Platinum-cobalt alloy catalyst and plasma treatment method and application thereof
By treating platinum-cobalt alloy catalysts with cold plasma, the problems of easy agglomeration and carbon corrosion of platinum-cobalt catalysts in fuel cells are solved, significantly improving the activity and stability of the catalysts, enhancing fuel cell performance, and making them suitable for large-scale production.
Patent Information
- Application Number
- CN202410926154.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Existing platinum-cobalt catalysts are prone to agglomeration and carbon corrosion in fuel cells, leading to reduced activity. Existing plasma treatment methods are characterized by high temperatures and unstable performance.
Platinum-cobalt alloy catalysts were treated with cold plasma. By selecting appropriate plasma type and atmosphere, controlling the low-temperature treatment and curing steps, and optimizing treatment parameters, the activity and stability of the catalysts were improved.
It significantly improves the activity and stability of platinum-cobalt alloy catalysts, enhances fuel cell performance, increases half-cell durability by more than 40%, and increases current density by 18.7%, making it suitable for large-scale production.
Smart Images

Figure CN118899455A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a platinum-cobalt alloy catalyst and a plasma treatment method and application thereof. Background Art
[0002] As energy and environmental problems become increasingly serious, people's demand for clean energy is becoming more and more urgent. Fuel cells, as an efficient and clean energy conversion technology, have received widespread attention. In fuel cells, catalysts play a vital role, among which platinum-cobalt catalysts have attracted much attention due to their high activity and stability. However, platinum-cobalt catalysts are prone to agglomeration and carbon corrosion during long-term operation, resulting in reduced activity, which in turn affects the performance of fuel cells. In order to solve this problem, researchers have proposed many methods, such as changing the preparation method, optimizing the platinum-cobalt ratio, adding additives, etc., but these methods often have certain limitations and cannot fundamentally solve the problem.
[0003] As an emerging material surface modification technology, plasma treatment technology has the advantages of simple operation, strong controllability, and good treatment effect. It is widely used in materials science, biomedicine and other fields. In recent years, researchers have begun to try to use plasma treatment technology to improve the performance of platinum-cobalt catalysts and have achieved certain results. However, existing plasma treatment methods often have some problems, such as high temperature during the treatment process and unstable treatment effect. Therefore, it is necessary to study a new plasma treatment method to further improve the performance of platinum-cobalt catalysts, thereby improving the overall performance of fuel cells. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a platinum-cobalt alloy catalyst and a plasma treatment method and application thereof. The treatment method of the present invention selects a suitable plasma type and treatment atmosphere, is carried out at a relatively low temperature, controls the treatment temperature and time to ensure the treatment effect, and subsequently stabilizes the plasma effect through a curing treatment, which can effectively improve the activity and stability of the platinum-cobalt alloy catalyst, thereby improving the overall performance of the fuel cell.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:
[0006] In a first aspect, an embodiment of the present invention provides a plasma treatment method for a platinum-cobalt alloy catalyst, comprising the following steps:
[0007] (1) Select the appropriate plasma type and processing atmosphere;
[0008] (2) evacuating the interior of the plasma surface treatment instrument to 10-100 Pa, introducing a treatment atmosphere with a flow rate of 10-600 sccm, and subjecting the platinum-cobalt alloy catalyst to plasma treatment for 3-60 min at a power of 50-800 W and a treatment temperature of 10-80° C.;
[0009] (3) Curing the platinum-cobalt alloy catalyst after the plasma treatment in step (2) at 50-120° C. for 10-1440 min in a nitrogen atmosphere.
[0010] Furthermore, the plasma used to treat the platinum-cobalt alloy catalyst in step (2) is cold plasma, and the temperature of the plasma is lower than 50°C.
[0011] Furthermore, the plasma used to treat the platinum-cobalt alloy catalyst in step (2) includes one or more of radio frequency plasma, microwave plasma, corona discharge plasma and glow discharge plasma.
[0012] Furthermore, the processing atmosphere in step (1) includes one or more of argon, hydrogen, nitrogen, oxygen and air.
[0013] Furthermore, in step (2), the power of the plasma treatment is 100-500 W, the treatment time is 5-30 min, and the treatment temperature is 10-50° C.
[0014] In a second aspect, an embodiment of the present invention provides a platinum-cobalt alloy catalyst, which is prepared by the plasma treatment method described in the first aspect.
[0015] In a third aspect, an embodiment of the present invention provides an application of the platinum-cobalt alloy catalyst described in the second aspect in a fuel cell.
[0016] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0017] 1. The method of the present invention selects a suitable plasma type and treatment atmosphere. The plasma adopts cold plasma (also called non-thermal plasma), in which the temperature of electrons is much higher than that of ions and neutral particles. In this plasma, the average kinetic energy of electrons is high, sufficient to maintain the ionization state of the plasma, but overall, the temperature of the plasma is relatively low, usually close to room temperature or lower, and the temperature of the selected plasma is lower than 50°C; it is carried out at a lower temperature, and the treatment effect is ensured by optimizing the treatment temperature and time, and the performance effect after plasma treatment is increased by subsequent curing treatment, and the continuous improvement effect is maintained.
[0018] 2. The present invention performs surface modification on the platinum-cobalt alloy catalyst through plasma treatment, which can increase the number of active sites of the catalyst and improve its electronic structure, thereby significantly improving the activity and stability of the platinum-cobalt alloy catalyst, and the durability of the half-cell at 30,000 cycles is increased by more than 40%.
[0019] 3. The present invention achieves effective regulation of the surface properties of the catalyst by adjusting plasma treatment parameters, such as power, treatment time, etc., thereby improving the performance of the catalyst.
[0020] 4. The present invention applies the plasma-treated platinum-cobalt alloy catalyst to the preparation of fuel cell electrodes, improves the dispersion performance of the catalyst, and verifies the effect of improving the performance of large-size single cells of fuel cells through performance tests. The current density at a voltage of 0.65V reaches 2A / cm 2 Above, the performance is improved by 18.7%.
[0021] 5. The method of the present invention belongs to direct surface treatment, does not require secondary separation, is simple and easy to operate, has strong operability, is suitable for large-scale production, and does not require changing the large-scale preparation process of the platinum-cobalt alloy catalyst before plasma treatment.
[0022] 6. The platinum-cobalt alloy catalyst prepared by this method has low cost and high fuel cell performance, which is conducive to promoting the commercial application of fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the process of plasma treatment of the platinum-cobalt alloy catalyst of the present invention.
[0024] Figure 2 It is a comparison chart of polarization curves of the platinum-cobalt alloy catalysts obtained in Example 4 of the present invention and Comparative Example 1 when applied to a single cell for testing.
[0025] Single cell area 320cm 2 The stoichiometric ratio of anode to cathode is 1.5:2.0, the anode dew point is set to 60°C, the cathode dew point is 60°C, the anode stack pressure is 1.6 bar, the cathode stack pressure is 1.5 bar, and the battery test temperature is 75°C. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0027] Example 1
[0028] A plasma treatment method for a platinum-cobalt alloy catalyst comprises the following steps:
[0029] (1) Using radio frequency plasma and argon atmosphere, the equipment used is Nan Technology Plasma Surface Treatment Instrument NE-PE02;
[0030] (2) The plasma surface treatment instrument was evacuated to 100 Pa, and a treatment atmosphere with a flow rate of 600 sccm was introduced. The platinum-cobalt alloy catalyst (prepared by the method described in the invention patent: ZL202110806266.5) was treated at a power of 800 W for 3 min, and the treatment temperature was 15±5°C; since the temperature will fluctuate to a certain extent during the treatment process and may rise, it is necessary to suppress the temperature rise, so the temperature is a range;
[0031] (3) Curing the platinum-cobalt alloy catalyst treated with plasma in step (2) at 120° C. for 10 min in a nitrogen atmosphere.
[0032] (4) Single cell preparation: accurately weigh 666 mg of the platinum-cobalt alloy carbon catalyst prepared in step (3); measure 128 mL of pure water, 128 mL of isopropanol and 12.8 mL of perfluorosulfonic acid resin solution, add them to the catalyst, and fully disperse them for 40 minutes to form a catalyst ink, which is evenly coated on the cut proton exchange membrane, which is recorded as the cathode; weigh the platinum-carbon catalyst in the same way, and coat it on the other side of the above proton exchange membrane, which is recorded as the anode, to form a membrane electrode CCM; use SGL 28BC model GDL, use a homemade assembly fixture, put the first GDL, CCM, and the second GDL in turn, tighten the fixing nut under a fixed assembly force of 1 MPa to complete the clamping, connect the gas pipeline, and after passing the air tightness test, conduct a single cell test.
[0033] (5) Single cell test conditions: Single cell area 320cm 2 The stoichiometric ratio of anode to cathode is 1.5:2.0, the anode dew point is set to 60°C, the cathode dew point is 60°C, the anode stack pressure is 1.6 bar, the cathode stack pressure is 1.5 bar, and the battery test temperature is 75°C.
[0034] Example 2
[0035] A plasma treatment method for a platinum-cobalt alloy catalyst, which differs from Example 1 in that step (1) uses a glow discharge plasma and a hydrogen treatment atmosphere, and other conditions are the same as those in Example 1; the preparation and testing conditions of a single cell of the platinum-cobalt alloy catalyst treated by this embodiment are the same as those in Example 1.
[0036] Example 3
[0037] A plasma treatment method for a platinum-cobalt alloy catalyst, which differs from Example 2 in that step (3) is cured at 50° C. for 1440 min under a nitrogen atmosphere, and other conditions are the same as those in Example 2; the preparation and testing conditions of a single cell using the platinum-cobalt alloy catalyst treated in this example are the same as those in Example 2.
[0038] Example 4
[0039] A plasma treatment method for a platinum-cobalt alloy catalyst is disclosed. The difference from Example 1 is that step (1) uses glow discharge plasma and nitrogen treatment atmosphere, and step (2) evacuates to 10 Pa, introduces a treatment atmosphere with a flow rate of 50 sccm, and treats for 60 minutes at a power of 100 W. Other conditions are the same as those in Example 1. The preparation and testing conditions of a single cell of the platinum-cobalt alloy catalyst treated by this example are the same as those in Example 1.
[0040] Example 5
[0041] A plasma treatment method for a platinum-cobalt alloy catalyst comprises the following steps:
[0042] (1) Using corona discharge plasma and argon atmosphere, the equipment used is Nan Technology Vacuum Plasma Surface Treatment Machine NE-PE180;
[0043] (2) The vacuum plasma surface treatment machine was evacuated to 100 Pa, and a treatment atmosphere with a flow rate of 600 sccm was introduced. The platinum-cobalt alloy catalyst (TEC36E52 platinum-cobalt catalyst product of Tanaka Precious Metals Co., Ltd., Japan) was treated at a power of 800 W for 60 min. The treatment temperature was 50±5°C. Since the temperature would fluctuate to a certain extent during the treatment process and might rise, it was necessary to suppress the temperature rise, so the temperature was within a range;
[0044] (3) Curing the platinum-cobalt alloy catalyst treated with plasma in step (2) at 120° C. for 10 min in a nitrogen atmosphere.
[0045] (4) Single cell preparation: accurately weigh 666 mg of the platinum-cobalt alloy carbon catalyst prepared in step (3); measure 128 mL of pure water, 128 mL of isopropanol and 12.8 mL of perfluorosulfonic acid resin solution, add them to the catalyst, and fully disperse them for 40 minutes to form a catalyst ink, which is evenly coated on the cut proton exchange membrane, which is recorded as the cathode; weigh the platinum-carbon catalyst in the same way, and coat it on the other side of the above proton exchange membrane, which is recorded as the anode, to form a membrane electrode CCM; use SGL 28BC model GDL, use a homemade assembly fixture, put the first GDL, CCM, and the second GDL in turn, tighten the fixing nut under a fixed assembly force of 1 MPa to complete the clamping, connect the gas pipeline, and after passing the air tightness test, conduct a single cell test.
[0046] (5) Single cell test conditions: Single cell area 320cm 2 The stoichiometric ratio of anode to cathode is 1.5:2.0, the anode dew point is set to 60°C, the cathode dew point is 60°C, the anode stack pressure is 1.6 bar, the cathode stack pressure is 1.5 bar, and the battery test temperature is 75°C.
[0047] Comparative Example 1
[0048] The difference from Example 4 is that no plasma treatment is performed, and the platinum-cobalt alloy catalyst prepared by the method described in Invention Patent ZL202110806266.5 in Example 4 is directly used to produce single cells, and the production and testing conditions are the same as those in Example 4.
[0049] Comparative Example 2
[0050] The difference from Example 2 is that the curing step (3) is not performed, and the other conditions are the same as those in Example 2; the preparation and testing conditions of the single cell using the platinum-cobalt alloy catalyst treated in this example are the same as those in Example 2.
[0051] Table 1 Electrochemical performance of platinum-cobalt catalysts in Examples 1-5 and Comparative Examples 1-2 tested under a three-electrode system
[0052]
[0053] *Electrochemical performance test conditions of the present invention: three-electrode system, electrolyte is 0.1M HClO4 saturated with oxygen; rotation speed: 1600rpm; scanning speed: 10mVs -1 ; The 30,000 endurance attenuation condition is to conduct a square wave test, at 0.6V and 0.95V vs.RHE, the two test voltages stay for 3s, and a test cycle is completed in 6s, scanning 10,000, 20,000, and 30,000 circles, the test scan rate is 20mV / s for CV and LSV, and the mass activity is calculated until 30,000 circles, and the constant temperature water bath is 25℃.
[0054] It can be seen from Table 1 that the mass activities of Examples 1-4 are all higher than those of Comparative Example 1, indicating that plasma treatment can improve the mass activity of platinum-cobalt alloy catalysts. The higher the mass activity, the better the corresponding oxidant performance, and the better the performance of the fuel cell monomer used. Compared with Comparative Example 2, Example 1 shows that the mass activity of the plasma-treated platinum-cobalt alloy catalyst and the durability of the platinum particles can be improved through the curing step.
[0055] Figure 1It is a schematic flow chart of plasma treatment of the platinum-cobalt alloy catalyst of the present invention. The catalyst obtained after plasma treatment and curing treatment is tested for catalytic performance. If the performance meets the requirements, a single cell test is made. It is found that the treatment method of the present invention can improve the performance of the fuel cell single cell; the catalyst whose catalytic performance does not meet the requirements is reprocessed.
[0056] from Figure 2 It can be seen that the current density of the platinum-cobalt alloy catalyst treated in Example 4 at the same voltage is higher than that of Comparative Example 1, indicating that the performance of the catalyst treated by the plasma treatment method of the present invention is better.
[0057] from Figure 2 It can be seen that the current density of the fuel cell monomer cell made by using the platinum-cobalt alloy catalyst treated by plasma of the present invention reaches 2A / cm at a voltage of 0.65V. 2 The performance has been improved by 18.7%, which is at the leading level in China.
[0058] Plasma treatment has advantages in improving the performance of platinum-cobalt catalysts. Plasma treatment can increase the open circuit voltage and maximum power density of the catalyst, while improving the stability of the catalyst. The reason for the performance improvement is most likely because plasma treatment can improve the surface properties of the catalyst, increase the number of active sites, optimize the electronic structure of the catalyst, etc., thereby improving the performance of the catalyst. Further application in fuel cell monomers can improve the actual power generation performance.
[0059] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A plasma treatment method for a platinum-cobalt alloy catalyst, characterized in that: The following steps are involved: (1) Select the appropriate plasma type and processing atmosphere; (2) The inside of the plasma surface treatment instrument is evacuated to 10-100 Pa, a treatment atmosphere with a flow rate of 10-600 sccm is introduced, and the platinum-cobalt alloy catalyst is plasma treated for 3-60 minutes at a power of 50-800 W and a treatment temperature of 10-80° C.; (3) Curing the platinum-cobalt alloy catalyst after the plasma treatment in step (2) at 50-120° C. for 10-1440 min in a nitrogen atmosphere.
2. The plasma treatment method of the platinum-cobalt alloy catalyst according to claim 1, characterized in that: The plasma used to treat the platinum-cobalt alloy catalyst in step (2) is cold plasma, and the temperature of the plasma is lower than 50°C.
3. The plasma treatment method of the platinum-cobalt alloy catalyst according to claim 1, characterized in that: The plasma used to treat the platinum-cobalt alloy catalyst in step (2) includes one or more of radio frequency plasma, microwave plasma, corona discharge plasma and glow discharge plasma.
4. The plasma treatment method of the platinum-cobalt alloy catalyst according to claim 1, characterized in that: The processing atmosphere in step (1) includes one or more of argon, hydrogen, nitrogen, oxygen and air.
5. The plasma treatment method of the platinum-cobalt alloy catalyst according to claim 1, characterized in that: In step (2), the power of the plasma treatment is 100-500 W, the treatment time is 5-30 min, and the treatment temperature is 10-50° C.
6. A platinum-cobalt alloy catalyst, characterized in that: The product is prepared by treating with the plasma method according to any one of claims 1 to 5.
7. Use of the platinum-cobalt alloy catalyst according to claim 6 in a fuel cell.
Citation Information
Cited By
A plasma synthesis method for rapidly constructing multi-level micro-nanostructured perovskite catalysts
CN119771512A