fastness. At 40°C, after washing 25 times*1h, the brightness can still reach 250-350 after washing, and the color fastness is above level 4. The production efficiency is high and the production is simple and quick. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a schematic diagram of the structure of the printed reflective material of the present invention;
[0042] Figure 2 The effect on the bead-planting film during the production process of the printed reflective material of the present invention;
[0043] Figure 3 This is the finished product effect of the printed reflective material of the present invention;
[0044] Figure 4 This is the finished product effect of the printed reflective material of the present invention;
[0045] Figure 5 The reflective effect of the finished product of the printed reflective material of the present invention;
[0046] In the figure: 1. Glass beads; 2. Ink layer; 3. Color base layer; 4. Glue layer; 5. Base material layer. DETAILED DESCRIPTION
[0047] Example 1
[0048] A printed reflective material comprises, from bottom to top, a substrate layer 5, a glue layer 4, a color base layer 3, an ink layer 2, and glass microbeads 1.
[0049] The surface of the glass microspheres is provided with a directional quaternary ammonium salt ion membrane, the particle size of the glass microspheres is 50-75 μm, and they are purchased from Zhejiang Xinghua New Materials Group Co., Ltd.
[0050] The processing method of the glass microspheres comprises the following steps:
[0051] Mix the cationic substance and coupling agent, heat to 90℃, add glass beads and stir at 1000rps for 4min, take out and dry at 120℃ for 60min.
[0052] The weight ratio of the cationic substance to the coupling agent is 1: 1. The cationic substance is octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, and the coupling agent is silane coupling agent KH-560.
[0053] The ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 2 μm.
[0054] The ink was purchased from Flora Konica 512i.
[0055] The color bottom layer is a metal vapor-deposited layer, the thickness of the metal vapor-deposited layer is 150nm, and the raw material for preparing the metal vapor-deposited layer is Al.
[0056] The adhesive layer is a polyurethane adhesive layer with a thickness of 200 μm. The polyurethane in the polyurethane adhesive layer has a number average molecular weight of 3000-4000 kg / mol and a solid content of 50 wt %, and is purchased from Zhejiang Xinghua Reflective Materials Co., Ltd., model 411.
[0057] The base material layer is a woven fabric, which is a 190T polyester pongee fabric.
[0058] A method for preparing a printed reflective material comprises the following steps:
[0059] S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it;
[0060] S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer;
[0061] S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer;
[0062] S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
[0063] The drying temperature in step S1 is 60° C. and the drying time is 1 min.
[0064] The drying procedure in step S4 is a gradient heating and cooling process. The product is continuously heated at 60°C, 80°C, and 100°C, and then passes through a cooling zone at 80°C and a 60°C oven. The product is continuously processed at a speed of 2min / m, and each temperature interval is 2min.
[0065] The hot pressing temperature in step S4 is 120° C. and the hot pressing pressure is 1 MPa.
[0066] Example 2
[0067] A printed reflective material comprises, from bottom to top, a substrate layer 5, a glue layer 4, a color base layer 3, an ink layer 2, and glass microbeads 1.
[0068] The surface of the glass microspheres is provided with a directional quaternary ammonium salt ion membrane, the particle size of the glass microspheres is 42-50 μm, and they are purchased from Zhejiang Xinghua New Materials Group Co., Ltd.
[0069] The processing method of the glass microspheres comprises the following steps:
[0070] Mix the cationic substance and coupling agent, heat to 90℃, add glass beads and stir at 1000rps for 4min, take out and dry at 120℃ for 60min.
[0071] The weight ratio of the cationic substance to the coupling agent is 1: 1. The cationic substance is octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, and the coupling agent is silane coupling agent KH-560.
[0072] The ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 3 μm.
[0073] The ink was purchased from Starlight 1024-10PL.
[0074] The color bottom layer is a metal vapor-deposited layer, the thickness of the metal vapor-deposited layer is 200nm, and the raw material for preparing the metal vapor-deposited layer is Al.
[0075] The adhesive layer is a polyurethane adhesive layer with a thickness of 200 μm. The polyurethane in the polyurethane adhesive layer has a number average molecular weight of 3000-4000 kg / mol and a solid content of 50 wt %, and is purchased from Zhejiang Xinghua Reflective Materials Co., Ltd., model 608.
[0076] The substrate layer is TPU purchased from Tianyang New Materials, model F6202.
[0077] A method for preparing a printed reflective material comprises the following steps:
[0078] S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it;
[0079] S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer;
[0080] S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer;
[0081] S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
[0082] The drying temperature in step S1 is 60° C. and the drying time is 1 min.
[0083] The drying procedure in step S4 is a gradient heating and cooling process. The product is continuously heated at 60°C, 80°C, and 100°C, and then passes through a cooling zone at 80°C and a 60°C oven. The product is continuously processed at a speed of 2min / m, and each temperature interval is 2min.
[0084] The hot pressing temperature in step S4 is 120° C. and the hot pressing pressure is 1 MPa.
[0085] Example 3
[0086] A printed reflective material comprises, from bottom to top, a substrate layer 5, a glue layer 4, a color base layer 3, an ink layer 2, and glass microbeads 1.
[0087] The surface of the glass microspheres is provided with a directional quaternary ammonium salt ion membrane, the particle size of the glass microspheres is 42-50 μm, and they are purchased from Zhejiang Xinghua New Materials Group Co., Ltd.
[0088] The processing method of the glass microspheres comprises the following steps:
[0089] Mix the cationic substance and the coupling agent, heat to 90°C, add glass beads and stir at 1000rps for 4 minutes, then dry and heat at 120°C for 60 minutes.
[0090] The weight ratio of the cationic substance to the coupling agent is 1: 1. The cationic substance is octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, and the coupling agent is silane coupling agent KH-560.
[0091] The ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 4 μm.
[0092] The ink was purchased from TAMISCONICA 512i-PL.
[0093] The color bottom layer is a metal vapor-deposited layer, the thickness of the metal vapor-deposited layer is 150nm, and the raw material for preparing the metal vapor-deposited layer is Al.
[0094] The adhesive layer is a polyurethane adhesive layer with a thickness of 160 μm. The polyurethane in the polyurethane adhesive layer has a number average molecular weight of 3000-4000 kg / mol and a solid content of 50 wt %, and is purchased from Zhejiang Xinghua Reflective Materials Co., Ltd., model 413.
[0095] The base material layer is a woven fabric, which is a 190T polyester pongee fabric.
[0096] A method for preparing a printed reflective material comprises the following steps:
[0097] S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it;
[0098] S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer;
[0099] S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer;
[0100] S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
[0101] The drying temperature in step S1 is 60° C. and the drying time is 1 min.
[0102] The drying procedure in step S4 is a gradient heating and cooling process. The product is continuously heated at 60°C, 80°C, and 100°C, and then passes through a cooling zone at 80°C and a 60°C oven. The product is continuously processed at a speed of 2min / m, and each temperature interval is 2min.
[0103] The hot pressing temperature in step S4 is 120° C. and the hot pressing pressure is 1 MPa.
[0104] Example 4
[0105] A printed reflective material comprises, from bottom to top, a substrate layer 5, a glue layer 4, a color base layer 3, an ink layer 2, and glass microbeads 1.
[0106] The surface of the glass microspheres is provided with a directional quaternary ammonium salt ion membrane, the particle size of the glass microspheres is 42-50 μm, and they are purchased from Zhejiang Xinghua New Materials Group Co., Ltd.
[0107] The processing method of the glass microspheres comprises the following steps:
[0108] Mix the cationic substance with the coupling agent solution, heat it to 90°C, put in glass beads and stir for 4 minutes at 1000rps, take it out and dry it at 120°C for 60 minutes.
[0109] The weight ratio of the cationic substance to the coupling agent is 1: 1. The cationic substance is trihydroxyethyl methyl quaternary ammonium methyl sulfate, and the coupling agent is silane coupling agent KH-560.
[0110] The ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 3 μm.
[0111] The ink was purchased from Honghua Digital CPK00060 series.
[0112] The color bottom layer is a white ink layer purchased from Honghua Digital CPK00060 series, and the thickness of the white ink layer is 2 μm.
[0113] The adhesive layer is a polyurethane adhesive layer, the thickness of the adhesive layer is 200 μm, and the number average molecular weight of the polyurethane in the polyurethane adhesive layer is 3000-4000.
[0114] The substrate layer is TPU purchased from Tianyang New Materials, model F6201.
[0115] A method for preparing a printed reflective material comprises the following steps:
[0116] S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it;
[0117] S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer;
[0118] S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer;
[0119] S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
[0120] The drying temperature in step S1 is 60° C. and the drying time is 1 min.
[0121] The drying procedure in step S4 is a gradient heating and cooling process. The product is continuously heated at 60°C, 80°C, and 100°C, and then passes through a cooling zone at 80°C and a 60°C oven. The product is continuously processed at a speed of 2min / m, and each temperature interval is 2min.
[0122] The hot pressing temperature in step S4 is 120° C. and the hot pressing pressure is 1 MPa.
[0123] Comparative Example 1
[0124] A printed reflective material and a preparation method thereof. The specific implementation manner is the same as that of Example 2, except that the color base layer is a metal vapor-deposited layer, and the thickness of the metal vapor-deposited layer is 1.5 μm.
[0125] Comparative Example 2
[0126] A printed reflective material and a preparation method thereof, the specific implementation is the same as that of Example 4, except that the thickness of the ink layer is 6 μm, the thickness of the white ink layer is 5 μm, and the thickness of the adhesive layer is 160 μm. The substrate layer is a woven fabric, which is a 190T polyester pongee fabric.
[0127] Comparative Example 3
[0128] A printed reflective material and a preparation method thereof. The specific implementation manner is the same as that of comparative example 2, except that the particle size of the glass microbeads is 33-42 μm and is purchased from Zhejiang Xinghua New Materials Group Co., Ltd.
[0129] The ink layer has a thickness of 8 μm, and the white ink layer has a thickness of 10 μm.
[0130] Performance Testing
[0131] 1. Retroreflection coefficient: Before washing, use a retroreflection coefficient tester to test at an incident angle of 5° and an observation angle of 12°, then wash 25 times at 40°C, 1 hour per time, and test the retroreflection coefficient after washing. The test results are shown in Table 2.
[0132] 2. Washing fastness:
[0133] ① Sample preparation requirements: The sample size is 5×25cm, and one sample is taken from the left, middle, and right sides of the sample width. When the fabric is a colorful or gradient color product, both the color and silver parts must be taken.
[0134] ②Sewing requirements: It needs to be sewn on the existing conventional 30×30cm base fabric. Two strips should be sewn on each base fabric, with an interval of 5cm and 5cm from the edge. When sewing, the middle of the strip should be folded as shown in the figure below, and the folded part should be controlled to be about 1cm.
[0135] ③ Washing method: refer to ISO 6330 4N, water hardness: <0.7mmol / L, detergent: ECE detergent 20g / time, washing machine: Siemens household drum washing machine, washing program: cotton standard 40℃, when the water hardness is higher than the required value, use deionized water and add the corresponding amount of calcium chloride to adjust the hardness to the required range. Washing times: 25 times. Evaluation criteria are shown in Table 1. Test results are shown in Table 2.
[0136] Table 1
[0137]
[0138]
[0139] 3. Color fastness:
[0140] ① Sample preparation requirements: Product size should not be less than 40mm×100mm, and two samples should be taken from different parts of the wide width.
[0141] ②Test requirements: The textile sample is sewn together with standard cotton and polyester adjacent fabrics, placed in soap solution or a mixture of soap and anhydrous sodium carbonate, and mechanically agitated in a solution with a bath ratio of 50:1 at the specified conditions of 30 minutes and 40°C, and then washed and dried. The original sample is used as a reference sample, and the gray sample card is used to evaluate the color change of the sample and the staining of the adjacent fabric. Test the color fastness after washing at 40°C for 25 hours.
[0142] The standard GB / T250 gray card is used for color judgment. The gray card consists of five pairs of matte gray cards, which are divided into five fastness levels according to the discernible color difference, namely 5, 4, 3, 2, and 1. Add half a level to every two levels, namely 4-5, 3-4, 2-3, and 1-2, and it will be expanded to a five-level nine-level gray card. The first component of each pair is neutral gray, among which only the second component of fastness level 5 is consistent with the first component, and the second components of other pairs become lighter in turn, and the color difference increases step by step. The color difference of each level is determined by chromaticity.
[0143] The test results are shown in Table 2.
[0144] Table 2
[0145]
[0146]
Claims
1. A printed reflective material, characterized in that: The printed reflective material comprises, from bottom to top, a substrate layer, a glue layer, a color base layer, an ink layer, and glass microbeads.
2. The printed reflective material according to claim 1, characterized in that: A directional quaternary ammonium salt ion membrane is arranged on the surface of the glass microbeads, and the particle size of the glass microbeads is 15-110 μm.
3. The printed reflective material according to claim 2, characterized in that: The quaternary ammonium salt ion membrane is obtained by soaking glass microbeads in a cationic solution, wherein the cationic solution is a combination of a cationic substance and a coupling agent. Preferably, the weight ratio of the cationic substance to the coupling agent is (1-3): (1-3).
4. The printed reflective material according to claim 3, characterized in that: The cationic substance is selected from one or a combination of stearyl trimethyl ammonium chloride, stearyl dimethyl amyl ammonium chloride, octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, trihydroxyethyl methyl quaternary ammonium methyl sulfate, and N,N-hexadecyl ethyl morpholine ethyl sulfate.
5. The printed reflective material according to claim 1, characterized in that: The ink layer is printed by an electronic inkjet printer, and the thickness of the ink layer is 1-5 μm.
6. The printed reflective material according to claim 1, characterized in that: The color bottom layer is a metal vapor deposition layer or a white ink layer, and the thickness of the white ink layer is 0-10 μm.
7. The printed reflective material according to claim 6, characterized in that: The thickness of the metal vapor-deposited layer is 50-200 nm, and the raw materials for preparing the metal vapor-deposited layer are selected from one or a combination of Al, Ag, ZnS, aluminum oxide, aluminum hydroxide, and silver oxide.
8. The printed reflective material according to claim 1, characterized in that: The adhesive layer is a polyurethane adhesive layer or an acrylic adhesive layer, and the thickness of the adhesive layer is 50-300 μm.
9. The printed reflective material according to claim 1, characterized in that: The substrate layer is selected from one or a combination of knitted fabric, woven fabric, non-woven fabric, TPU, and PES.
10. A method for preparing the printed reflective material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1 prints an ink layer on the surface of the glass microbeads of the implanted bead film and dries it; S2 superimposes a color base layer on the surface of the dried ink layer to control the thickness of the color base layer; S3 then the bead-planting film is unwound and passed through the glue coating area, and the glue coating amount is controlled to obtain a glue layer; S4 is drying, and the adhesive layer and the base material layer are composited and hot pressed to obtain.
Citation Information
Patent Citations
Production process of fancy reflective bead planting film
CN113777683A
Colorful reflective film
CN212749301U
Antistatic light reflection cloth and preparation method therefor
CN104965246A
Manufacturing process of washable high-brightness colored reflective product
CN111515109A
High-strength tear-resistant reflective film and preparation process thereof
CN111897040A