Micro-nano-scale multifunctional composite carrier film as well as preparation process and application thereof

By adopting the preparation process of micro-nano-scale multifunctional carrier film in the carrier film, combining the conductive functional layer and the thermal insulation layer, the problems of the carrier film adhesion and surface defects are solved, and the efficient insulation and stability of the battery is achieved, reducing the number of cells cost and complexity.

CN118899447APending Publication Date: 2024-11-05FAR EAST COPPER FOIL (YIBIN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960428.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing support film has poor adhesion between the layers, has surface defects, and is complex in preparation process, high cost and unstable performance, which limits the application and development of multifunctional composite support films.

Method used

The preparation process of micro-nano-level multifunctional carrier films is adopted, including intermediate layer, thermal insulation layer, grafting layer, pre-plating layer and functional layer. Through vacuum evaporation and flexible scraper coating, the conductive function of aluminum, copper or silver is formed. The layer, combined with a coating layer of conductive carbon material, improves adhesion and electrical conductivity.

Benefits of technology

Effectively prevent battery short circuit, isolate the heat of the battery during circulating charging and discharging, improve the peel strength between the film layers and the stability of the battery, reduce costs and improve performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899447A_ABST
    Figure CN118899447A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of films, in particular to a micro-nano-scale multifunctional composite carrier film as well as a preparation process and application thereof. The invention discloses a micro-nano-scale multifunctional carrier film. The micro-nano-scale multifunctional carrier film comprises a middle layer, the heat insulation layers are arranged on the upper layer and the lower layer of the middle layer; the grafting layer is arranged on the heat insulation layer; the pre-plating layer is arranged on the grafting layer; the functional layer is arranged on the pre-plating layer; and the coating layer is arranged on the functional layer. After the micro-nano-scale multifunctional carrier film is applied, short circuit of a battery can be effectively prevented, meanwhile, the heat insulation layer can well isolate heat generated in the cyclic charging and discharging process of the battery, and thermal runaway of the battery is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thin films, and in particular to a micro-nano multifunctional composite carrier thin film and a preparation process and application thereof. Background Art

[0002] Multifunctional composite carrier films are often used as carrier materials for different devices due to their excellent mechanical properties; such carrier films have the characteristics of high structural complexity, strong functionality and a wide range of applications.

[0003] The current carrier film uses a polymer as a substrate, and a metal conductive layer is attached to the upper and lower surfaces of the substrate. This carrier film can be used as a carrier film in multiple fields such as new energy, electronics, optoelectronics, etc., and has low cost and reliable safety performance. However, the adhesion between the layers of this carrier film is poor, and there are many defects on the surface of the film material. Moreover, the traditional preparation process often has certain defects, such as complex process, high cost, low yield, unstable performance, etc., which limits the application and development of multifunctional composite carrier films. Therefore, it is necessary to seek a new preparation process to improve preparation efficiency, reduce cost, stability and performance.

[0004] Therefore, it is necessary to provide a micro-nano multifunctional composite carrier film and its preparation process and application. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present application provides a micro-nano multifunctional composite carrier film and its preparation process and application. The micro-nano multifunctional carrier film can effectively prevent battery short circuit after application. At the same time, the insulation layer can well isolate the heat generated by the battery during the cyclic charging and discharging process to prevent thermal runaway of the battery.

[0006] The technical solution adopted by this application to solve its technical problem is:

[0007] In a first aspect, the present application provides a micro-nano multifunctional carrier film, comprising an intermediate layer;

[0008] Thermal insulation layers, arranged on the upper and lower layers of the middle layer;

[0009] A grafting layer, disposed on the thermal insulation layer;

[0010] A pre-plating layer is disposed on the grafting layer;

[0011] A functional layer is disposed on the pre-plating layer;

[0012] The coating layer is disposed on the functional layer.

[0013] Furthermore, the material of the middle layer is any one of PET (polyethylene terephthalate), PP (polypropylene), PE (polyethylene), PVC (polyvinyl chloride), PI (polyimide), and PC (polycarbonate).

[0014] Furthermore, the material of the thermal insulation layer is any one of silicon oxide, zirconium oxide, titanium oxide, silicon carbide and aluminum oxide.

[0015] Furthermore, the grafting layer is made of any one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), modified styrene-butadiene rubber (SBR), and polyurethane.

[0016] Furthermore, the material of the pre-plating layer is any one of aluminum oxide, copper oxide, and silicon oxide.

[0017] Furthermore, the material of the functional layer is any one of aluminum, copper, gold and silver.

[0018] In a second aspect, the present application provides a method for preparing a micro-nano multifunctional carrier film, comprising the following steps:

[0019] S1. Basement membrane treatment

[0020] Use the base film material as the middle layer, and select the high molecular polymer material as the base film material of the film layer; bake the base film material at 40-60°C for 12-18h to evaporate the water adsorbed on the surface of the base film material;

[0021] Corona treatment of the base film material;

[0022] S2. Deposition of thermal insulation layer on base film material

[0023] The nano thermal insulation layer is deposited on the base film material by vacuum evaporation, and the vacuum degree of deposition is 1*10 -2 -5*10 -2 Pa, the deposition thickness is 10-100nm;

[0024] S3. Applying grafting layer on thermal insulation layer

[0025] The coating process uses a flexible scraper coating, with a coating speed of 5-30m / min, and the coating solid content can be as high as 20% to 40%. The coating liquid viscosity ranges from 400-600MPa·s, the coating amount is in the range of 5 to 20g / m, and the coating thickness is 10nm-100nm;

[0026] S4. Deposition of pre-plating layer on the grafted layer

[0027] The pre-plating layer is deposited on the grafting layer by vacuum evaporation, and the vacuum degree of deposition is 5*10 -3 -1*10-2 Pa, evaporation boat temperature is 950℃-1050℃, coating speed is 20-40m / min, coating thickness is 100-200nm;

[0028] S5. Deposition of functional layer on pre-plating layer

[0029] The functional layer is deposited on the pre-plating layer by evaporation, and the vacuum degree of deposition is 5*10 -3 -1*10 -2 Pa, the film thickness is controlled to about 1μm within five times of evaporation;

[0030] S6. Coating treatment on the functional layer

[0031] The conductive coating slurry is coated on the functional layer with a coating thickness of 10-100 nm. The conductive coating slurry includes the following raw materials in mass fraction:

[0032] 90% conductive carbon material, 5% solvent, 5% binder.

[0033] Furthermore, during the corona treatment, the inter-electrode distance is 2-10 mm, the voltage is 20-40 kV, the temperature is 22° C., the relative humidity is 38%, and the corona treatment time is 10-120 s.

[0034] In a third aspect, the present application provides an application of a micro-nano-scale multifunctional carrier film, wherein the micro-nano-scale multifunctional carrier film is applied to battery preparation.

[0035] The beneficial effects of this application are:

[0036] The micro-nano multifunctional carrier film described in the present application can be applied according to the characteristics of different materials. For example, if the deposited functional layer material is copper or aluminum and is used as a battery current collector, the current collector formed by preparing a micro-nano multifunctional carrier film can effectively prevent the battery from short circuiting. At the same time, the thermal insulation layer can effectively isolate the heat generated by the battery during the cyclic charge and discharge process to prevent thermal runaway of the battery. The grafting layer can enhance the bonding force between the micron functional layer and the substrate and enhance the peeling strength between the film layers, thereby enhancing the stability of the battery during the cyclic charge and discharge process. The coating layer can solve the problems of low conductivity and high internal resistance caused by the use of polymer substrate materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present application is further described below in conjunction with the accompanying drawings and embodiments.

[0038] Figure 1 It is a schematic diagram of the structure of the micro-nano multifunctional composite carrier film described in the present application;

[0039] Figure 2 is a SEM image of the micro-nano multifunctional composite carrier film described in the present application;

[0040] Among them: 1. Intermediate layer; 2. Thermal insulation layer; 3. Grafting layer; 4. Pre-plating layer; 5. Functional layer; 6. Coating layer. DETAILED DESCRIPTION

[0041] The following will clearly and completely describe the concept, specific structure and technical effects of the present application in combination with the embodiments and drawings, so as to fully understand the purpose, characteristics and effects of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of them. Based on the embodiments of the present application, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present application. In addition, all the connection / connection relationships involved in the patent do not simply refer to the direct connection of components, but refer to the formation of a better connection structure by adding or reducing connection accessories according to the specific implementation situation. The various technical features created in this application can be combined interactively without conflicting with each other.

[0042] like Figure 1 As shown, the present application provides a micro-nano multifunctional carrier film, comprising an intermediate layer 1;

[0043] A heat-insulating layer 2, arranged on the upper and lower layers of the intermediate layer 1;

[0044] A grafting layer 3 is arranged on the thermal insulation layer 2;

[0045] A pre-plating layer 4 is arranged on the grafting layer 3;

[0046] A functional layer 5 is disposed on the pre-plating layer 4;

[0047] The coating layer 6 is disposed on the functional layer 5 .

[0048] Specifically, a high molecular polymer material is selected as the middle layer. For example, the material of the middle layer 1 is any one of PET (polyethylene terephthalate), PP (polypropylene), PE (polyethylene), PVC (polyvinyl chloride), PI (polyimide), and PC (polycarbonate).

[0049] Specifically, the material of the heat insulation layer 2 is any one of silicon oxide, zirconium oxide, titanium oxide, and aluminum oxide.

[0050] Specifically, the grafting layer 3 is made of any one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), modified styrene-butadiene rubber (SBR), and polyurethane. The function of the grafting layer is to improve the bonding force between the heat insulation layer and the plating layer.

[0051] Specifically, the material of the pre-plating layer 4 is any one of aluminum oxide, copper oxide, and silicon oxide. The function of the pre-plating layer is to improve the conductivity and prepare for the subsequent thickening of the functional layer.

[0052] Specifically, the material of the functional layer 5 is any one of aluminum, copper, gold and silver.

[0053] Specifically, a coating layer is coated on the functional layer, and the coated material is a conductive carbon material, which may be conductive carbon black, carbon nanotubes, graphene, etc., and the coating thickness is 10-100nm; the conductive coating slurry containing the conductive carbon material includes the following raw materials by mass fraction: 90% of the conductive carbon material, 5% of the solvent polyvinyl alcohol, and 5% of the binder (the binder is any one of polyvinylidene fluoride, water-based polyester resin, water-based acrylic resin, and water-based polyurethane resin). The function of the coating layer is to improve the conductivity of the entire micro-nano multifunctional carrier film.

[0054] The method for preparing the above-mentioned micro-nano multifunctional carrier film comprises the following steps:

[0055] S1. Basement membrane treatment

[0056] Use the base film material as the middle layer, and select the high molecular polymer material as the base film material of the film layer; bake the base film material at 40-60°C for 12-18h to evaporate the water adsorbed on the surface of the base film material;

[0057] The base film material is subjected to corona treatment; specifically, the base film material is subjected to corona treatment, and high-frequency high-voltage electricity is applied to the treatment device to cause corona discharge, thereby generating small and dense purple-blue sparks. Various plasmas generated after air ionization are accelerated under the action of a strong electric field, thereby impacting the base film material in the treatment device. The energy of these plasma particles is generally several to tens of electron volts, which is close to the chemical bond energy of the base film material. Therefore, it can induce the chemical bond breakage of the surface molecules of the base film material and degrade it, thereby increasing the surface roughness. During corona discharge, a large amount of ozone is also generated. Ozone is a strong oxidant that oxidizes the surface molecules of the base film material to produce carbonyl compounds, peroxide compounds, etc. In addition, corona treatment also has the functions of removing oil, water vapor and dust. After the above-mentioned physical and chemical modifications, the wettability and adhesion of the surface of the base film material are improved. During corona treatment, the inter-electrode distance is 2-10mm, the voltage is 20-40kV, the temperature is 22℃, the relative humidity is 38%, and the corona treatment time is 10-120s.

[0058] S2. Deposition of thermal insulation layer on base film material

[0059] The nano thermal insulation layer is deposited on the base film material by vacuum evaporation, and the vacuum degree of deposition is 1*10 -2 -5*10 -2Pa, the deposition thickness is 10-100nm; vacuum evaporation uses crucible evaporation as the base, and the materials used include but are not limited to: silicon oxide, zirconium oxide, titanium oxide, silicon carbide, aluminum oxide, etc.; by depositing a thermal insulation layer, the middle layer is protected from environmental factors during the coating process, such as high temperature burning, water vapor adsorption, mechanical damage, etc.

[0060] S3. Applying grafting layer on thermal insulation layer

[0061] The coating process uses a flexible scraper, with a coating speed of 5-30m / min, and the coating solid content can be as high as 20% to 40%. The coating liquid viscosity ranges from 400-600MPa·s, the coating amount is in the range of 5 to 20g / m, and the coating thickness is 10-100nm.

[0062] S4. Deposition of pre-plating layer on the grafted layer

[0063] A nano pre-plating layer is deposited on the nano grafting layer by vacuum evaporation, and the vacuum degree of deposition is 5*10 -3 -1*10 -2 Pa, high purity aluminum wire (purity is 99.9%) or high purity copper or high purity silicon is used as raw materials for high temperature evaporation coating. When evaporating aluminum wire, the evaporation boat temperature is 750℃-850℃, the concentration of metal vapor is maintained at 50mol / L~60mol / L, the coating speed is 30m / min, and the coating thickness is 100-200nm.

[0064] S5. Deposition of functional layer on pre-plating layer

[0065] The functional layer is deposited on the pre-plating layer by evaporation, and the vacuum degree of deposition is 5*10 -3 -1*10 -2 Pa, and the film thickness was controlled to about 1μm within five evaporation passes.

[0066] S6. Coating treatment on the functional layer

[0067] The conductive coating slurry is coated on the functional layer with a coating thickness of 10-100 nm. The conductive coating slurry includes the following raw materials in mass fraction:

[0068] 90% conductive carbon material, 5% solvent, 5% binder.

[0069] Example 1

[0070] The aluminum composite current collector is prepared by the following preparation method, and the polymer film is a polyethylene terephthalate (PET) film.

[0071] The following steps are involved:

[0072] (1) After the evaporation chamber of the vacuum evaporation equipment is evacuated, a polyethylene terephthalate (PET) film with a thickness of 6 μm that has been pre-treated (corona and baking) is placed in the evaporation chamber as the evaporation substrate. Then, a high-purity aluminum ingot with a purity of 99.9% and a size of φ3*3 mm is placed in a 1*10 -2 Pa vacuum degree was placed in a crucible and evaporated at 1350℃. At the same time, a high-purity oxygen ventilation device was installed next to each crucible. During the evaporation process, the aluminum vapor concentration was maintained at 20mol / L, the oxygen concentration introduced was 30mol / L, the evaporation rate was 20m / min, and a nano-insulation layer was deposited with a thickness of 50nm.

[0073] (2) A nano-grafted layer is coated on the nano-insulation layer, polytetrafluoroethylene (PTFE) is selected as the coating liquid, and a flexible scraper coating process is adopted. The coating speed is controlled at 5-30 m / min, the solid content of the coating is 20%, the viscosity of the coating liquid is 400 MPa·s, and the coating thickness is 100 nm.

[0074] (3) A nano pre-plating layer is deposited on the nano grafted layer by vacuum evaporation, and the vacuum degree of the deposition is 5*10 -3 Pa, high-purity aluminum wire (purity of 99.9%) is used as raw material for high-temperature evaporation coating. The temperature of the evaporation boat for evaporation coating of aluminum wire is 800℃, the evaporation rate is 30m / min, the aluminum vapor concentration is maintained at 50mol / L, and the coating thickness is 100nm.

[0075] (4) Double-sided coating is achieved by a double-chamber winding vacuum coating system. The wire is fed by a wire feeder. The aluminum wire melts and evaporates on the evaporation boat to form an aluminum metal layer on the PET surface. The thickness of the aluminum metal layer on the upper and lower surfaces is 1 μm respectively. The aluminum composite current collector with a thickness of 8 μm is obtained by winding under a tension of 125N. The SEM image of the aluminum composite current collector is shown in FIG. Figure 2 As shown. Figure 2 It can be seen that the surface of the aluminum composite current collector is rough and jagged, and it is calculated that the particle size range of the aluminum metal particles is 120-150nm.

[0076] Comparative Example 1

[0077] The aluminum composite current collector is prepared by the following preparation method, and the polymer film is a polyethylene terephthalate (PET) film. The specific steps are as follows:

[0078] (1) After the evaporation chamber of the vacuum evaporation equipment is evacuated, a polyethylene terephthalate (PET) film with a thickness of 6 μm that has been pre-treated (corona and baking) is placed in the evaporation chamber as the evaporation substrate. Then, a high-purity aluminum ingot with a purity of 99.9% and a size of φ3*3 mm is placed in a 1*10 -2Pa vacuum degree was placed in a crucible and evaporated at 1350℃. At the same time, a high-purity oxygen ventilation device was installed next to each crucible. During the evaporation process, the aluminum vapor concentration was maintained at 20mol / L, the oxygen concentration introduced was 30mol / L, the evaporation rate was 20m / min, and a nano-insulation layer was deposited with a thickness of 50nm.

[0079] (2) A nano pre-plating layer is deposited on the nano thermal insulation layer by vacuum evaporation, and the vacuum degree of the deposition is 8*10 -3 Pa, high-purity aluminum wire (purity of 99.9%) is used as raw material for high-temperature evaporation coating. The temperature of the evaporation boat for evaporating aluminum wire is 800°C, the coating speed is 30m / min, the aluminum vapor concentration is maintained at 50mol / L, and the coating thickness is 100nm.

[0080] (3) Double-sided coating is achieved through a double-chamber winding vacuum coating system. The wire is fed using a wire feeder. The aluminum wire melts and evaporates on an evaporation boat to form an aluminum metal layer on the PET surface. The thickness of the aluminum metal layer on the upper and lower surfaces is 1 μm, respectively. The aluminum composite current collector with a thickness of 8 μm is obtained by winding the coil under a tension of 125 N.

[0081] Comparative Example 2

[0082] The following preparation method is used to prepare the aluminum composite current collector, and the polymer film is a polyethylene terephthalate (PET) film. The specific steps are as follows:

[0083] (1) After the evaporation chamber of the vacuum evaporation equipment is evacuated, a polyethylene terephthalate (PET) film with a thickness of 6 μm that has been pre-treated (corona and baking) is placed in the evaporation chamber as the evaporation substrate. Then, a high-purity aluminum ingot with a purity of 99.9% and a size of φ3*3 mm is placed in a 1*10 -2 Pa vacuum degree was placed in a crucible and evaporated at 1350℃. At the same time, a high-purity oxygen ventilation device was installed next to each crucible. During the evaporation process, the aluminum vapor concentration was maintained at 20mol / L, the oxygen concentration introduced was 30mol / L, the evaporation rate was 20m / min, and a nano-insulation layer was deposited with a thickness of 50nm.

[0084] (2) A nano-grafted layer is coated on the nano-insulation layer, polytetrafluoroethylene (PTFE) is selected as the coating liquid, and a flexible scraper coating process is adopted. The coating speed is controlled at 5-30 m / min, the solid content of the coating is 20%, the viscosity of the coating liquid is 400 MPa·s, and the coating thickness is 100 nm.

[0085] (3) Double-sided coating is achieved through a double-chamber winding vacuum coating system. The wire is fed using a wire feeder. The aluminum wire melts and evaporates on an evaporation boat to form an aluminum metal layer on the PET surface. The thickness of the aluminum metal layer on the upper and lower surfaces is 1 μm, respectively. The aluminum composite current collector with a thickness of 8 μm is obtained by winding the coil under a tension of 125 N.

[0086] The aluminum composite current collectors prepared in Example 1, Comparative Examples 1 and 2 were subjected to the following performance tests:

[0087] For tensile strength, elongation, and surface roughness performance tests, please refer to the national standard GB / T5230-2020 "Electrolytic Copper Foil for Printed Circuit Boards";

[0088] For the surface square resistance performance test, please refer to the national standard GB / T 17473.3-2008 "Test method for precious metal paste for microelectronics technology - square resistance determination";

[0089] For surface tension performance test, please refer to the national standard GB / T 22638.4-2016 "Aluminum foil test method Part 4: Determination of surface wetting tension";

[0090] For adhesion performance test, please refer to the national standard GB / T 2792-2014 "Test method for peel strength of adhesive tape"; the above test results are summarized in Table 1.

[0091] Table 1

[0092] Test indicators Example 1 Comparative Example 1 Comparative Example 2 Tensile strength MPa 180 172 170 Elongation % 113 95 104 Surface resistance mΩ / □ 34 36 39 Surface roughness μm 0.124 0.346 0.135 Surface tension mN / m 42 38 40 Adhesion N / 15mm 2 1.6 1.9

[0093] As can be seen from Table 1, the aluminum composite current collector of Example 1 has a longitudinal tensile strength of 180 MPa, an elongation of 113%, a surface square resistance of 34 mΩ / □, a surface roughness of 0.124 μm, a surface tension of 42 mN / m, and an adhesion of 2 N / 15 mm.

[0094] As can be seen from Table 1, the aluminum composite current collector of Comparative Example 1 has a longitudinal tensile strength of 172 MPa, an elongation of 95%, a surface square resistance of 36 mΩ / □, a surface roughness of 0.346 μm, a surface tension of 38 mN / m, and an adhesion of 1.6 N / 15 mm.

[0095] As can be seen from Table 1, the aluminum composite current collector of Example 1 has a longitudinal tensile strength of 170 MPa, an elongation of 104%, a surface square resistance of 39 mΩ / □, a surface roughness of 0.135 μm, a surface tension of 40 mN / m, and an adhesion of 1.9 N / 15 mm.

[0096] Battery Assembly:

[0097] Positive electrode: composed of the aluminum composite current collector prepared as described above (Example 1, Comparative Example 1, Comparative Example 2) and a lithium iron phosphate active material layer coated on the aluminum composite current collector;

[0098] Negative electrode: graphite;

[0099] Electrolyte: liquid electrolyte with lithium hexafluorophosphate as solute;

[0100] Diaphragm: Polyethylene (PE) microporous diaphragm;

[0101] The prepared positive electrode sheet, negative electrode sheet and separator are wound into an electrode group, and then the lithium-ion battery is made by aluminum-plastic packaging, liquid injection, standing, pressurization and degassing.

[0102] The performance of the carrier film was tested using a lithium-ion battery test system in accordance with the standard GB / T 31484-2015 "Requirements and test methods for cycle life of power batteries for electric vehicles". The specific test conditions included: 1000 cycles at 25°C, 1C charge and discharge rate, 100% discharge depth and 2 atmospheres. The test results are shown in Table 2.

[0103] Table 2

[0104] Test indicators Example 1 Comparative Example 1 Comparative Example 2 Internal resistance mΩ 15 27 30 Capacity retention rate % 90 87 89

[0105] As can be seen from Table 2, in Example 1, the aluminum composite current collector is tested by a lithium-ion battery testing system, and the discharge capacity is ≥ 90% of the initial capacity and the resistance is 15 mΩ.

[0106] The aluminum composite current collector of Comparative Example 1 has a discharge capacity ≥ 87% of the initial capacity and a resistance of 27 mΩ;

[0107] The aluminum composite current collector of Comparative Example 2 has a discharge capacity ≥ 89% of the initial capacity and a resistance of 30 mΩ.

[0108] The above is a specific description of the preferred implementation of the present application, but the invention of the present application is not limited to the described embodiments. Technical personnel familiar with the field can also make various equivalent modifications or substitutions without violating the spirit of the present application. These equivalent modifications or substitutions are all included in the scope defined by the claims of the present application.

Claims

1. A micro-nano multifunctional carrier film, characterized in that: comprising an intermediate layer (1); A heat-insulating layer (2) is arranged on the upper and lower layers of the intermediate layer (1); A grafting layer (3) is arranged on the thermal insulation layer (2); A pre-plating layer (4) is arranged on the grafting layer (3); A functional layer (5) is disposed on the pre-plating layer (4); The coating layer (6) is arranged on the functional layer (5).

2. The multifunctional carrier film according to claim 1, characterized in that: The material of the intermediate layer (1) is any one of PET (polyethylene terephthalate), PP (polypropylene), PE (polyethylene), PVC (polyvinyl chloride), PI (polyimide), and PC (polycarbonate).

3. The multifunctional carrier film according to claim 1, characterized in that: The material of the heat insulation layer (2) is any one of silicon oxide, zirconium oxide, titanium oxide and aluminum oxide.

4. The multifunctional carrier film according to claim 1, characterized in that: The material of the grafting layer (3) is any one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), modified styrene-butadiene rubber (SBR), and polyurethane.

5. The multifunctional carrier film according to claim 1, characterized in that: The material of the pre-plating layer (4) is any one of aluminum oxide, copper oxide and silicon oxide.

6. The multifunctional carrier film according to claim 1, characterized in that: The material of the functional layer (5) is any one of aluminum, copper, gold and silver.

7. A method for preparing a micro-nano multifunctional carrier film according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Basement membrane treatment Use the base film material as the middle layer, and select the high molecular polymer material as the base film material of the film layer; bake the base film material at 40-60°C for 12-18h to evaporate the water adsorbed on the surface of the base film material; Corona treatment of the base film material; S2. Deposition of thermal insulation layer on base film material The nano thermal insulation layer is deposited on the base film material by vacuum evaporation, and the vacuum degree of deposition is 1*10 -2 -5*10 -2 Pa, the deposition thickness is 10-100nm; S3. Deposition of grafted layer on thermal insulation layer The coating process uses a flexible scraper, with a coating speed of 5-30m / min, and the coating solid content can be as high as 20% to 40%. The coating liquid viscosity ranges from 400-600MPa·s, the coating amount is in the range of 5 to 20g / m, and the coating thickness is 10-100nm; S4. Deposition of pre-plating layer on the grafted layer The pre-plating layer is deposited on the grafting layer by vacuum evaporation, and the vacuum degree of deposition is 5*10 -3 -1*10 -2 Pa, evaporation boat temperature is 950℃-1050℃, coating speed is 20-40m / min, coating thickness is 100-200nm; S5. Deposition of functional layer on pre-plating layer The functional layer is deposited on the pre-plating layer by evaporation. The vacuum degree during the evaporation process is 5*10 -3 -1*10 -2 Pa; S6. Coating treatment on the functional layer The conductive coating slurry is coated on the functional layer with a coating thickness of 10-100 nm. The conductive coating slurry includes the following raw materials in mass fraction: 90% conductive carbon material, 5% solvent, 5% binder.

8. The preparation method according to claim 7, characterized in that: In step S1, during the corona treatment, the inter-electrode distance is 2-10 mm, the voltage is 20-40 kV, the temperature is 22° C., the relative humidity is 38%, and the corona treatment time is 10-120 s.

9. An application of a micro-nano multifunctional carrier film, characterized in that: The micro-nano multifunctional carrier film described in any one of claims 1 to 6 or the micro-nano multifunctional carrier film prepared by the preparation method described in any one of claims 7 to 8 is applied to battery preparation.