Polymer electrolyte, secondary battery, and electric device
By designing polymer electrolytes containing cyano, ester and sulfonic acid monomers copolymerized, the problems of low energy density of lithium-ion batteries and safety hazards in liquid batteries are solved, and high energy density and long-term cycle stability are achieved. It is suitable for Matching of lithium metal and lithium-rich manganese-based positive electrode.
Patent Information
- Application Number
- CN202411230196.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-05
AI Technical Summary
The existing lithium-ion batteries have low energy density, and the safety risks of liquid batteries. The interface performance between the inorganic electrolyte and the electrode limits its practical application and is incompatible with the current preparation process.
By designing polymer electrolytes, including polymer substrates and copolymers, copolymers are copolymerized by cyano, ester and sulfonic acid monomers, providing mechanical strength and high reduction resistance to form a stable interface with lithium metal anode and Lithium-rich manganese-based positive electrode matching improves the energy density and cycle stability of the battery.
Achieve high energy density (500Wh/kg) and long-term cycle stability, improve the mechanical and dynamic performance of the battery, and is suitable for the matching of lithium metal and lithium-rich manganese-based positive electrodes, solving the low energy density and liquid state of lithium-ion batteries. Battery safety hazards.
Smart Images

Figure BDA0005027284860000101 
Figure BDA0005027284860000111
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular, to polymer electrolytes, secondary batteries and electrical devices. Background Art
[0002] In the field of new energy, the performance of batteries is becoming increasingly important. Compared with lithium-ion batteries (LIBs), lithium metal batteries (LMBs) based on liquid electrolytes have higher energy density, but the internal short circuit caused by lithium dendrite growth poses a serious safety hazard; LMBs based on solid electrolytes have high energy density and high safety, but have problems such as low ionic conductivity and poor interface contact. Gel polymer electrolytes have attracted widespread attention due to their improved safety, reduced interface impedance between solid electrolytes and electrodes, and compatibility with the "roll-to-roll" LMBs manufacturing process. At the same time, lithium-rich manganese-based cathodes (LRMO) have the advantages of high capacity, high voltage and low cost, and are considered to have great potential to match lithium metal to prepare ultra-high energy density batteries. However, the poor interface performance between LRMO and electrolytes hinders their practical application, so it is necessary to develop new polymer electrolytes.
[0003] It can be seen that the existing technology has the following disadvantages: the energy density of lithium-ion batteries is low, and lithium metal and lithium-rich manganese-based positive electrodes need to be matched. Then there are safety hazards in liquid batteries. The interface performance between inorganic electrolytes and electrodes limits their practical application, and they are incompatible with the current preparation process. Therefore, it is urgent to develop corresponding polymer electrolytes. Summary of the invention
[0004] This application achieves simultaneous matching of lithium metal and lithium-rich manganese-based batteries through the structural design of the polymer electrolyte, thereby achieving high energy density of the battery.
[0005] Some embodiments of the present application provide a polymer electrolyte, including: a polymer substrate; and a copolymer, wherein the polymer substrate includes a supporting material, and the copolymer contains a cyano group, an ester group, and a sulfonic acid group. In the present application, the polymer substrate (A) provides mechanical strength as a supporting material, and the function of the copolymer (B) is to form a stable interface between the positive and negative electrodes. As can be seen from the above, the copolymer (B) is copolymerized by three types of monomers, which contain cyano groups, ester groups, and sulfonic acid groups, respectively, which are polar groups, can improve the mechanical properties of the electrolyte, and have high reduction resistance and oxidation resistance, can form a stable SEI film (solid electrolyte interface film) with the negative electrode, and form a stable CEI (cathode electrolyte interface film) with the positive electrode, can simultaneously match the lithium metal negative electrode and the lithium-rich manganese-based positive electrode, so that the prepared secondary battery has a high energy density and can be cycled for a long time.
[0006] In some embodiments, the mass ratio of the polymer substrate to the copolymer is in the range of 10:90-90:10, and optionally the mass ratio is 30:70. Within this range, the polymer substrate (A) can provide sufficient mechanical properties, and the copolymer (B) is stable with both the positive and negative electrode interfaces and can provide additional dynamics, which is beneficial to the performance of capacity.
[0007] In some embodiments, the copolymer is copolymerized by acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC). The molar ratio of the monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) is 5-25:50-90:5-25. Optionally, the molar ratio of the monomers of acrylonitrile (AN) and vinylene carbonate (VC) is equal. Optionally, the molar ratio of the monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) is 20:60:20. In the present application, acrylonitrile AN has polar functional groups and has high-voltage stability; vinylene carbonate (VC) is stable with lithium metal and can form a stable SEI; lithium p-styrene sulfonate (LiSS) has an additional source of lithium ions, which can provide additional kinetics and further improve the rate performance of the battery.
[0008] In some embodiments, the polymer substrate is selected from any one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), PVDF-HFP-PTFE (fluororubber), polyimide (PI), and polymethyl methacrylate (PMMA).
[0009] Some other embodiments of the present application provide a secondary battery, characterized in that it includes a positive electrode plate, a negative electrode plate and an electrolyte layer, wherein the electrolyte layer includes the above-mentioned polymer electrolyte.
[0010] Still other embodiments of the present application provide an electrical device, characterized in that it includes the above-mentioned secondary battery.
[0011] Through the structural design of the polymer electrolyte, the use of different polymer substrate support materials, and copolymers formed by copolymerization of different monomers, the composition and proportion can be adjusted to match lithium metal and LRMO, achieving an energy density of 500Wh / kg and 500 cycles of long-term stable circulation. DETAILED DESCRIPTION
[0012] The present application is designed by the structure of polymer electrolyte, so that it contains two polymers, specifically, including polymer substrate (A) and copolymer (B), polymer substrate (A) includes supporting material, and copolymer (B) contains cyano group, ester group and sulfonic acid group. In the present application, polymer substrate (A) provides mechanical strength as supporting material, and the role of copolymer (B) is to form a stable interface with positive and negative electrodes. As can be seen from the above, copolymer (B) is copolymerized by three types of monomers, containing cyano group, ester group and sulfonic acid group respectively, which are polar groups, can improve the mechanical properties of electrolyte, and have high reduction resistance and oxidation resistance, can form a stable SEI film (solid electrolyte interface film) with the negative electrode, and form a stable CEI (cathode electrolyte interface film) with the positive electrode, can match lithium metal negative electrode and lithium-rich manganese-based positive electrode at the same time, can make the prepared secondary battery have high energy density, reach 500Wh / kg, and can be circulated for a long time.
[0013] In some embodiments, the mass ratio of the polymer substrate (A) to the copolymer (B) is in the range of 10:90-90:10, and optionally 30:70. Within this range, the polymer substrate (A) can provide sufficient mechanical properties, and the copolymer (B) is stable with both the positive and negative electrode interfaces and can provide additional dynamics, which is beneficial to the performance of capacity.
[0014] In some embodiments, the polymer substrate (A) is a commercially available polymer, including but not limited to fluorine-containing polymers such as polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), PVDF-HFP-PTFE (fluororubber), and fluorine-free polymers such as polyimide (PI) and polymethyl methacrylate (PMMA).
[0015] In some embodiments, the copolymer is copolymerized by acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC), wherein the polymerization method may be free radical polymerization, including simple free radical polymerization, atom transfer radical polymerization, reversible addition-fragmentation chain transfer polymerization, etc. In the present application, acrylonitrile AN has polar functional groups and has high-voltage stability; vinylene carbonate (VC) is stable with lithium metal and can form a stable SEI; lithium p-styrene sulfonate (LiSS) has an additional lithium ion source, which can provide additional kinetics and further improve the rate performance of the battery.
[0016] Specifically, the molar ratio of monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) is 5-25:50-90:5-25, optionally 20:60:20. Within this range, the overall ionic conductivity of the electrolyte layer can be ensured to be high, and the cycle performance and capacity of the battery are excellent. In the present application, the molar ratio of monomers of acrylonitrile (AN) and vinylene carbonate (VC) is equal. In this case, a stable interface can be formed with both the positive and negative electrodes, thereby improving the stability of the battery.
[0017] In addition, some embodiments of the present application also provide a method for preparing the above-mentioned polymer electrolyte, comprising the following steps:
[0018] The polymer substrate (A) is a commercially available polymer, including but not limited to fluorine-containing polymers such as polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), PVDF-HFP-PTFE (fluororubber), and fluorine-free polymers such as polyimide (PI) and polymethyl methacrylate (PMMA).
[0019] The synthesis method of copolymer (B) is as follows: acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) are mixed and dissolved in a certain amount of solvent (such as dimethyl sulfoxide), and then 0.1wt% azobisisobutyronitrile (AIBN) is dissolved in the mixture. The resulting solution is kept at 60°C for 15 hours under an argon atmosphere. The resulting solid is dissolved in anhydrous dimethyl sulfoxide and washed with toluene to remove residual monomers and initiators to obtain a pure copolymer. The molar ratio of the monomers of AN, LiSS and VC is 5-25:50-90:5-25, and the molar ratio of the monomers of AN and VC is optionally equal, and the molar ratio of the monomers of AN, LiSS and VC is optionally 20:60:20. In some embodiments, the above-mentioned solvent may include polar solvents such as dimethyl sulfoxide (DMSO) and N,N dimethylformamide. In some specific embodiments, the solvent may be DMSO, and the mass fraction of the polymer solution may be 10%.
[0020] Polymer preparation: The polymer substrate (A) and the copolymer (B) are mixed in a solvent (DMSO), and after sufficient heating and stirring to dissolve, the solution is poured into a mold and dried to obtain a polymer film; or the polymer substrate (A) can be electrospun, and a solution of the copolymer (B) is poured onto the polymer substrate (A) and dried to form a film to obtain a polymer film, wherein the mass ratio of the polymer substrate (A): copolymer (B) is 10:90-90:10, and can be optionally 30:70.
[0021] Preparation of polymer electrolyte: The polymer film obtained above is immersed in a high-voltage resistant electrolyte for 24 hours. The electrolyte here includes but is not limited to some commonly used high-voltage resistant electrolytes (above 4.5V).
[0022] In the above embodiment, the high-voltage resistant electrolyte includes but is not limited to: lithium hexafluorophosphate (LiPF6) 14%, lithium bis(fluorosulfonyl)imide (LiFSI) 1%, lithium difluorophosphate (LiPO2F2) 0.8%, lithium tetrafluoroborate (LiBF4) 0.1%, vinylene carbonate (VC) 0.1%, 1,3-propane sultone (1,3-PS) 1%, ethylene carbonate (EC) 24.9%, ethyl methyl carbonate (EMC) 41.5%, and diethyl carbonate (DEC) 16.6%.
[0023] Some embodiments of the present application also provide a secondary battery and an electrical device including the secondary battery. The secondary battery includes a positive electrode sheet, a negative electrode sheet, and an electrolyte layer.
[0024] Preparation method of positive electrode sheet: Disperse positive electrode active material, positive electrode conductive agent and positive electrode binder in a solvent in a mass ratio of 95:2:3 to form a uniform positive electrode slurry, apply the positive electrode slurry on the surface of the positive electrode collector, and after drying, cold pressing and other processes, form a positive electrode active material layer on the positive electrode collector to obtain a positive electrode sheet. The ratio between the components in the positive electrode slurry can be set with reference to the conventional ratio, and is not limited here. The positive electrode conductive agent is selected from one of carbon black, acetylene black, graphene, carbon nanotubes, carbon nanofibers, etc. or a combination of two or more mixed in any proportion. The positive electrode binder selects one of PVDF and its derivatives. The positive electrode active material may include one or more of lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium manganese oxide (LMO), lithium nickel manganese oxide (LNMO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA) and lithium-rich manganese-based oxide (LRMO). In some embodiments, the positive electrode collector may be aluminum foil.
[0025] Negative electrode
[0026] The lithium metal is selected from different thicknesses (such as lithium metal having a thickness of 10 μm to 600 μm).
[0027] Electrolyte layer
[0028] The above-mentioned polymer electrolyte was used directly as the polymer electrolyte layer.
[0029] Secondary battery
[0030] The positive electrode sheet, electrolyte layer and negative electrode sheet are sequentially placed into the mold for assembly; after assembly, pressurization is applied and the nut at the top of the column is tightened with a constant pressure to obtain a secondary battery.
[0031] Note: The assembly process is completed in a glove box with an argon atmosphere, and the particle diameters of the corresponding powders of the positive electrode sheet, electrolyte layer and negative electrode sheet are kept consistent.
[0032] It should be noted that the lithium ion secondary battery prepared by the above method. However, the battery prepared in the present application may also be a sodium ion secondary battery or a potassium ion secondary battery.
[0033] Those skilled in the art will understand that the above-described method for preparing the battery is only an example, and other commonly used methods in the art may be used without departing from the contents disclosed in the present application.
[0034] The reagents and raw materials used in the present invention are commercially available.
[0035] The present invention has no special requirements for the assembly method of the above-mentioned battery, and an assembly method familiar to those skilled in the art can be used. In addition, the above-mentioned technical solution can be applied not only to commonly used all-solid-state lithium-ion batteries, but also to all-solid-state sodium-ion batteries, all-solid-state potassium-ion batteries and other types of kinetic batteries. The above-mentioned secondary battery can be applied to any suitable electrical device, including but not limited to electric vehicles.
[0036] Some specific embodiments and comparative examples are listed below to better illustrate the present application.
[0037] Example 1
[0038] (1) Preparation of polymer electrolyte:
[0039] The polymer substrate (A) is polyvinylidene fluoride (PVDF).
[0040] The synthesis method of copolymer (B) is as follows: acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) are mixed and dissolved in a solvent (the solvent can be DMSO, and the mass fraction of the polymer solution can be 10%), and then 0.1wt% azobisisobutyronitrile (AIBN) is dissolved in the mixture. The resulting solution is kept at 60°C for 15 hours under an argon atmosphere. The resulting solid is dissolved in anhydrous dimethyl sulfoxide and washed with toluene to remove residual monomers and initiators to obtain a pure copolymer, wherein the molar ratio of the monomers of AN, LiSS and VC is 20:60:20.
[0041] The polymer substrate (A) and the copolymer (B) are mixed in a solvent, and after sufficient heating and stirring to dissolve, the solution is poured into a polytetrafluoroethylene mold and dried to obtain a polymer film, wherein the mass ratio of the polymer substrate (A) to the copolymer (B) is 30:70.
[0042] The polymer film obtained above was immersed in a high-voltage resistant electrolyte commonly used in the art for 24 hours to obtain a polymer electrolyte.
[0043] (2) Positive electrode
[0044] The positive electrode active material is selected from lithium-rich manganese-based oxide (LRMO), the positive electrode conductive agent is selected from carbon black, the positive electrode binder is selected from PVDF, and the positive electrode current collector is selected from aluminum foil.
[0045] (3) Negative electrode
[0046] Selected from 10μm lithium metal.
[0047] (4) Electrolyte layer
[0048] The above-mentioned polymer electrolyte was used directly as the polymer electrolyte layer.
[0049] (5) Secondary battery
[0050] The positive electrode sheet, electrolyte layer and negative electrode sheet are sequentially placed into the mold for assembly; after assembly, the pressure is increased to 100 MPa and the nut at the top of the column is tightened to a constant pressure to obtain a secondary battery.
[0051] Note: The assembly process is completed in a glove box with an argon atmosphere, and the particle diameters of the corresponding powders of the positive electrode sheet, electrolyte layer and negative electrode sheet are kept consistent.
[0052] Example 2
[0053] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Example 2 is 10:90.
[0054] Example 3
[0055] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Example 3 is 90:10.
[0056] Example 4
[0057] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Example 4 is 50:50.
[0058] Example 5
[0059] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Example 5 is 60:40.
[0060] Example 6
[0061] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 6 is 5:90:5.
[0062] Example 7
[0063] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 7 is 25:50:25.
[0064] Example 8
[0065] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 8 is 10:80:10.
[0066] Example 9
[0067] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 9 is 15:70:15.
[0068] Example 10
[0069] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 10 is 20:60:20.
[0070] Embodiment 11
[0071] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Example 11 is 20:65:15.
[0072] Example 12
[0073] The preparation method is consistent with that of Example 1, except that the polymer substrate (A) in Example 12 is PVDF-HFP.
[0074] Embodiment 13
[0075] The preparation method is consistent with that of Example 1, except that the polymer substrate (A) in Example 13 is PVDF-HFP-PTFE.
[0076] Embodiment 14
[0077] The preparation method is consistent with that of Example 1, except that the polymer substrate (A) in Example 14 is polyimide (PI).
[0078] Embodiment 15
[0079] The preparation method is consistent with that of Example 1, except that the polymer substrate (A) in Example 15 is polymethyl methacrylate (PMMA).
[0080] Example 16
[0081] The preparation method is consistent with that of Example 1, except that the polymer substrate (A) in Example 16 is a mixture of polyvinylidene fluoride (PVDF) and polyimide (PI) (mass ratio is 1:1).
[0082] Comparative Example 1
[0083] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Comparative Example 1 is 5:95.
[0084] Comparative Example 2
[0085] The preparation method is consistent with that of Example 1, except that the mass ratio of the polymer substrate (A) to the copolymer (B) in Comparative Example 2 is 95:5.
[0086] Comparative Example 3
[0087] The preparation method is consistent with that of Example 1, except that Comparative Example 3 contains only the polymer substrate (A) but no copolymer (B).
[0088] Comparative Example 4
[0089] The preparation method is consistent with that of Example 1, except that Comparative Example 4 contains only the copolymer (B) but no polymer substrate (A).
[0090] Comparative Example 5
[0091] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 5 is 3:94:3.
[0092] Comparative Example 6
[0093] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 6 is 30:40:30.
[0094] Comparative Example 7
[0095] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 7 is 0:75:25.
[0096] Comparative Example 8
[0097] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 8 is 25:75:0.
[0098] Comparative Example 9
[0099] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 9 is 50:0:50.
[0100] Comparative Example 10
[0101] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 10 is 0:0:100.
[0102] Comparative Example 11
[0103] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 11 is 0:100:0.
[0104] Comparative Example 12
[0105] The preparation method is consistent with that of Example 1, except that the molar ratio of the monomers of AN, LiSS and VC in the copolymer (B) in Comparative Example 12 is 100:0:0.
[0106] Performance Testing Methods
[0107] Under 25°C environment, the secondary batteries prepared in Examples 1 to 16 and Comparative Examples 1 to 12 were charged and discharged for a long cycle after being fixed in capacity, and the number of cycles at room temperature was measured; the test conditions were to perform a long cycle charge and discharge test on the battery after being fixed in capacity, and during the process, the first cycle fixed capacity discharge specific capacity and the number of cycles at room temperature when SOH was 50% were recorded; the operating voltage range was 1.9 to 3.7V, the fixed capacity ratio was 0.1C, and the normal temperature cycle test ratio was 0.3C. For Example 4, its test method was the same as that of other Examples and Comparative Examples, except that the operating voltage range was 1.4 to 4.25V.
[0108] Note: The following conditions are met at the same time for good performance: Li / Li symmetrical battery 1mA / cm 2 The cycle short-circuit time is greater than 500h, the number of cycles of the LMR / Li battery at room temperature is greater than 300 when the SOH is 80%, and the 1C capacity is greater than 170mAh / g.
[0109] The test results are shown in Table 1 below.
[0110] Table 1. Secondary battery performance test results of Examples 1 to 16 and Comparative Examples 1 to 12
[0111]
[0112]
[0113] As can be seen from the above-mentioned embodiments 1-16, the present application is designed by the structure of the polymer electrolyte so that it contains two polymers, specifically, including a polymer substrate (A) and a copolymer (B), the polymer substrate (A) includes a supporting material and provides mechanical support, and the copolymer (B) contains a cyano group, an ester group and a sulfonic acid group. In the present application, the polymer substrate (A) provides mechanical strength as a supporting material, and the role of the copolymer (B) is to form a stable interface with the positive and negative electrodes. As can be seen from the above, the copolymer (B) is copolymerized by three types of monomers, respectively containing a cyano group, an ester group, and a sulfonic acid group, which are polar groups, can improve the mechanical properties of the electrolyte, and have high reduction resistance and oxidation resistance, can form a stable SEI film (solid electrolyte interface film) with the negative electrode, and form a stable CEI (cathode electrolyte interface film) with the positive electrode, can simultaneously match the lithium metal negative electrode and the lithium-rich manganese-based positive electrode, can make the prepared secondary battery have a high energy density, and can be circulated for a long time. Furthermore, the copolymer (B) is copolymerized by acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC). The three copolymers have different functions. Acrylonitrile (AN) has a polar functional group cyano and has high-voltage stability; vinylene carbonate (VC) is stable with lithium metal and can form a stable SEI; lithium p-styrene sulfonate (LiSS) has an additional source of lithium ions, which improves the capacity and rate performance of the battery.
[0114] Specifically, by comparing Examples 1-5 with Comparative Examples 1-4, it can be seen that the mass ratio of polymer substrate (A) to copolymer (B) is in the range of 10:90-90:10, and optionally 30:70. The polymer substrate (A) can be used as a supporting material to provide mechanical strength, and a stable interface is formed between the copolymer (B) and the positive and negative electrodes, so that the prepared secondary battery has good performance, high energy density and can be cycled for a long time. Specifically, it can be seen from Example 1 that 30% of the polymer substrate (A) is sufficient to provide mechanical properties, 70% of the AN and VC in the copolymer (B) are stable with the positive and negative electrode interfaces, and the LiSS contained will provide additional kinetics, which is conducive to the use of capacity. It can be seen from Example 2 that the content of copolymer (B) becomes higher, the overall ionic conductivity of the electrolyte layer is very high, and the corresponding secondary battery has a high 1C capacity, which can reach 193mAh / g. It can be seen from Examples 3-5 that there are more polymer substrates (A) and the overall mechanical properties are very good, so the corresponding secondary battery has good cycle stability. It can be seen from Comparisons 1 and 4 that the polymer substrate (A) is too little and the mechanical properties are too poor, so the long-term cycle stability of the corresponding secondary battery is poor; it can be seen from Comparative Examples 2 and 3 that the copolymer (B) is too little, the interface stability with the positive and negative electrodes is poor, and the conductivity is low, so the formed secondary battery has poor long-term cycle stability and low capacity.
[0115] Comparing Examples 6-11 and Comparative Examples 5-12, it can be seen that the molar ratio of the monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) in the copolymer (B) is 5-25:50-90:5-25, which can be optionally 20:60:20, and the molar ratio of the monomers of acrylonitrile (AN) and vinylene carbonate (VC) is optionally equal. When within this range, the ionic conductivity is high, the capacity is high, and the cycle stability and capacity of the resulting secondary battery are excellent. Specifically, it can be seen from Examples 6 and 8 that when there is more lithium p-styrene sulfonate (LiSS) in the copolymer (B), the ionic conductivity is high, and the capacity of the corresponding secondary battery is high, which can reach 195 mAh / g. It can be seen from Examples 7 and 9-10 that there are more acrylonitrile (AN) and vinylene carbonate (VC) in the copolymer (B), so that the cycle stability of the corresponding secondary battery is better. As can be seen from Example 11, when the molar ratio of acrylonitrile (AN) and vinylene carbonate (VC) monomers is equal or unequal, although the performance of the corresponding secondary battery is improved, the improvement effect is limited. This is because when acrylonitrile (AN) and vinylene carbonate (VC) are unequal, the balance between the stability of the positive and negative electrodes of the corresponding secondary battery may be affected, thereby affecting the performance of the secondary battery. As can be seen from Comparative Example 5, when there are too few AN and VC in the copolymer (B), the interface stability between the positive and negative electrodes is poor, so the long-term cycle stability of the corresponding secondary battery is poor. As can be seen from Comparative Example 6, when there is too little LiSS in the copolymer (B), the interface stability between the positive and negative electrodes is poor, so the long-term cycle stability of the secondary battery is poor. As can be seen from Comparative Example 7, when the copolymer (B) does not contain AN, the interface stability between the positive electrode is very poor, so the long-term cycle stability of the secondary battery is poor. As can be seen from Comparative Example 8, when the copolymer (B) does not contain VC, the interface stability between the negative electrode is very poor, so the long-term cycle stability of the secondary battery is poor. As can be seen from Comparative Example 9, when the copolymer (B) does not contain LiSS, the conductivity is low, so the capacity of the secondary battery is low. As can be seen from Comparative Example 10, when the copolymer (B) does not contain AN and LiSS, the interface stability with the positive electrode is poor, and the conductivity is also low, so the long-term cycle stability of the secondary battery is poor and the capacity is low. As can be seen from Comparative Example 11, when the copolymer (B) does not contain AN and VC, the interface stability with both the positive and negative electrodes is poor, so the long-term cycle stability of the secondary battery is poor. As can be seen from Comparative Example 12, when the copolymer (B) does not contain LiSS and VC, the interface stability with the negative electrode is poor, and the conductivity is also low, so the long-term cycle stability of the secondary battery is poor and the capacity is low.
[0116] As can be seen from Examples 12 to 16, the polymer substrate (A) can be selected from any one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), PVDF-HFP-PTFE (fluororubber), polyimide (PI), and polymethyl methacrylate (PMMA), so that the cycle stability and capacity of the formed secondary battery are good. In addition, PVDF-HFP has similar performance to PVDF, and the cycle stability and capacity of the formed secondary battery are excellent.
[0117] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that this equivalent construction does not deviate from the spirit and scope of the present invention, and that they can make multiple changes, substitutions and changes herein without departing from the spirit and scope of the present invention.
Claims
1. A polymer electrolyte, characterized in that include: polymer substrate; as well as Copolymers, The polymer substrate comprises a supporting material, and the copolymer contains a cyano group, an ester group and a sulfonic acid group.
2. The polymer electrolyte according to claim 1, characterized in that The mass ratio of the polymer substrate to the copolymer is in the range of 10:90-90:
10.
3. The polymer electrolyte according to claim 1, characterized in that The mass ratio of the polymer substrate to the copolymer is 30:
70.
4. The polymer electrolyte according to claim 1, characterized in that The copolymer is prepared by copolymerization of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC).
5. The polymer electrolyte according to claim 4, characterized in that The molar ratio of the monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) is 5-25:50-90:5-25.
6. The polymer electrolyte according to claim 5, characterized in that The molar ratio of the monomers of the acrylonitrile (AN) and the vinylene carbonate (VC) is equal.
7. The polymer electrolyte according to claim 5, characterized in that The molar ratio of the monomers of acrylonitrile (AN), lithium p-styrene sulfonate (LiSS) and vinylene carbonate (VC) is 20:60:
20.
8. The polymer electrolyte according to claim 1, characterized in that The polymer substrate is selected from any one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), PVDF-HFP-PTFE (fluororubber), polyimide (PI), and polymethyl methacrylate (PMMA).
9. A secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet and an electrolyte layer, wherein the electrolyte layer comprises a polymer electrolyte according to any one of claims 1-8.
10. An electrical device, characterized in that: The secondary battery according to claim 9 is included.