Electrolyte and secondary battery
By optimizing the proportion of solvents in the electrolyte, increasing the amount of high viscosity solvents and reducing the amount of low viscosity solvents, the problem of insufficient wetting and stability of the electrolyte under high winding pressure is solved, and fast charging and raising of high energy density batteries is achieved. High temperature stability improves the fast charging and cycling performance of the battery.
Patent Information
- Application Number
- CN202411172070.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
AI Technical Summary
It is difficult for existing electrolytes to take into account both wetting and high temperature stability under high winding pressure, and cannot meet the needs of high-speed fast charging, resulting in attenuation of the high-temperature storage performance and fast charging and cycling performance of the battery.
By optimizing the types and proportions of solvents in the electrolyte, increasing the amount of high-viscosity solvents and reducing the amount of low-viscosity solvents, the overall viscosity of the electrolyte conforms to the logarithmic law, ensuring chemical stability, and achieving excellent results in high-energy-density winding structural batteries fast charging capability and high temperature stability.
It realizes the high wetting and stability in high-winding electrode assembly, meets the needs of high-rate fast charging, and improves the fast charging cycle performance and high-temperature storage performance of the battery.
Smart Images

Figure BDA0005009588510000161 
Figure BDA0005009588510000171 
Figure BDA0005009588510000172
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to an electrolyte and a secondary battery. Background Art
[0002] Lithium-ion batteries are widely used in consumer electronics, electric vehicles and energy storage due to their long cycle life, high operating voltage, low self-discharge rate, no memory effect and environmental friendliness. In the above application areas, people have higher and higher requirements for battery life and charging speed, and there is an urgent need for fast-charging batteries with higher energy density.
[0003] In order to improve the energy density of batteries, the battery structure design is developing towards high volume energy density, especially the electrode assembly with a winding structure inside, such as cylindrical batteries. As the volume energy density inside the battery increases, the interlayer pressure between the wound pole pieces of the electrode assembly also increases. Under high winding pressure, it is difficult for the electrolyte to infiltrate the interlayer of the electrode assembly, which has a negative impact on the battery charge and discharge cycle.
[0004] To address the problem of insufficient wettability of the electrolyte, the existing technology generally improves the wettability of the electrolyte by increasing the content of low-viscosity solvents in the electrolyte. However, as the demand for fast charging of batteries becomes higher and higher, the existing electrolytes are difficult to meet the demand for high-rate fast charging under high winding pressure, resulting in serious degradation of the high-temperature storage performance and fast-charging cycle performance of batteries using existing electrolyte solutions.
[0005] Therefore, it is necessary to design an electrolyte and a secondary battery to solve the above technical problems. Summary of the invention
[0006] In view of the above shortcomings of the prior art, the present invention provides an electrolyte and a secondary battery to improve the technical problems in the prior art that the electrolyte is difficult to balance wettability and high temperature stability under high winding pressure and cannot meet the requirements of fast charging at high rates.
[0007] To achieve the above-mentioned object and other related objects, the present invention provides an electrolyte, the electrolyte comprising a lithium salt and a solvent, wherein the solvent comprises a cyclic carbonate, a linear carbonate and a carboxylate; the mass percentage of the cyclic carbonate relative to the electrolyte is 8% to 24%, the linear carbonate comprises dimethyl carbonate and at least one of ethyl methyl carbonate and diethyl carbonate, the sum of the masses of the ethyl methyl carbonate and the diethyl carbonate relative to the electrolyte is 2% to 10%, the mass percentage of the carboxylate relative to the electrolyte is 20% to 40%, the carboxylate comprises a first component and a second component, the viscosity of the first component at 25±2°C is 0.4-0.5mPa·s, the viscosity of the second component at 25±2°C is 0.3-0.4mPa·s, the mass percentage of the first component relative to the electrolyte is 15% to 40%, and the mass percentage of the second component relative to the electrolyte is 0% to 15%.
[0008] In one example of the present invention, the first component includes one or more of ethyl acetate, methyl propionate, propyl acetate, and ethyl propionate, and the second component includes one or more of methyl acetate, ethyl formate, and methyl formate.
[0009] In an example of the present invention, the cyclic carbonate includes fluoroethylene carbonate and at least one of ethylene carbonate and propylene carbonate.
[0010] In an example of the present invention, the mass percentage of the fluoroethylene carbonate relative to the electrolyte is 2% to 8%.
[0011] In an example of the present invention, the linear carbonate includes dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
[0012] In an example of the present invention, the electrolyte further includes an additive, the additive includes 1,3-propylene sultone, vinyl sulfate and tetravinylsilane, and the mass percentage of the additive relative to the electrolyte is 0.8% to 2%.
[0013] In an example of the present invention, the lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, the mass percentage of the lithium salt relative to the electrolyte is 8% to 20%, and the mass percentage of the lithium bis(fluorosulfonyl)imide relative to the electrolyte is 0% to 2%.
[0014] The present invention also provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte described in any one of the above examples.
[0015] In an example of the present invention, the secondary battery is a cylindrical battery.
[0016] In an example of the present invention, the upper limit of the operating voltage of the secondary battery is above 4.15V.
[0017] The electrolyte provided by the present invention optimizes the dosage of solvents with different viscosities so that the overall viscosity of the electrolyte is in a relatively low range while ensuring that the solvent has sufficient chemical stability, thereby achieving excellent fast charging capability and high temperature stability in a battery with a high energy density wound structure. DETAILED DESCRIPTION
[0018] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.
[0019] For simplicity, only some numerical ranges are explicitly disclosed herein, and each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unspecified range.
[0020] At present, the existing technical solutions generally reduce the overall viscosity of the electrolyte and improve the wetting performance of the electrolyte by increasing the amount of low-viscosity solvent in the electrolyte (such as reducing the content of ethylene carbonate and increasing the content of dimethyl carbonate in the electrolyte), thereby improving the problem of insufficient wettability between the electrodes under high winding interlayer pressure. However, the inventors have found that due to the poor chemical stability of low-viscosity solvents, the existing electrolyte solutions will deteriorate the chemical stability of the electrolyte due to excessive use of low-viscosity solvents. The existing electrolytes deteriorate the high-temperature performance of the battery and are also difficult to meet the requirements of faster charging at higher rates.
[0021] To this end, the inventors have provided an electrolyte based on their in-depth understanding of the solution viscosity theory. The electrolyte optimizes the type and proportion of solvents, adjusts the amount of high-viscosity solvents and low-viscosity solvents in the electrolyte, and increases the amount of high-viscosity solvents and reduces the amount of low-viscosity solvents so that the overall viscosity of the mixed electrolyte conforms to the logarithmic law, thereby maintaining the overall viscosity of the electrolyte in a relatively low range, while ensuring that the electrolyte solvent has sufficient chemical stability. As a result, the electrolyte can take into account both high wettability and stability, so that the electrolyte can meet the high-rate fast charging requirements in batteries with wound electrode assemblies.
[0022] The electrolyte includes a lithium salt and a solvent, and the solvent includes a cyclic carbonate, a linear carbonate and a carboxylate.
[0023] The mass percentage of the cyclic carbonate relative to the electrolyte is any value between 8% and 24%; for example, it can be 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22% or 24%. Since the cyclic carbonate has a higher conductivity and viscosity in the solvent, the cyclic carbonate is maintained within the above-mentioned suitable mass percentage range in the electrolyte to ensure both lower viscosity and higher conductivity of the electrolyte. If the content of the cyclic carbonate in the electrolyte is too high, the viscosity of the electrolyte will be too high, thereby deteriorating the fast charging performance of the battery; if the content of the cyclic carbonate in the electrolyte is too low, although the viscosity of the electrolyte can be reduced, it will also cause the conductivity of the electrolyte to decrease, thereby also deteriorating the fast charging performance of the battery.
[0024] The linear carbonate includes at least one of dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) and diethyl carbonate (DEC). For example, the linear carbonate can be a combination of ethyl methyl carbonate and dimethyl carbonate; or a combination of diethyl carbonate and dimethyl carbonate; or a combination of dimethyl carbonate, diethyl carbonate and dimethyl carbonate. It should be noted that when the linear carbonate is a composition, there is no restriction on the ratio between the components in the composition, and the linear carbonate can be mixed in any ratio.
[0025] In the linear carbonate, the sum of the masses of ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) relative to the mass percentage of the electrolyte is any value between 2% and 10%; specifically, when the component included in the linear carbonate is ethyl methyl carbonate, the mass percentage of ethyl methyl carbonate relative to the electrolyte is any value between 2% and 10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%; when the component included in the linear carbonate is diethyl carbonate, The mass percentage of diethyl carbonate relative to the electrolyte is any value between 2% and 10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%; when the component included in the linear carbonate is a combination of ethyl methyl carbonate and diethyl carbonate, the mass percentage of the sum of ethyl methyl carbonate and diethyl carbonate relative to the electrolyte is any value between 2% and 10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.
[0026] Since ethyl methyl carbonate and diethyl carbonate have high viscosity and good chemical stability in the solvent, maintaining ethyl methyl carbonate and / or diethyl carbonate in the electrolyte within the above-mentioned appropriate mass percentage range can ensure the high-temperature stability of the electrolyte while avoiding the increase in the viscosity of the electrolyte. If the content of ethyl methyl carbonate and / or diethyl carbonate in the electrolyte is too high, the viscosity of the electrolyte will be too high, thereby deteriorating the fast charging performance of the battery; if the content of ethyl methyl carbonate and / or diethyl carbonate in the electrolyte is too low, the chemical stability of the electrolyte will be deteriorated, causing the high-temperature storage capacity recovery rate of the battery to deteriorate significantly.
[0027] The mass percentage of the carboxylate relative to the electrolyte is 20% to 40%, and the carboxylate includes a first component and a second component, the viscosity of the first component at 25±2°C is 0.4-0.5 mPa·s, and the viscosity of the second component at 25±2°C is 0.3-0.4 mPa·s. Wherein, the mass percentage of the first component relative to the solvent is any value from 15% to 40%, for example, it can be 15%, 17%, 20%, 23%, 25%, 27%, 30%, 33%, 35%, 37% or 40%. The mass percentage of the second component relative to the electrolyte is less than or equal to 15%, that is, the mass percentage of the second component relative to the electrolyte is any value from 0% to 15%, for example, it can be 0%, 2%, 4%, 5%, 6%, 8%, 10%, 12%, 14% or 15%.
[0028] Based on the ratio of the two higher viscosity components of cyclic carbonate and linear carbonate, the high viscosity first component and the low viscosity second component in the carboxylate are limited to the above mass percentage range, so that the overall viscosity of the electrolyte composed of solvents at each viscosity level conforms to the logarithmic law, thereby maintaining the overall viscosity of the electrolyte in a low range while ensuring that the conductivity of the electrolyte will not decay. In addition, by limiting the content of low viscosity solvents in the electrolyte, the chemical stability of the electrolyte can be effectively maintained, thereby maintaining the high temperature storage performance of the battery.
[0029] In some embodiments, the first component in the carboxylate includes one or more of ethyl acetate (EA), methyl propionate (MP), propyl acetate (PA), and ethyl propionate (EP). That is, the first component in the carboxylate can be any one of the above-listed types, such as ethyl acetate, methyl propionate, propyl acetate, or ethyl propionate; the first component in the carboxylate can also be any combination of the above-listed types, such as a combination of ethyl acetate and methyl propionate, or a combination of ethyl acetate and propyl acetate, or a combination of ethyl acetate and ethyl propionate, or a combination of ethyl acetate, methyl propionate, and propyl acetate, or a combination of ethyl acetate, methyl propionate, and ethyl propionate, or a combination of ethyl acetate, methyl propionate, propyl acetate, and ethyl propionate. It should be noted that when the first component in the carboxylate is a combination, there is no restriction on the ratio between the components in the combination, and any ratio can be mixed.
[0030] In some embodiments, the second component in the carboxylic acid ester includes one or more of methyl acetate (MA), ethyl formate (EF), and methyl formate (MF). That is, the second component in the carboxylic acid ester can be any one of the types listed above, such as methyl acetate, ethyl formate, or methyl formate; the second component in the carboxylic acid ester can also be any combination of the types listed above, such as a combination of methyl acetate and ethyl formate, or a combination of methyl acetate and methyl formate, or a combination of ethyl formate and methyl formate, or a combination of methyl acetate, ethyl formate, and methyl formate. It should be noted that when the second component in the carboxylic acid ester is a combination, there is no restriction on the ratio between the components in the combination, and they can be mixed in any ratio.
[0031] In certain embodiments, cyclic carbonate comprises at least one of fluoroethylene carbonate (FEC) and ethylene carbonate (EC) and propylene carbonate (PC), for example, cyclic carbonate can be a composition of fluoroethylene carbonate and ethylene carbonate, or a composition of fluoroethylene carbonate and propylene carbonate, or a composition of fluoroethylene carbonate, ethylene carbonate and propylene carbonate. It should be noted that the ratio between the components in the cyclic carbonate composition is not limited, and can be mixed in any proportion.
[0032] In some embodiments, in the cyclic carbonate, the mass percentage of fluoroethylene carbonate (FEC) relative to the electrolyte is any value between 2% and 8%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7% or 8%. An appropriate amount of fluoroethylene carbonate in the solvent can take into account both the protection effect of the electrolyte on the negative electrode interface and the control of the battery's cyclic gas production. Among them, when the content of fluoroethylene carbonate in the solvent is too high, although the excess fluoroethylene carbonate can improve the rate performance of the electrolyte, it is also easy to decompose at high temperature to produce hydrogen fluoride, affecting the high temperature storage performance of the battery; when the content of fluoroethylene carbonate in the solvent is too low, too little fluoroethylene carbonate cannot play the role of negative electrode film formation to protect the negative electrode, which will cause side reactions between the electrolyte and the negative electrode during the cycle, destroying the cycle stability of the battery and deteriorating the storage capacity of the battery.
[0033] In some embodiments, the electrolyte further includes additives, including 1,3-propylene sultone (PST), dithiothreitol (DTD) and tetravinylsilane (TVSi). The additives help to form a stable solid electrolyte interface film (SEI) at the negative electrode interface, which can further enhance the film-forming effect of the electrolyte at the negative electrode interface, enhance the protective effect on the negative electrode interface, and improve the charge and discharge cycle performance of the battery.
[0034] In some embodiments, the mass percentage of the additive relative to the electrolyte is any value between 0.8% and 2%, for example, it can be 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8% or 2%. When the total content of the additive in the electrolyte is within the above range, it can promote the formation of the SEI film at the negative electrode interface without excessively increasing the impedance of the battery, thereby affecting the fast charging performance of the battery. When the content of the additive in the electrolyte is too little, it will lead to insufficient film formation of the SEI film at the negative electrode interface, making it difficult to effectively protect the negative electrode, thereby having a negative impact on the cycle capacity of the battery; when the content of the additive in the electrolyte is too much, it will cause the impedance of the SEI film at the negative electrode interface to be too high, which will have a negative impact on the fast charging performance of the battery.
[0035] In addition, it should be noted that the lithium salt in the electrolyte can be selected from conventional lithium salts in the art. As an example, the lithium salt is selected from one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium bis(fluorooxalatoborate) (LiODFB) and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI). Preferably, the lithium salt is selected from lithium hexafluorophosphate (LiPF6) with good comprehensive performance, or lithium hexafluorophosphate (LiPF6) is mainly used, and other lithium salts are added in appropriate amounts to take advantage of their advantages and improve the performance of the electrolyte. For example, in some embodiments, the lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, and the mass percentage of the lithium salt in the electrolyte is any value between 8% and 20%, such as 8%, 10%, 12%, 14%, 15%, 16%, 17%, 18% or 20%; wherein the mass percentage of lithium bis(fluorosulfonyl)imide in the electrolyte is any value between 0% and 2%, such as 0%, 0.2%, 0.4%, 0.5%, 0.7%, 1%, 1.3%, 1.5%, 1.7% or 2%. When the content of lithium bis(fluorosulfonyl)imide is too high, the corrosion to the electrode current collector will be more serious, so in this embodiment, the content of lithium bis(fluorosulfonyl)imide is limited to the above range to protect the electrode current collector.
[0036] The electrolyte of the present invention can be prepared according to a conventional preparation method, for example, the electrolyte is prepared in a glove box, the argon or nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is less than 10ppm. In the glove box, the solvent is mixed and stirred, and then the lithium salt is added to the mixed solvent under stirring conditions, and the stirring is continued until the lithium salt is completely dissolved, and finally the additive can be added and stirred evenly.
[0037] The present invention also provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte described in any one of the above embodiments. During the battery charging and discharging process, lithium ions are inserted and removed back and forth between the positive electrode sheet and the negative electrode sheet, and the separator is arranged between the positive electrode sheet and the negative electrode sheet to play a role of isolation; the electrolyte plays a role of conducting lithium ions between the positive electrode sheet and the negative electrode sheet.
[0038] The composition and preparation method of the secondary battery are described in detail below:
[0039] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. Among them, the positive current collector is, for example, a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel or carbon. In addition to the foil, the positive current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Among them, the thickness of the positive current collector is, for example, 8μm-15μm. In one embodiment, the positive current collector is, for example, aluminum foil, and the thickness of the aluminum foil is, for example, 13μm. The positive current collector has two surfaces opposite to each other in its own thickness direction, and the positive active material layer is disposed on any one or both of the two opposite surfaces of the positive current collector. The positive active material layer includes a positive active material, a positive conductive agent and a positive binder. There is no specific restriction on the positive active material, the positive conductive agent and the positive binder here, and those skilled in the art can choose according to actual needs.
[0040] As an example, the positive electrode active material can be selected from ternary materials, lithium-containing phosphates, and spinel materials, wherein the ternary materials include lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide doped with metal ions, lithium nickel cobalt aluminum oxide doped with metal ions, etc.; lithium-containing phosphates include lithium iron manganese phosphate, lithium iron phosphate, lithium manganese phosphate, etc. The positive electrode binder is selected from polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE), etc. The positive electrode conductive agent is selected from one of carbon black, acetylene black, graphene, carbon nanotubes, carbon nanofibers, etc., or a combination of two or more of them mixed in any proportion.
[0041] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector can be made of a material with good electrical conductivity and mechanical strength, such as copper foil. The negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent, a negative electrode binder and a thickener. The specific types of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are not specifically limited here. Materials known in the art that can be used in lithium-ion batteries can be used, and those skilled in the art can select according to actual needs.
[0042] As an example, the negative electrode active material is selected from one or more combinations of carbon materials and silicon materials. For example, carbon materials include hard carbon, artificial graphite, natural graphite, etc., and silicon materials include elemental silicon, silicon oxide compounds, silicon carbon compounds, etc. The negative electrode conductive agent is selected from one of carbon black, acetylene black, graphene, carbon nanotubes, carbon nanofibers, etc., or a combination of two or more mixed in any proportion. The negative electrode binder is selected from any one of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), or a combination of several mixed in any proportion; the thickener is selected from carboxymethyl cellulose CMC-Na or CMC-Li.
[0043] The isolation membrane is selected from conventional types in the art, for example, PE or PP porous membrane can be selected as the isolation membrane, the thickness of the isolation membrane is 9 to 18 μm, the air permeability is 180 s / 100 mL to 380 s / 100 mL; the porosity is 30% to 50%.
[0044] The battery assembly is carried out according to conventional methods, for example: after preparation, the negative electrode sheet, the separator, and the positive electrode sheet are stacked and wound in sequence, so that the separator is located between the positive and negative electrodes to play a role of isolation. Then the wound electrode assembly is packaged into a shell, transferred to a vacuum oven at 120°C for drying, and the above-prepared electrolyte 3.0g / Ah is injected and sealed, and the electrolyte is formed, and finally a lithium-ion battery with a capacity of 1Ah is prepared.
[0045] In some embodiments, the upper limit of the working voltage of the secondary battery is greater than or equal to 4.15V. For example, in one example, the working voltage of the secondary battery is 2.5V to 4.25V. Since the upper limit of the working voltage of the secondary battery is mainly determined by the positive electrode active material, the positive electrode active material in this embodiment can be selected from conventional high energy density positive electrode materials in the art, such as high nickel ternary materials or nickel manganese spinel materials. Among them, the high nickel ternary material is LiNi a Co b M 1-a-b O2, 0.8≤a<1, 0<b≤0.1, M element is selected from at least one of Mn, Al, Ti, Zr, Cu, Ca, Ta and Mg. For example, the high nickel ternary material can be LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0046] In some embodiments, the negative electrode active material is a composition of graphite and silicon material, wherein the silicon material includes at least one of elemental silicon, silicon oxide compound, and silicon carbon composite, wherein the silicon oxide compound can be SiO x(0 < x < 2), where the mass percentage of silicon material in the negative electrode active material is less than or equal to 5%, and can be, for example, 1%, 2%, 3%, 4% or 5%.
[0047] In the above embodiments, due to the increase in the content of silicon material in the negative electrode active material, the potential volume expansion of the negative electrode sheet increases during the charge and discharge cycles of the battery. By adding appropriate fluoroethylene carbonate and additive components to the electrolyte, an SEI film is continuously formed at the interface of the negative electrode active material to prevent the over-expanded negative electrode from damaging the original SEI film layer on the interface and being exposed in the electrolyte, thereby realizing the protection of the negative electrode during the battery cycle. In one example, the mass percentage of fluoroethylene carbonate relative to the electrolyte is any value between 2% and 8%, and the mass percentage of the additive relative to the electrolyte is any value between 0.8% and 2%.
[0048] It should be noted that the structural type of the above secondary battery is not limited. The secondary battery can be any conventional secondary battery on the market, such as a soft-pack battery, a square-shell battery or a cylindrical battery. In some embodiments, the above secondary battery is a cylindrical battery. Due to the different structure of the cylindrical battery from that of the soft-pack and square-shell batteries, the winding tension of the internal electrode assembly is large and the interlayer pressure of the electrode sheet winding is large. It is difficult for the existing electrolyte to simultaneously consider wettability, conductivity and chemical stability under the high interlayer pressure of winding, and thus cannot meet the fast charging requirements of the cylindrical battery. Compared with the existing electrolyte solutions, the electrolyte provided by the present invention has both low viscosity, high conductivity and good chemical stability, can adapt to the fast charging requirements of high volume energy density cylindrical batteries, and improve the cycle performance of the secondary battery under fast charging cycles.
[0049] The technical solutions of the present invention will be described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products, or can be prepared by conventional methods in the art.
[0050] Example 1
[0051] This example provides an electrolyte, and the preparation method of the electrolyte is as follows:
[0052] In an argon atmosphere glove box with a water content of <10ppm, battery-grade ethylene carbonate (EC), propylene carbonate (PC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), ethyl acetate (EA), and methyl acetate (MA) are mixed in corresponding proportions to form a solvent; then 1,3-propylene sultone (PST), vinyl sulfate (DTD) and tetravinylsilane (TVSi) are added to the solvent as additives; finally, lithium hexafluorophosphate (LiPF6) and lithium bis(fluoromethanesulfonyl)imide (LiFSI) are added to the solvent. The contents of the main components of the electrolyte thus configured are shown in Table 1. Taking the total mass of the electrolyte as 100%, the mass percentage of the cyclic carbonate (including EC, PC and FEC) is 16%, wherein the mass percentage of FEC is 5%, and EC and PC not shown in the table always make up the remaining part of the cyclic carbonate in a ratio of 1:1; the mass percentage of EMC as one of the linear carbonates in the electrolyte is 8%, and another linear carbonate DMC not shown in the table is always added in a mass ratio to make up the mass of the entire electrolyte so that the total amount of the electrolyte in each embodiment and comparative example is the same. For example, in this embodiment, the mass percentage of DMC added to the electrolyte is 19.6%; the mass percentage of EA added as a solvent with a viscosity of 0.4 to 0.5 mPa·s is 30%, and the mass percentage of MA added as a solvent with a viscosity of 0.3 to 0.4 mPa·s is 10%; the mass percentage of lithium hexafluorophosphate is 14%, and the mass ratios of lithium bis(fluoromethanesulfonyl)imide and other added additives to the electrolyte are all shown in Table 1.
[0053] Example 2
[0054] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that, in the solvent, ethyl acetate (EA) is replaced by an equal amount of methyl propionate (MP), and methyl acetate (MA) is replaced by an equal amount of methyl formate (MF).
[0055] Example 3
[0056] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the amounts of EC and PC are increased in a ratio of 1:1, so that the total content of cyclic carbonate is increased to 24% of the total mass of the electrolyte.
[0057] Example 4
[0058] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the amounts of EC and PC are reduced in a ratio of 1:1, so that the total content of cyclic carbonate is reduced to 8% of the total mass of the electrolyte.
[0059] Example 5
[0060] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of FEC in the electrolyte is increased to 8%, and the amounts of EC and PC are reduced in a ratio of 1:1 to ensure that the content of cyclic carbonate in the electrolyte is maintained at 16%.
[0061] Example 6
[0062] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of FEC in the electrolyte is reduced to 2%, and at the same time, the amounts of EC and PC are increased in a ratio of 1:1 to ensure that the content of cyclic carbonate in the electrolyte is maintained at 16%.
[0063] Example 7
[0064] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of EMC in the electrolyte is increased to 10%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0065] Example 8
[0066] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of EMC in the electrolyte is reduced to 2%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0067] Example 9
[0068] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of EA in the electrolyte is reduced to 15%, the content of MA in the electrolyte is increased to 15%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0069] Example 10
[0070] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of EA in the electrolyte is increased to 40%, and the content of MA in the electrolyte is reduced to 0%.
[0071] Embodiment 11
[0072] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of EA in the electrolyte is reduced to 15%, the content of MA in the electrolyte is reduced to 5%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0073] Example 12
[0074] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the content of MA in the electrolyte is reduced to 0%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0075] Example 13
[0076] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that, in the electrolyte, the content of LiFSI in the electrolyte is adjusted to 2%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0077] Embodiment 14
[0078] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that, in the electrolyte, the content of LiFSI in the electrolyte is adjusted to 0%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0079] Embodiment 15
[0080] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that, in the electrolyte, the content of the additive DTD in the electrolyte is adjusted to 0.4%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Embodiment 1.
[0081] Example 16
[0082] This embodiment provides an electrolyte of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that, in the electrolyte, the content of the additive PST in the electrolyte is adjusted to 0.5%, the content of the additive TVSi in the electrolyte is adjusted to 0.5%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that in Embodiment 1.
[0083] Comparative Example 1
[0084] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the amounts of EC and PC are increased in a ratio of 1:1, so that the total content of the cyclic carbonate is increased to 30% of the total mass of the electrolyte.
[0085] Comparative Example 2
[0086] This comparative example provides an electrolyte of the same system as Example 1. The difference between this comparative example and Example 1 is that the amounts of EC and PC are reduced in a ratio of 1:1, so that the total content of cyclic carbonate is reduced to 6% of the total mass of the electrolyte.
[0087] Comparative Example 3
[0088] This comparative example provides an electrolyte of the same system as Example 1. The difference between this comparative example and Example 1 is that the content of FEC in the electrolyte is increased to 10%, and the amounts of EC and PC are reduced in a 1:1 ratio to ensure that the content of cyclic carbonate in the electrolyte is maintained at 16%.
[0089] Comparative Example 4
[0090] This comparative example provides an electrolyte of the same system as Example 1. The difference between this comparative example and Example 1 is that the content of FEC in the electrolyte is reduced to 0%, and the corresponding amounts of EC and PC are increased in a ratio of 1:1 to ensure that the content of cyclic carbonate in the electrolyte is maintained unchanged at 16%.
[0091] Comparative Example 5
[0092] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the content of EMC in the electrolyte is increased to 15%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0093] Comparative Example 6
[0094] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the content of EMC in the electrolyte is reduced to 0%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0095] Comparative Example 7
[0096] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the content of EA in the electrolyte is increased to 50%, the content of MA in the electrolyte is reduced to 0%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0097] Comparative Example 8
[0098] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the content of EA in the electrolyte is reduced to 10%, the content of MA in the electrolyte is reduced to 0%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0099] Comparative Example 9
[0100] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the content of EA in the electrolyte is reduced to 15%, the content of MA in the electrolyte is increased to 20%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0101] Comparative Example 10
[0102] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that, in the electrolyte, the content of LiFSI in the electrolyte is adjusted to 3%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0103] Comparative Example 11
[0104] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that, in the electrolyte, the content of the additive DTD in the electrolyte is adjusted to 0.2%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.
[0105] Comparative Example 12
[0106] This comparative example provides an electrolyte of the same system as that of Example 1. The difference between this comparative example and Example 1 is that, in the electrolyte, the content of the additive PST in the electrolyte is adjusted to 0.6%, the content of the additive TVSi in the electrolyte is adjusted to 0.6%, and the content of DMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that in Example 1.
[0107] The electrolytes prepared in Examples 1 to 16 and Comparative Examples 1 to 12 were respectively used in lithium ion batteries to verify the efficacy of the present invention. The preparation process of the lithium ion battery is as follows:
[0108] Preparation of positive electrode sheet: LiNi 0.8 Co 0.1 Mn 0.1O2, the positive electrode conductive agent Super P, and the positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 98:1:1, and the solvent N-methylpyrrolidone is added. Under the action of a vacuum mixer, it is stirred until it becomes uniformly transparent to obtain the positive electrode slurry. The positive electrode slurry is uniformly coated on the aluminum foil. After the aluminum foil is dried at room temperature, it is transferred to an oven for drying, and then through cold pressing and slitting, the positive electrode sheet is obtained.
[0109] Preparation of the negative electrode sheet: The negative electrode active material (97% artificial graphite and 3% silicon oxide SiO x (0 < x < 2)), the negative electrode conductive agent Super P, the negative electrode thickener sodium carboxymethylcellulose (CMC-Na), and the negative electrode binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96:1:1:2. After adding deionized water, it is fully stirred under the action of a vacuum mixer until it is uniform to obtain the negative electrode slurry; the negative electrode slurry is uniformly coated on the negative electrode current collector copper foil, dried at room temperature, and then transferred to an oven for drying, and the negative electrode sheet is obtained through processes such as cold pressing and slitting.
[0110] Selection of the separator: A polypropylene film with a thickness of 12 μm is used as the separator.
[0111] Preparation of the battery: The positive electrode sheet, the separator, and the negative electrode sheet are stacked in sequence, so that the separator is in the middle of the positive electrode sheet and the negative electrode sheet to play a role in isolation, and a bare battery core is obtained by stacking. The positive electrode, the separator, and the negative electrode prepared above are wound into a core in sequence, so that the separator is in the middle of the positive and negative electrodes to play a role in isolation. Then it is installed in a large cylindrical battery case with a size of 4695, 1.7 g / Ah of the above-prepared electrolyte is injected, and then it is sealed, and electrolytic liquefaction is carried out, and finally a cylindrical lithium-ion battery (that is, a lithium-ion battery) is prepared.
[0112] The electrolytes provided in Examples 1 to 16 and Comparative Examples 1 to 12 are subjected to viscosity testing, and the secondary batteries assembled with the electrolytes are subjected to performance testing. Among them, the electrolyte parameters of Examples 1 to 16 and Comparative Examples 1 to 12 are shown in Table 1, and the test results are shown in Table 2. The test methods are as follows:
[0113] (1) Electrolyte viscosity testing: A viscosity tester is used to measure the viscosity of the electrolyte at a temperature of 25°C.
[0114] (2) Fast charging performance testing of the secondary battery: In an oven at a specified temperature (high temperature 45°C), the battery is charged at a current rate of 4C within a test voltage range of 2.5 V (discharge cut-off voltage) to 4.25 V (charge cut-off voltage), and the battery capacity when the negative electrode potential reaches -20 mV is recorded, and the SOC (State Of Charge) of the battery at this time is calculated.
[0115] (3) High-temperature storage performance test of secondary batteries: First, in a test voltage range of 2.5 V (discharge cut-off voltage) to 4.25 V (charge cut-off voltage) at room temperature (room temperature 25°C), the battery is charged and discharged at a current rate of 0.33C and the initial discharge capacity is calculated; then, the battery is charged to full charge at a current rate of 0.33C, and the fully charged battery is placed in an oven at a specified temperature (high temperature 60°C) for storage for 15 days. After that, the battery is taken out and discharged at a current rate of 0.33C and the recovery discharge capacity is calculated; finally, the above process is repeated with a cycle of 15 days until the 120th day, and the ratio of the recovery discharge capacity on the 120th day to the initial discharge capacity is calculated and recorded as the storage capacity recovery rate.
[0116] Table 1: Electrolyte parameters provided in Examples 1 to 16 and Comparative Examples 1 to 12.
[0117]
[0118]
[0119] The contents in Table 1 are all the mass percentages of the components relative to the electrolyte.
[0120] Table 2: Performance test results of the assembled batteries in Examples 1 to 16 and Comparative Examples 1 to 12.
[0121]
[0122]
[0123] It can be seen from the test results of Examples 1 and 2 that, in the electrolyte, solvents from the same viscosity range have similar chemical stabilities and have the same effect on the overall viscosity of the electrolyte. Therefore, replacing the type of solvent in the same viscosity range has little effect on the fast charging performance and high-temperature storage performance of the battery.
[0124] By comparing the test results of Examples 1, 3, and 4 with Comparative Examples 1 and 2, it can be known that when the cyclic carbonate is maintained in an appropriate mass percentage range of 8% to 24% in the electrolyte, the conductivity of the electrolyte can be guaranteed not to decrease while adjusting the low viscosity of the electrolyte. Among them, although the reduction in the content of cyclic carbonate in the electrolyte can reduce the viscosity of the electrolyte, it will also cause the conductivity of the electrolyte to decrease. When the mass percentage of cyclic carbonate in the electrolyte is reduced to below 8%, the fast charging performance of the battery will be deteriorated; at the same time, if the mass percentage of cyclic carbonate in the electrolyte increases to more than 24%, the viscosity of the electrolyte will be too large, thereby deteriorating the fast charging performance of the battery.
[0125] By comparing the test results of Examples 1, 5, 6 and Comparative Examples 3 and 4, it can be seen that when the mass percentage of FEC in the electrolyte is within an appropriate range of 2% to 8%, it can take into account both the high-temperature stability of the electrolyte and the protective effect on the negative electrode interface. When the mass percentage of FEC in the electrolyte is greater than 8%, the excess FEC is easily decomposed at high temperatures to produce hydrogen fluoride, which deteriorates the high-temperature storage performance of the battery; when the mass percentage of FEC in the solvent is less than 2%, too little FEC cannot play the role of negative electrode film formation to protect the negative electrode, which will cause side reactions between the electrolyte and the negative electrode during the cycle, destroying the cycle stability of the battery, and also deteriorating the high-temperature storage performance of the battery.
[0126] By comparing the test results of Examples 1, 7, 8 and Comparative Examples 5 and 6, it can be seen that when the mass percentage of EMC in the electrolyte is within an appropriate range of 2% to 10%, the viscosity of the electrolyte can be avoided from increasing while ensuring the high-temperature stability of the electrolyte, and the fast-charging performance and high-temperature storage performance of the battery can be improved. If the content of EMC in the electrolyte is higher than 10%, the viscosity of the electrolyte will be too high, thereby deteriorating the fast-charging performance of the battery; if the content of EMC in the electrolyte is lower than 2%, the chemical stability of the electrolyte will be deteriorated, causing the high-temperature storage capacity recovery rate of the battery to significantly decay.
[0127] By comparing the test results of Examples 1, 9 to 12 and Comparative Examples 7 to 9, it can be known that the content of carboxylates with different viscosities will significantly affect the fast charging performance and high-temperature storage performance of the battery. Among them, the higher the amount of low-viscosity carboxylate solvent used, the stronger the fast charging ability of the battery, and the same content of low-viscosity carboxylates can improve the fast charging ability of the battery much more than high-viscosity carboxylates. Therefore, increasing the amount of low-viscosity components in carboxylates can reduce the total amount of carboxylates in the electrolyte, and can make the viscosity of the electrolyte at a lower level; however, as the amount of low-viscosity carboxylates increases, the overall chemical stability of the electrolyte decreases, which will deteriorate the high-temperature storage performance of the battery. Therefore, the carboxylate content in the electrolyte is limited to less than 15%, and the total carboxylate amount is maintained below 40% to maintain the high-temperature storage performance of the battery.
[0128] Comparison of the test results of Examples 1, 13, 14 and Comparative Example 10 shows the necessity of limiting the LiFSI content in the electrolyte. When the mass percentage of LiFSI in the electrolyte is higher than 2%, LiFSI will cause serious corrosion to the current collector, affecting the reliability of the battery.
[0129] By comparing the test results of Examples 1, 15, 16 and Comparative Examples 11 and 12, it can be known that when the total content of the additive in the electrolyte is within an appropriate range of 0.8% to 2%, it can promote the formation of the SEI film at the negative electrode interface without excessively increasing the impedance of the battery. When the mass percentage of the additive in the electrolyte is lower than 0.8%, the SEI film at the negative electrode interface will not form sufficiently, making it difficult to effectively protect the negative electrode, thereby negatively affecting the battery's cycle capacity; when the mass percentage of the additive in the electrolyte is higher than 2%, the impedance of the SEI film at the negative electrode interface will be too high, which will have a negative impact on the battery's fast charging performance.
[0130] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. An electrolyte, characterized in that: include: Lithium salts; a solvent, the solvent comprising cyclic carbonates, linear carbonates and carboxylates; Among them, the mass percentage of the cyclic carbonate relative to the electrolyte is 8% to 24%, the linear carbonate includes dimethyl carbonate and at least one of ethyl methyl carbonate and diethyl carbonate, the sum of the masses of the ethyl methyl carbonate and the diethyl carbonate relative to the electrolyte is 2% to 10%, the mass percentage of the carboxylic acid ester relative to the electrolyte is 20% to 40%, the carboxylic acid ester includes a first component and a second component, the viscosity of the first component at 25±2°C is 0.4~0.5mPa·s, the viscosity of the second component at 25±2°C is 0.3~0.4mPa·s, the mass percentage of the first component relative to the electrolyte is 15% to 40%, and the mass percentage of the second component relative to the electrolyte is 0% to 15%.
2. The electrolyte according to claim 1, characterized in that The first component includes one or more of ethyl acetate, methyl propionate, propyl acetate, and ethyl propionate, and the second component includes one or more of methyl acetate, ethyl formate, and methyl formate.
3. The electrolyte according to claim 1, characterized in that: The cyclic carbonate includes fluoroethylene carbonate and at least one of ethylene carbonate and propylene carbonate.
4. The electrolyte according to claim 3, characterized in that The mass percentage of the fluoroethylene carbonate relative to the electrolyte is 2% to 8%.
5. The electrolyte according to claim 1, characterized in that The linear carbonates include dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
6. The electrolyte according to claim 1, characterized in that The electrolyte further includes an additive, wherein the additive includes 1,3-propylene sultone, vinyl sulfate and tetravinylsilane, and the mass percentage of the additive relative to the electrolyte is 0.8% to 2%.
7. The electrolyte according to claim 1, characterized in that The lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide. The mass percentage of the lithium salt relative to the electrolyte is 8% to 20%, and the mass percentage of the lithium bis(fluorosulfonyl)imide relative to the electrolyte is 0% to 2%.
8. A secondary battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte according to any one of claims 1 to 7.
9. The secondary battery according to claim 8, characterized in that: The secondary battery is a cylindrical battery.
10. The secondary battery according to claim 8, characterized in that: The upper limit of the working voltage of the secondary battery is higher than 4.15V.