Electron selective passivation contact structure and application thereof
By using magnesium oxide as an electron-selective passivation contact structure in crystalline silicon solar cells, combining silicon oxide tunneling layer and hydrogen passivation cap layer, the efficiency limitations and optical parasitic absorption problems of metal-semiconductor contact areas are solved, and the problem of improvement of the The conversion efficiency and short-circuit current density of solar cells reduce preparation costs and energy consumption.
Patent Information
- Application Number
- CN202410850852.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-05
AI Technical Summary
There are problems in crystalline silicon solar cells with Auger recombination and band gap narrowing in metal-semiconductor contact areas, resulting in limited conversion efficiency and difficult regulation of doping concentration in non-metal contact areas, affecting device efficiency; at the same time, the existing The passivated contact structure has problems with optical parasitic absorption, use of flammable and toxic gases and production energy consumption.
Magnesium oxide is used as an electron selective passivation contact structure, by depositing the silicon oxide tunneling layer, the magnesium oxide layer and the hydrogen passivation cap layer in sequence, the optical and electrical properties of the doped magnesium oxide layer are optimized, the contact resistance is reduced, and the contact resistance is reduced through The atomic layer deposition process controls thickness and doping concentration to achieve excellent surface passivation and electron selective transmission.
The absolute photoelectric conversion efficiency of solar cells is improved by about 1% to 3.5%, which significantly improves the short-circuit current density Jsc, and avoids optical parasitic absorption problems caused by silicon thin films, reducing preparation costs and energy consumption.
Smart Images

Figure CN118899346A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to an electron selective passivation contact structure and application thereof. Background Art
[0002] At present, the crystalline silicon cell industry generally adopts the passivated emitter and rear surface (PERC) structure design, which uses heavily doped p + or + The emitter enables carriers to be transported selectively, and the highly doped region helps the carriers to be transported laterally to the metal electrode. Surface passivation and optical antireflection are usually achieved by Al2O3, SiN x Or a combination of them. However, there are some limiting factors in the conversion efficiency of PERC cells, especially in the metal-semiconductor contact area, where high doping leads to problems such as Auger recombination and band gap narrowing, thus affecting device efficiency. In contrast, in the non-metallic contact area, only slight uniform doping is required to ensure carrier transport. This difference in doping concentration requirements is difficult to control, which restricts the device efficiency (generally around 24%).
[0003] To overcome these limitations, a passivation contact structure was developed to achieve both surface passivation and carrier selective transport. The passivation contact structure is usually composed of a multilayer film, mainly including a passivation layer and a carrier selective layer. The passivation contact avoids the recombination loss of the metal-semiconductor contact, thereby improving the open circuit voltage and conversion efficiency of the solar cell.
[0004] At present, heterojunction (HJT) cells and tunnel oxide passivated contact (TOPCon) cells are two successful industrialization technology routes, and their maximum efficiency exceeds 26%. However, these technologies still have some limitations, such as optical parasitic absorption problems, the risk of using flammable and toxic gases, and energy consumption problems in the production process. In response to these problems, some new methods and technologies are being studied, such as doping or preparing microcrystalline silicon in amorphous silicon and polycrystalline silicon. However, the process involved is cumbersome and the equipment cost is high.
[0005] For crystalline silicon solar cells, the presence of surface defects will reduce device efficiency, so high-quality surface passivation is crucial. In recent years, wide-bandgap metal oxides have been widely used in passivation and carrier selection transport layers, such as VO x 、MoO x , WO x etc. can be used for hole transport layer, while TiO2, ZnO, MgO, SrO xetc. can be used for electron transport layer. However, the passivation effect of most single-layer metal oxide films is limited, and they usually need to be used in combination with passivation layers such as silicon oxide, a-Si:H, and Al2O3. Among them, magnesium oxide as an electron selective transport layer mainly relies on its own high electron concentration and bulk conductivity. When magnesium oxide prepared by atomic layer deposition or thermal evaporation is used as the full-area electron transport layer on the back of crystalline silicon cells, the current photoelectric conversion efficiency is limited to 20%, mainly due to the low open circuit voltage V oc The limitation is attributed to the poor passivation performance of monolayer MgO on crystalline silicon surface.
[0006] In general, for crystalline silicon solar cells, passivation contact structure and its preparation method is a promising research and application direction, which is expected to solve a series of technical challenges currently faced by crystalline silicon cells.
[0007] The doping-free passivation contact adopts physical (thermal evaporation, electron beam evaporation) or chemical vapor deposition, and uses wide bandgap metal oxide as the passivation layer and carrier selective transport layer, which can avoid the problems of optical parasitic absorption and high preparation cost caused by silicon film. Magnesium oxide has a low work function (4.2eV) and a wide optical bandgap (7.8eV), which is suitable as an electron selective passivation contact. At present, the applications of magnesium oxide in crystalline silicon solar cells include thermally evaporated magnesium oxide (Conductive and Stable Magnesium Oxide Electron-Selective Contacts for Efficient Silicon Solar Cells. Advanced Energy Materials, 2016, 7, 1601863), electron beam evaporated magnesium oxide (Heterojunction solar cells with asymmetrically carrier-selective contact structure of molybdenum-oxide / silicon / magnesium-oxide. Solar Energy, 2018, 159: 704 and Activating and optimizing evaporation-processed magnesium oxide passivating contact for silicon solar cells. Nano Energy, 2019, 62, 181.), and atomic layer deposited magnesium oxide (Low-Temperature Atomic Layer Deposited Magnesium Oxide as a Passivating Electron Contact for c-Si-Based Solar Cells [J]. IEEE Journal of Photovoltaics, 2020, 10, 398.), but their passivation contact performance and battery performance are poor. At present, the electron-selective passivation contact based on magnesium oxide is mainly limited to the balance between surface passivation performance and contact resistance. Thermally evaporated magnesium oxide has no passivation effect on the crystalline silicon surface. When it is used as a full-area electron-selective contact on the back end of the device, the conversion efficiency (20%) is mainly limited to the low open-circuit voltage (629mV) caused by surface carrier recombination. The practical application of thermal evaporation deposition method on the production line is limited. It is difficult to control the large-area uniform and ultra-thin thickness of magnesium oxide (1nm) by evaporating powder. The open-circuit voltage limit of electron beam evaporated magnesium oxide passivation is iV ocThe open circuit voltage limit is 680-690mV. As the thickness of magnesium oxide increases, the contact resistance increases sharply. The device efficiency is limited by V oc Tradeoffs with FF. Summary of the invention
[0008] The purpose of the present invention is to provide an electron selective passivation contact structure based on magnesium oxide, a preparation method thereof, and a solar cell. The electron selective passivation contact structure has an excellent surface passivation effect, and the maximum open circuit voltage can reach 740mV. Combined with the characteristics of the magnesium oxide material itself, after removing the hydrogen passivation cap layer, magnesium oxide can retain excellent surface passivation and simultaneously realize the electron selective transmission function. The passivation contact structure can be applied to crystalline silicon cells and perovskite-crystalline silicon stacked devices to eliminate optical parasitic absorption caused by silicon thin films and improve the photoelectric conversion efficiency of solar cells. Applying it to the light-incident surface of solar cells can significantly increase the short-circuit current density J sc , about 1mA / cm 2 ~4mA / cm 2 , the absolute photoelectric conversion efficiency can be increased by about 1% to 3.5%.
[0009] The present invention provides an electron selective passivation contact structure, which is arranged on the surface of a silicon substrate, and the surface of the silicon substrate is selected from one of a light-receiving surface and a backlight surface of the silicon substrate; the electron selective passivation contact structure comprises a silicon oxide tunneling layer, a magnesium oxide layer and a hydrogen passivation cap layer deposited in sequence.
[0010] Preferably, the thickness of the magnesium oxide layer is 1-50 nm.
[0011] Preferably, the magnesium oxide layer is selected from an intrinsic magnesium oxide layer or a doped magnesium oxide layer; the doping elements in the doped magnesium oxide layer include one or two of Al, B, H and Zn.
[0012] Furthermore, the doping concentration in the doped magnesium oxide layer is 1% to 20% atomic concentration.
[0013] Furthermore, the magnesium oxide layer is deposited by atomic layer deposition, and the thickness and doping concentration of the doped magnesium oxide layer are controlled by the number of super cycles in an atomic layer deposition super cycle mode and the cycle ratio in a doping sub cycle.
[0014] Specifically, the doping element is boron (B), the doping cycle ratio of magnesium oxide to boron oxide in the atomic layer deposition super cycle mode is 5-60:1; the number of super cycles in the atomic layer deposition super cycle mode is 2-50 times; and the doping atomic concentration of the boron element is 1-20%.
[0015] Preferably, the silicon oxide tunneling layer has a thickness of 0.5-2 nm.
[0016] Furthermore, the preparation method of the silicon oxide tunneling layer is selected from a dry method or a wet method; the dry method is a thermal oxidation method or an ozone oxidation method, and the wet method is a nitric acid oxidation method.
[0017] Preferably, the hydrogen passivation cap layer comprises Al2O3, TiO2 and SiN x One or more of the above, with a thickness of 5-200nm.
[0018] The present invention also provides a solar cell, the surface of which has the above-mentioned electron selective passivation contact structure, and the surface of the solar cell is selected from the light-receiving surface or the backlight surface of the solar cell.
[0019] The technical solution of the present invention has the following advantages over the prior art:
[0020] The electron selective passivation contact structure of the present invention has excellent surface passivation performance and realizes electron selective transmission. The wide bandgap magnesium oxide layer can avoid the optical parasitic absorption problem caused by the silicon film, and has a high electron concentration and bulk conductivity. The magnesium oxide layer can further optimize its optical and electrical properties by doping. By doping B, Al, H, and Zn elements, the electron concentration and bulk conductivity of the magnesium oxide layer are increased, and its work function is reduced to further induce the silicon conduction band to bend downward, thereby reducing the electron transmission barrier. Reasonable regulation of the doping cycle ratio and thickness of the magnesium oxide layer can obtain low contact resistance. In addition, the hydrogen passivation cap layer can be selectively retained or removed according to the conductivity type and device structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic structural diagram of the electron selective passivation contact structure in Example 1 of the present invention;
[0022] Figure 2 is p in Example 2 of the present invention + Schematic diagram of the structure of n-structure crystalline silicon battery;
[0023] Figure 3 is p in Example 3 of the present invention + Schematic diagram of the structure of n-structure crystalline silicon battery;
[0024] Figure 4 This is a schematic diagram of the structure of a double-sided passivated contact crystalline silicon cell in Example 4 of the present invention;
[0025] Figure 5 This is a schematic diagram of the structure of a perovskite-crystalline silicon tandem battery in Example 5 of the present invention;
[0026] Figure 6 Schematic diagram of the structure of the perovskite-crystalline silicon tandem battery in Example 6 of the present invention.
[0027] Description of reference numerals: 101 - silicon oxide tunneling layer, 102 - magnesium oxide layer, 103 - hydrogen passivation cap layer, 201 - silicon substrate, 202 - p + Emitter, 203-silicon oxide tunneling layer, 204-magnesium oxide layer, 205-aluminum oxide passivation layer, 206-silicon nitride anti-reflection layer, 207-aluminum electrode, 208-aluminum-silver composite electrode, 301-silicon substrate, 302-p + Emitter, 303-silicon oxide tunneling layer, 304-doped magnesium oxide layer, 305-aluminum oxide passivation layer, 306-silicon nitride anti-reflection layer, 307-aluminum electrode, 308-aluminum silver composite electrode, 315-aluminum oxide capping layer, 316-silicon nitride capping layer, 401-silicon substrate, 402-silicon oxide tunneling layer, 403-magnesium oxide layer, 404-first transparent conductive layer, 405-low-temperature silver electrode, 406-intrinsic amorphous silicon layer, 407-boron-doped amorphous silicon layer, 408-second transparent conductive layer, 501-silicon substrate, 502-intrinsic amorphous silicon layer, 503-boron-doped amorphous silicon layer, 504-indium tin oxide, 505-low-temperature silver electrode, 506-silicon oxide tunneling layer, 507-magnesium oxide layer, 508-hole transport layer HTL, 509-perovskite absorption layer, 510-C 60 layer, 511-SnO2 layer, 512-indium zinc oxide, 513-anti-reflection layer, 601-silicon substrate, 602-silicon oxide tunneling layer, 603-boron-doped polysilicon layer, 604-silver-cadmium composite electrode, 605-silicon oxide tunneling layer, 606-magnesium oxide layer, 607-hole transport layer HTL, 608-perovskite absorption layer, 609-C 60 layer, 610-SnO2 layer, 611-indium zinc oxide layer, 612-anti-reflection layer, 613-Ag electrode. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0030] The present invention discloses an electron selective passivation contact structure, which is located on the light receiving surface and / or the backlight surface of a silicon substrate. The electron selective passivation contact structure comprises a silicon oxide tunneling layer, an intrinsic or doped magnesium oxide layer (the magnesium oxide is doped with Al, B, H, Zn, etc. to optimize its work function, conductive properties, etc.), and a hydrogen passivation cap layer, which are stacked in sequence.
[0031] The present invention also discloses a method for preparing an electron selective passivation contact structure, comprising:
[0032] Depositing a silicon oxide tunneling layer, a magnesium oxide layer, and a hydrogen passivation cap layer in sequence on the light-receiving surface and / or the backlight surface of the silicon substrate;
[0033] Among them, magnesium oxide can be further optimized in terms of work function, conductivity, etc. by doping with Al, B, H, Zn, etc.;
[0034] The deposition of the intrinsic or doped magnesium oxide layer is performed by an atomic layer deposition process, and the doping concentration and deposition thickness of the doped magnesium oxide layer are controlled by the number of cycles and the cycle ratio in a super cycle mode.
[0035] The invention also discloses a solar cell, comprising an electron selective passivation contact structure, wherein the electron selective passivation contact structure is located on the light receiving surface or the backlight surface of the solar cell.
[0036] The electron selective passivation contact structure comprises a silicon oxide tunneling layer, a magnesium oxide layer and a hydrogen passivation cap layer which are stacked in sequence.
[0037] The thickness of the magnesium oxide layer is 1 nm to 50 nm.
[0038] In addition, the thickness of the silicon oxide tunneling layer is 0.5 nm to 2 nm. The preparation methods of silicon oxide include but are not limited to dry methods: thermal oxidation, ozone oxidation, etc., and wet methods: nitric acid oxidation.
[0039] Furthermore, the electron selective passivation contact structure further includes a hydrogen passivation capping layer stacked on the intrinsic magnesium oxide layer, including an Al2O3 layer, a TiO2 layer, a SiN x One or more of the layers have a thickness of 10 nm to 200 nm.
[0040] The method for preparing the electron selective passivation contact structure in this embodiment includes:
[0041] A silicon oxide tunneling layer, a magnesium oxide layer, and a hydrogen passivation cap layer are sequentially deposited on the light-receiving surface or the backlight surface of the silicon substrate.
[0042] The deposition of the intrinsic magnesium oxide layer is performed by an atomic layer deposition (ALD) method.
[0043] The magnesium oxide layer can further reduce its work function through doping, thereby optimizing its optical, electrical and other properties.
[0044] The doping elements of the doped magnesium oxide layer include but are not limited to one of Al, B, H, and Zn or a combination of two, and the doping atom concentration is 1% to 20%. The deposition of the doped magnesium oxide layer is performed by an atomic layer deposition (ALD) process, and the doping quality and deposition thickness are controlled by the number of super cycles in the super cycle mode and the cycle ratio in the doping sub-cycle. The super cycle mode is calculated as n*(m:1), where n is the number of super cycles and m:1 is the cycle ratio in each doping sub-cycle. In this embodiment, the control of the doping concentration and deposition thickness can be achieved by controlling the values of n and m.
[0045] When the doped magnesium oxide layer is a boron-doped magnesium oxide layer, the cycle ratio of magnesium oxide to boron oxide in each doping sub-cycle of the super cycle mode is (5-60):1, and the number of super cycles n is 2-50 times;
[0046] In general, the silicon oxide tunneling layer / magnesium oxide layer / hydrogen passivation capping layer structure achieves excellent surface passivation and electron selective transmission performance. The use of a wide-bandgap transparent magnesium oxide layer avoids the optical parasitic absorption problem caused by silicon thin film. The doped magnesium oxide layer is expected to obtain a lower work function, further inducing the silicon energy band to bend downward and reduce the electron transmission barrier. The thickness is reasonably controlled to obtain low contact resistance.
[0047] The intrinsic or doped magnesium oxide layer uses the atomic layer deposition (ALD) equipment that is currently widely used to produce Al2O3 passivation films, and does not have the expensive problem of plasma enhanced chemical vapor deposition (PECVD) systems. The deposition process does not involve the use of dangerous and explosive gases such as B2H6 and PH3. The electron selective passivation contact structure of silicon oxide tunneling layer / magnesium oxide layer / hydrogen passivation cap layer is also expected to overcome the temperature adaptation problem in the preparation of HJT and TOPCon cells, because its optimal passivation corresponding annealing temperature is close to the current aluminum paste sintering temperature. In addition, its scope of use covers both homojunction and heterojunction contact structure batteries, and can even be expanded to perovskite-crystalline silicon stacked solar cells.
[0048] Example 1
[0049] In this embodiment, an intrinsic magnesium oxide layer is taken as an example, which is deposited by an atomic layer deposition process.
[0050] like Figure 1 As shown, the electron selective passivation contact structure in this embodiment includes a silicon oxide tunneling layer 101 and an intrinsic magnesium oxide layer 102 stacked in sequence.
[0051] This embodiment uses an intrinsic magnesium oxide layer with a thickness of 4.5 nm, and uses a layer with a thickness higher than 4.5 nm as a comparison, as shown in Table 1 for details.
[0052] In addition, the tunneling layer 101 is a silicon oxide layer with a thickness of 1.5 nm. The silicon oxide is prepared by ozone oxidation for 15 minutes.
[0053] Furthermore, the electron selective passivation contact structure further includes a hydrogen passivation capping layer 103 stacked on the intrinsic magnesium oxide layer.
[0054] Exemplarily, the hydrogen passivation capping layer is an Al2O3 layer with a thickness of 30 nm.
[0055] The method for preparing the electron selective passivation contact structure in this embodiment includes:
[0056] A tunneling layer and an intrinsic magnesium oxide layer are deposited on the surface of a silicon substrate.
[0057] The deposition of the intrinsic magnesium oxide layer is performed by an atomic layer deposition (ALD) process.
[0058] In this embodiment, the electron selective passivation contact structure based on silicon oxide layer / intrinsic magnesium oxide layer / hydrogen passivation cover layer is similar to TOPCon battery, with silicon oxide layer as passivation layer. The presence, preparation method and quality of silicon oxide layer have a decisive influence on the final passivation effect. The magnesium oxide layer has a high electron concentration and low work function, so it has a selective electron extraction function. Doping the magnesium oxide layer (B, Al, etc.) can further optimize its optical and electrical properties. Analogous to TOPCon battery, hydrogen passivation cover layer (Al2O3, TiO2, SiN x etc.) or other hydrogen injection methods are used to further improve the passivation performance. Removing the hydrogen passivation cap layer after annealing does not make the passivation effect worse. Whether to remove it depends on whether it is applied to a homojunction contact structure or a heterojunction contact structure battery.
[0059] The passivation and electrical performance data of magnesium oxide layers with different thicknesses are shown in the following table:
[0060] Table 1 Passivation and electrical properties data of magnesium oxide layers with different thicknesses
[0061]
[0062] The electron selective passivation contact structure in Table 1 is a silicon oxide layer / intrinsic magnesium oxide layer / Al2O3 structure, and the thickness of the Al2O3 hydrogen passivation cap layer is 30nm. The composite current density J0 is the measured value under the condition of the optimal annealing temperature without removing the Al2O3 cap layer. The experimental results show that after removing Al2O3, the increase of J0 is very small, about 5-20fA / cm 2 In Table 1, when the intrinsic magnesium oxide thickness is 4.5nm, the composite current density J0 is 20.3fA / cm 2 , contact resistance ρ after removing Al2O3 c 80mΩ·cm 2 These indicators make it promising as an electron-selective passivation contact for application in crystalline silicon solar cells and perovskite-crystalline silicon tandem cells.
[0063] Example 2
[0064] Figure 2 The electron selective passivation contact structure is shown in Figure 2. + Schematic diagram of an n-structure crystalline silicon cell, which includes a silicon substrate 201, p + The emitter 202, the aluminum oxide passivation layer 205, the silicon nitride anti-reflection layer 206 and the aluminum electrode 207, and the silicon oxide layer 203, the magnesium oxide layer 204 and the aluminum-silver composite electrode 208 are sequentially deposited on the back of the silicon substrate 201.
[0065] Similar to TOPCon cells, the silicon oxide layer 203 serves as a surface passivation layer, and the low work function magnesium oxide layer 204 can induce the silicon energy band to bend downward, reducing the electron transmission barrier. The thickness of the magnesium oxide layer is reasonably adjusted to obtain low contact resistance. The hydrogen passivation cap layer can be prepared simultaneously when the aluminum oxide passivation layer 205 / silicon nitride anti-reflection layer 206 is prepared at the front end, and the back Al2O3 / SiN is removed on one side after annealing. x , the aluminum-silver composite electrode 208 covering the entire area is used as an electrode and a back reflection structure. In addition, the annealing process can be coupled to the front-end high-temperature sintering process to reduce the process flow.
[0066] Example 3
[0067] Figure 3 The electron selective passivation contact structure is shown in Figure 2. + Schematic diagram of an n-structure crystalline silicon cell, which includes a silicon substrate 301, p + The emitter 302, the aluminum oxide passivation layer 305, the silicon nitride anti-reflection layer 306 and the aluminum electrode 307, and the silicon oxide layer 303, the doped magnesium oxide layer 304, the aluminum oxide capping layer 315, the silicon nitride capping layer 316 and the aluminum-silver composite electrode 308 are sequentially deposited on the back of the silicon substrate 301.
[0068] The deposition of the doped magnesium oxide layer 304 is performed by an atomic layer deposition (ALD) process, and the doping quality and deposition thickness are controlled by the number of super cycles in the super cycle mode and the cycle ratio in the doping sub-cycle. The super cycle mode is calculated as n*(m:1), where n is the number of super cycles and m:1 is the cycle ratio in each doping sub-cycle. In this embodiment, the doping quality and deposition thickness can be controlled by controlling the values of n and m.
[0069] When the doped magnesium oxide layer is a boron-doped magnesium oxide layer, the cycle ratio of magnesium oxide to boron oxide in each doping sub-cycle of the super cycle mode is 12:1, and the number of super cycles n is 10 times.
[0070] The aluminum oxide capping layer 315 and the silicon nitride capping layer 316 in this embodiment are hydrogen-containing capping layers, which together with the front aluminum oxide passivation layer 305 and the silicon nitride anti-reflection layer 306 can be obtained by one-time double-sided deposition using ALD, PECVD and other equipment, and the annealing activation passivation step can be coupled with the high-temperature sintering process.
[0071] The difference from the second embodiment is that the aluminum oxide capping layer 315 and the silicon nitride capping layer 316 on the back side of the silicon substrate 301 are retained in this embodiment, and the rest is the same as the second embodiment.
[0072] Example 4
[0073] Figure 4 The figure shows a schematic diagram of an electron selective passivation contact structure applied to a double-sided passivation contact cell, which includes a silicon substrate 401, a silicon oxide layer 402, a magnesium oxide layer 403, and a first transparent conductive layer 404 deposited in sequence on the front side of the silicon substrate 401, and an intrinsic amorphous silicon layer 406, a boron-doped amorphous silicon layer 407, and a second transparent conductive layer 408 deposited in sequence on the back side of the silicon substrate 401, and low-temperature silver electrodes 405 are formed on both the front and back sides.
[0074] The back side of the battery in this embodiment takes the hole selection end of the HJT battery as an example. In other embodiments, transition metal oxides such as MoO x , VO x Equal hole selection materials for replacement.
[0075] The low work function magnesium oxide layer can induce the silicon energy band to bend downward, reducing the electron transmission barrier. The thickness can be reasonably adjusted to obtain low contact resistance. This battery overcomes the optical parasitic absorption problem of silicon at the front end of the device in the HJT or TOPCon passivation contact structure, and improves the conversion efficiency of the battery.
[0076] Example 5
[0077] Figure 5The schematic diagram of the electron selective passivation contact structure applied to the perovskite-crystalline silicon stacked cell is shown, which includes a silicon substrate 501, an intrinsic amorphous silicon layer 502, a boron-doped amorphous silicon layer 503, an indium tin oxide 504 and a low-temperature silver electrode 505 deposited on the back of the silicon substrate 501 in sequence, and a silicon oxide layer 506, a magnesium oxide layer 507, a perovskite hole transport layer HTL508, a perovskite layer 509, and a C 60 Layer 510 , SnO2 layer 511 , indium zinc oxide layer 512 , anti-reflection layer 513 , and low-temperature silver electrode 505 .
[0078] After removing the hydrogen passivation cap layer, the electron selective passivation contact structure is replaced by the silicon oxide layer / magnesium oxide layer with the a-Si:H(i) / a-Si:H(n) / ITO structure in the current high-efficiency perovskite-crystalline silicon solar cell structure, thereby avoiding the optical parasitic absorption problem caused by amorphous silicon a-Si film, which can make the device J sc Significant improvement.
[0079] Example 6
[0080] Figure 6 The schematic diagram of the electron selective passivation contact structure applied to the perovskite-crystalline silicon stacked cell is shown, which includes a silicon substrate 601, SiO2 deposited on the back of the silicon substrate 601, x layer 602, boron-doped polysilicon layer 603, silver-cadmium composite electrode 604, silicon oxide layer 605, magnesium oxide layer 606, perovskite hole transport layer HTL607, perovskite layer 608, C 60 Layer 609 , SnO 2 layer 610 , indium zinc oxide layer 611 , anti-reflection layer 612 , and Ag electrode 613 .
[0081] After removing the hydrogen passivation capping layer, the electron selective passivation contact structure replaces the SiO2 in the current high-efficiency perovskite-crystalline silicon solar cell structure. x / poly-Si(n + ) structure, thus avoiding the optical parasitic absorption problem caused by polycrystalline silicon poly-Si film, which can make the device J sc Significant improvement.
[0082] Effect evaluation 1
[0083] It should be understood that several specific battery structures are used as examples in the above-mentioned embodiments 2 to 6. In other embodiments, the electron selective passivation contact structure can also be applied to other battery structures. It can be located on the light-receiving side (front) of the battery or on the backlight side (back) of the battery. Examples will not be given one by one here for detailed description.
[0084] It can be seen from the above technical solutions that the present invention has the following beneficial effects:
[0085] The electron selective passivation contact structure of the present invention can simultaneously achieve excellent surface passivation and electron selective transmission. The magnesium oxide layer can avoid the optical parasitic absorption problem caused by the silicon film. The doped magnesium oxide layer is expected to obtain a lower work function, further induce the silicon energy band to bend downward, and reduce the electron transmission barrier. Reasonable control of thickness to obtain low contact resistance;
[0086] In addition, the passivation performance of the electron selective passivation contact structure can be further improved by combining the hydrogen passivation capping layer, and the hydrogen passivation capping layer can be selectively retained or removed according to the conductivity type and device structure.
[0087] When the passivation contact structure is used for the devices described in Embodiments 4 and 5 or other passivation contact structures during the front end, the short-circuit current density J of the device can be significantly increased. sc , about 1mA / cm 2 ~4mA / cm 2 , the absolute photoelectric conversion efficiency can be increased by 1% to 3.5%.
[0088] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0089] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0090] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. An electron selective passivation contact structure, characterized in that: The electron selective passivation contact structure is arranged on the surface of a silicon substrate, and the surface of the silicon substrate is selected from one of a light-receiving surface and a backlight surface of the silicon substrate; the electron selective passivation contact structure comprises a silicon oxide tunneling layer, a magnesium oxide layer and a hydrogen passivation cap layer prepared in sequence.
2. The electron selective passivation contact structure according to claim 1, characterized in that: The thickness of the magnesium oxide layer is 1-50 nm.
3. The electron selective passivation contact structure according to claim 1, characterized in that: The magnesium oxide layer comprises an intrinsic magnesium oxide layer or a doped magnesium oxide layer; the doping elements in the doped magnesium oxide layer comprise one or two of Al, B, H and Zn.
4. The electron selective passivation contact structure according to claim 3, characterized in that: The doping concentration in the doped magnesium oxide layer is 1% to 20% by weight atomic concentration.
5. The electron selective passivation contact structure according to claim 3, characterized in that: The magnesium oxide layer is prepared by an atomic layer deposition method, and the thickness and doping concentration of the doped magnesium oxide layer are controlled by the number of super cycles in an atomic layer deposition super cycle mode and the cycle ratio in a doping sub cycle.
6. The electron selective passivation contact structure according to claim 1, characterized in that: The silicon oxide tunneling layer has a thickness of 0.5-2 nm and is prepared by a method selected from thermal oxidation, ozone oxidation or nitric acid oxidation.
7. The electron selective passivation contact structure according to claim 1, characterized in that: Hydrogen passivation capping layers include Al2O3, TiO2 and SiN x One or more of which has a thickness of 5-200nm.
8. A solar cell, characterized in that: The surface of the solar cell has the electron selective passivation contact structure according to any one of claims 1 to 7, and the surface of the solar cell is selected from the light-receiving surface or the backlight surface of the solar cell.
Citation Information
Patent Citations
Solar cell with double-sided light incident structure
CN112701182A
Electron selective passivation contact structure, solar cell and preparation method
CN114678430A
Electron selective transmission material for photovoltaic device and application of electron selective transmission material
CN115148831A
Tunneling oxide layer passivation contact battery back structure, and preparation method therefor and use thereof
WO2023213025A1
Cited By
Passivation contact composite layer and perovskite-crystalline silicon laminated solar cell
CN119653924A
Electron passivation contact structure, preparation method and solar cell
CN119997671A