Curable compositions, treated backing, coated abrasive articles including same, and methods of making and using same

By preparing treated backings using specific curable compositions, the problem of insufficient separation and curing of abrasive layers from the backing is solved, and the abrasive performance and stability of coated abrasive articles are improved.

CN118900747APending Publication Date: 2024-11-053M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028858.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing coated abrasive products are separated from the backing due to friction heating during use, and the radically polymerized compositions have insufficient curing and deteriorated abrasive properties due to oxygen inhibition.

Method used

A curable composition is adopted, comprising 45-80% epoxy resin, 6-12% trifunctional (meth)acrylate, 5-45% polythiol, 0-10% dicyandiamide, 0.1-2% free radical photoinitiator, 0.5-1% 2-alkylimidazole and 0-5% phenolic resin were prepared by reaction of epichlorohydrin with bisphenol A or bisphenol F for preparation and treatment. and partially cured on the backing to improve adhesion and antioxidant properties.

Benefits of technology

Excellent backing flatness and adhesion are achieved, the curing stability and abrasive properties of the abrasive layer are improved, and the risk of separation between the abrasive layer and the backing is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900747A_ABST
    Figure CN118900747A_ABST
Patent Text Reader

Abstract

A curable composition comprising from 45% to 80% by weight of an epoxy resin, the epoxy resin being capable of being prepared by reacting an epichlorohydrin with at least one of bisphenol A or bisphenol F; from 6% to 12% by weight of an at least trifunctional (meth) acrylate; from 5% to 45% by weight of a polythiol; 0% to 10% by weight of dicyandiamide; 0.1% to 2% of a free radical photoinitiator; from 0.5 wt% to 1 wt% of a 2-alkyl imidazole; and 0% to 5% of a phenolic resin. The curable composition can be used to prepare a treated backing, which can be incorporated into a coated abrasive article and used to abrade a workpiece.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Generally speaking, coated abrasive articles have abrasive grains fixed to a backing. More typically, a coated abrasive article includes a backing having two opposing major surfaces and an abrasive layer fixed to one major surface. The abrasive layer generally comprises abrasive grains and a binder, wherein the binder is used to fix the abrasive grains to the backing.

[0002] A common type of coated abrasive product has an abrasive layer including a base coat, a size coat and abrasive grains. When manufacturing such coated abrasive products, a base coat comprising a base coat precursor is applied to the main surface of the backing. The abrasive grains are then at least partially embedded in the base coat precursor (e.g., via electrostatic coating), and the base coat precursor is fully cured (i.e., cross-linked) to fix the particles to the cured base coat precursor (i.e., base coat). The size coat precursor is then applied to the base coat and abrasive grains, and the size coat precursor is then at least partially cured to provide a size coat. Some coated abrasive products also include a top coat covering the abrasive layer. The top coat generally includes a grinding aid and / or an anti-filling material.

[0003] Another common type of coated abrasive article includes an abrasive layer fixed to a major surface of a backing, wherein the abrasive layer is provided by applying a slurry consisting of a curable binder precursor (which includes a curable composition) and abrasive particles to the major surface of the backing and then curing the binder precursor.

[0004] Some coated abrasive articles also include a backing treatment, such as a backsize layer (i.e., a coating on the major surface of the backing opposite the major surface having the abrasive layer), a presize layer, a bonding layer (i.e., a coating between the abrasive layer and the major surface to which the abrasive layer is attached), and / or an impregnant. Optionally, the backing may also include a subsize layer treatment. A subsize layer is similar to an impregnant, except that it is applied to a previously treated backing.

[0005] Conventional backing treatments for coated abrasive constructions include soluble phenolic resins, phenolic / latex blends, urea-formaldehyde and melamine-formaldehyde resins. Backing treatments (such as these) typically show good adhesion to resol phenolic, urea-formaldehyde and epoxy-based primer layers and slurry layers. However, since these types of backing treatments are typically only partially cured before primer coating is applied, they typically emit various volatiles such as water, phenol and formaldehyde, which can impart additional porosity, particles and / or hinder the curing of the primer layer to the abrasive layer. During use, the temperature of the coated abrasive typically rises due to friction heating. Whether the backing is processed or not, this type of heating can all cause problems, such as separation of the abrasive layer from the backing.

[0006] Free radical polymerizable compositions have been included in backing treatments that can be polymerized using electromagnetic radiation (e.g., ultraviolet (UV) and / or visible light). However, free radical polymerization can be inhibited by oxygen in the air, resulting in an undercured surface and degraded abrasive properties. In addition, significant shrinkage of the free radical polymerizable composition can occur, resulting in stress accumulation and curling of the backing. Summary of the invention

[0007] Advantageously and unexpectedly, the method of making treated backings according to the present disclosure provides excellent backing flatness and adhesion to resol phenolic, urea formaldehyde, and epoxy based make coats, and the formulations exhibit good resistance to surface oxygen inhibition.

[0008] In one aspect, the present disclosure provides a curable composition comprising, based on the total weight of components a) to g),

[0009] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0010] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0011] c) 5 to 45% by weight of polythiol;

[0012] d) 0 to 10% by weight of dicyandiamide;

[0013] e) 0.1% to 2% of a free radical photoinitiator;

[0014] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0015] g) 0% to 5% phenolic resin.

[0016] In another aspect, the present disclosure provides a treated backing comprising a fabric having a backing treatment contacting at least a portion of the fabric, wherein the backing treatment comprises the reaction product of a curable composition comprising, based on the total weight of components a) through g):

[0017] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0018] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0019] c) 5 to 45% by weight of polythiol;

[0020] d) 0 to 10% by weight of dicyandiamide;

[0021] e) 0.1% to 2% of a free radical photoinitiator;

[0022] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0023] g) 0% to 5% phenolic resin.

[0024] In yet another aspect, the present disclosure provides a method of making a treated backing, the method comprising:

[0025] Contacting at least a portion of the fabric with a curable composition preparable from components comprising, based on the total weight of components a) to g),

[0026] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0027] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0028] c) 5 to 45% by weight of polythiol;

[0029] d) 0 to 10% by weight of dicyandiamide;

[0030] e) 0.1% to 2% of a free radical photoinitiator;

[0031] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0032] g) 0% to 5% phenolic resin; and

[0033] The curable composition is at least partially cured.

[0034] In yet another aspect, the present disclosure provides a coated abrasive article comprising an abrasive layer secured to a major surface of a treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder, wherein the treated backing comprises at least one of a presize layer, an impregnant or subsize layer, or a bonding layer, the treated backing comprising a reaction product of components, based on the total weight of components a) to g), comprising:

[0035] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0036] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0037] c) 5 to 45% by weight of polythiol;

[0038] d) 0 to 10% by weight of dicyandiamide;

[0039] e) 0.1% to 2% of a free radical photoinitiator;

[0040] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0041] g) 0% to 5% phenolic resin.

[0042] In one embodiment, the abrasive layer includes a make layer and a size layer.

[0043] In another embodiment, the abrasive layer comprises abrasive particles dispersed in a binder.

[0044] In yet another aspect, the present disclosure provides a method of making a coated abrasive article, the method comprising:

[0045] A curable backing treatment precursor is disposed on at least a portion of the backing, the curable backing treatment precursor comprising the following components, based on the total weight of components a) to g):

[0046] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0047] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0048] c) 5 to 45% by weight of polythiol;

[0049] d) 0 to 10% by weight of dicyandiamide;

[0050] e) 0.1% to 2% of a free radical photoinitiator;

[0051] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0052] g) 0% to 5% phenolic resin; and

[0053] at least partially curing the curable backing treatment precursor to provide a treated backing; and

[0054] An abrasive layer is secured to the major surface of the treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder.

[0055] The coated abrasive according to the present disclosure can be used to grind a workpiece by the following method, which comprises:

[0056] Providing a coated abrasive article according to the present invention;

[0057] frictionally contacting at least a portion of the abrasive layer with at least a portion of a surface of a workpiece; and

[0058] At least one of the coated abrasive article or the workpiece is moved relative to the other to abrade at least a portion of the surface.

[0059] As used in this article:

[0060] "Substantially free" means containing less than one weight percent (e.g., less than 0.1 weight percent, 0.01 weight percent, or 0 weight percent) of the following;

[0061] "(Meth)acryloyl" refers to methacryloyl and / or acryloyl groups (i.e. ) and / or and

[0062] "Weight %" and "weight percent" are interchangeable. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 is a cross-sectional side view of an exemplary coated abrasive article according to the present disclosure;

[0064] Figure 2 is a cross-sectional side view of another exemplary coated abrasive article according to the present disclosure; and

[0065] Figure 3 is a cross-sectional side view of another exemplary coated abrasive article according to the present disclosure. DETAILED DESCRIPTION

[0066] The curable composition according to one aspect of the present disclosure comprises, based on the total weight of components a) to g):

[0067] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0068] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0069] c) 5 to 45% by weight of polythiol;

[0070] d) 0 to 10% by weight of dicyandiamide;

[0071] e) 0.1% to 2% of a free radical photoinitiator;

[0072] f) 0.5 wt % to 1 wt % of an imidazole curing agent; and

[0073] g) 0% to 5% phenolic resin.

[0074] Based on the total weight of components a) to g), the curable composition according to the present disclosure includes 45% to 80% by weight of at least one epoxy resin, which can be prepared by reacting at least one of epichlorohydrin and bisphenol A or bisphenol F; however, in some embodiments, based on the total weight of components a) to g), the composition according to the present disclosure may include 45% to 55% by weight or 70% to 80% by weight of at least one epoxy resin, which can be prepared by reacting at least one of epichlorohydrin and bisphenol A or bisphenol F. Typically, the average epoxy functionality of such resins is 2, but higher and lower functionality is also available. The epoxy resin can be liquid or solid. Whether liquid or solid, the epoxy resin can be selected to be soluble in the composition according to the present disclosure. In some cases, heating the composition according to the present disclosure can promote the dissolution of the epoxy resin.

[0075] Examples of useful epoxy resins include epoxy resins formed by reacting bisphenol A or bisphenol F with epichlorohydrin, and mixtures of such resins. Examples of bisphenol A-epichlorohydrin derived epoxy resins, bisphenol A diglycidyl ether (commonly referred to in the art as DGEBA), and bisphenol F diglycidyl ether, as well as commercially available epoxy resins having the trade name EPON (e.g., EPON RESIN 825, EPON 828, EPON RESIN 828, EPON RESIN 1001F, EPON RESIN 1002F, EPON RESIN 1004F, EPON RESIN 1009F, and EPON RESIN 2003), which are sold by Hexion, Columbus, Ohio, and many epoxy resins having the trade name DER (e.g., DER 331, DER 332, DER 351, DER 352, DER 354, and DER 356), which are sold by Olin Chemical Company, Clayton, Missouri.

[0076] Based on the total weight of components a) to g), the curable composition according to the present disclosure comprises 6 to 12 weight % of at least one at least trifunctional (meth)acrylate. The phrase "at least one trifunctional (meth)acrylate" means a compound comprising at least three (e.g., at least 3, 4 or even 5) (meth)acryloyloxy groups. For example, based on the total weight of components a) to g), the curable composition according to the present disclosure may comprise 6 to 10 weight % or 9 to 12 weight % of multifunctional urethane (meth)acrylate. Blends of more than one trifunctional (meth)acrylate may also be used.

[0077] Exemplary useful at least trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, sorbitol tri(meth)acrylate, sorbitol hexa(meth)acrylate, and mixtures thereof.

[0078] Based on the total weight of components a) to f), the curable composition according to the present disclosure comprises 5 wt % to 45 wt % of at least one polythiol (i.e., organic polythiol). In some embodiments, based on the total weight of components a) to f), the composition may comprise 5 wt % to 15 wt % or even 35 wt % to 45 wt % of one or more polythiols. The polythiol may have 2, 3, 4, 5, 6, 7, 8 or more thiol (-SH) groups.

[0079] Examples of polythiols having more than two thiol groups include propane-1,2,3-trithiol; 1,2-bis[(2-mercaptoethyl)thio]-3-mercaptopropane; tetrakis(7-mercapto-2,5-dithioheptyl)methane; and trithiocyanic acid.

[0080] Exemplary useful dithiols include 1,2-ethanedithiol, 1,2-propanedithiol, 1,3-propanedithiol, 1,3-butanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,3-pentanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,3-dimercapto-3-methylbutane, dipentenedithiol, ethylcyclohexyldithiol (ECHDT), dimercaptodiethyl sulfide, methyl-substituted dimercaptodiethyl sulfide, dimethyl-substituted dimercaptodiethyl sulfide, dimercaptodioxaoctane, 1,5-dimercapto-3-oxapentane, benzene-1,2-dithiol, benzene-1,3-dithiol, benzene-1,4-dithiol, and toluene-2,4-dithiol. Examples of polythiols having more than two thiol groups include propane-1,2,3-trithiol; 1,2-bis[(2-mercaptoethyl)thio]-3-mercaptopropane; tetrakis(7-mercapto-2,5-dithioheptyl)methane; and trithiocyanic acid.

[0081] Also useful polythiols include polythiols formed by esterification reactions of polyols with thiol-containing carboxylic acids or their derivatives. Examples of polythiols formed by esterification reactions of polyols with thiol-containing carboxylic acids or their derivatives include those made by esterification reactions between thioglycolic acid or 3-mercaptopropionic acid and several polyols to form thioglycolic acid esters or mercaptopropionic esters, respectively.

[0082] Examples of polythiol compounds that may be preferred due to relatively low odor levels include, but are not limited to, esters of thioglycolic acid, α-mercaptopropionic acid, and β-mercaptopropionic acid with polyols (polyols), such as diols (e.g., ethylene glycol), triols, tetraols, pentaols, and hexaols. Specific examples of such polythiols include, but are not limited to, ethylene glycol bis(thioglycolic acid), ethylene glycol bis(β-mercaptopropionic acid), trimethylolpropane tris(thioglycolic acid), trimethylolpropane tris(β-mercaptopropionic acid) and their ethoxylated versions, pentaerythritol tetra(thioglycolic acid), pentaerythritol tetra(β-mercaptopropionic acid), and tris(hydroxyethyl)isocyanurate tris(β-mercaptopropionic acid). However, these polyols are generally less desirable in applications where there is concern about possible hydrolysis of the esters.

[0083] Suitable polythiols also include those commercially available from Bruno Bock Chemische Fabrik GmbH & Co. KG. as THIOCURE PETMP (pentaerythritol tetrakis(3-mercaptopropionate), TMPMP (trimethylolpropane tris(3-mercaptopropionate), ETTMP (ethoxylated trimethylolpropane tris(3-mercaptopropionate), such as ETTMP 1300 and ETTMP 700), GDMP (ethylene glycol di(3-mercaptopropionate), TMPMA (trimethylolpropane tris(thioglycolate)), TEMPIC (tris[2-(3-mercaptopropionyloxy)ethyl]isocyanurate), and PPGMP (propylene glycol 3-mercaptopropionate). A specific example of the polymer polythiol is polypropylene ether glycol bis(β-mercaptopropionate), which is prepared by an esterification reaction of polypropylene ether glycol (eg, PLURACOL P201, Wyandotte Chemical Corp.) and β-mercaptopropionic acid.

[0084] Suitable polythiols also include those that can be prepared by esterification of a polyol with a thiol-containing carboxylic acid or a derivative thereof, those prepared by the ring-opening reaction of an epoxide with H2S (or its equivalent), those prepared by the addition of H2S (or its equivalent) to a carbon-carbon double bond, polysulfides, polythioethers and polydiorganosiloxanes. Specifically, these include 3-mercaptopropionic acid esters (also known as β-mercaptopropionic acid esters) of ethylene glycol and trimethylolpropane (the former from Chemische Fabrik GmbH & Co. KG and the latter from Sigma-Aldrich); POLYMERCAPTAN 805C (thiolated castor oil); POLYMERCAPTAN 407 (mercaptohydroxy soybean oil) from Chevron Phillips Chemical Co. LLP, and CAPCURE, particularly CAPCURE 3-800 (a polyoxyalkylene triol having mercapto terminal groups), from Gabriel Performance Products, Ashtabula, Ohio, and GPM-800, which is equivalent to CAPCURE 3-800, also from Gabriel Performance Products.

[0085] Oligomeric or polymeric polythioether polythiols useful in practicing the present disclosure are also described, for example, in U.S. Pat. Nos. 4,609,762 (Morris et al.), 5,225,472 (Cameron et al.), 5,912,319 (Zook et al.), 5,959,071 (DeMoss et al.), and 6,509,418 (Zook et al.).

[0086] In some embodiments, polythiols are oligomeric or polymeric. Examples of available oligomeric or polymeric polythiols include polythioethers and polysulfides. Polythioethers include thioether bonds (i.e., -S-) in their backbone structures. Polysulfides include disulfide bonds (i.e., -SS-) in their backbone structures.

[0087] Other useful polythiols can be formed by the addition of hydrogen sulfide (H2S) (or its equivalent) to carbon-carbon double bonds. For example, dipentenes and triglycerides that have been reacted with H2S (or its equivalent). Specific examples include dipentene dithiol and those polythiols available from Chevron Phillips Chemical Co. LLP as POLYMERCAPTAN 358 (thiolated soybean oil) and POLYMERCAPTAN 805C (thiolated castor oil). Preferred polythiols, at least for some applications, are POLYMERCAPTAN 358 and 805C because they are made largely from renewable materials (i.e., triglycerides, soybean oil, and castor oil) and have relatively low odor compared to many mercaptans. Useful triglycerides have an average of at least two unsaturated sites per molecule, i.e., carbon-carbon double bonds, and sufficient sites are converted to have an average of at least 2 mercaptans per molecule. For soybean oil, this requires about 42% or more of the carbon-carbon double bonds to be converted, and for castor oil, this requires about 66% or more of the carbon-carbon double bonds to be converted. Higher conversions are generally preferred, and POLYMERCAPTAN 358 and 805C are available with conversions greater than about 60% and 95%, respectively. Useful polythiols of this type also include those derived from the reaction of H2S (or its equivalent) with glycidyl ethers of bisphenol A epoxy resins, bisphenol F epoxy resins, and thermoplastic novolac epoxy resins. A preferred polythiols of this type are QX11, derived from bisphenol A epoxy resins, available from Japan Epoxy Resins (JER) as EPOMATE. Other suitable polythiols include those available from JER as EPOMATE QX10 and EPOMATE QX20.

[0088] Other useful polythiols are polysulfides containing thiol groups, such as those available from Toray Fine Chemicals Co., Ltd as THIOKOL LP-2, LP-3, LP-12, LP-31, LP-32, LP-33, LP-977, and LP-980, and polythioether oligomers and polymers, such as those described in PCT Publication No. WO 2016 / 130673 A1 (DeMoss et al.).

[0089] According to the curable composition of the present disclosure, an optional amount of dicyandiamide is included to accelerate the curing of the curable composition. For example, based on the total weight of components a) to g), the curable composition may include greater than or equal to 0% by weight to 10% by weight of dicyandiamide. Dicyandiamide has a variety of commercial sources, such as Air Products and Chemicals, Allentown, Pennsylvania, sold as AMICURE CG-1200 and AMICURE CG-1400.

[0090] The curable composition according to the present disclosure comprises an effective amount of a photoinitiator for curing the composition. For example, based on the total weight of components a) to g), the curable composition may comprise 0.1 wt % to 2 wt % or 0.3 wt % to 1 wt % of a free radical photoinitiator.

[0091] The free radical photoinitiator that can be used can be a single photoinitiator, or a combination of two or more photoinitiators. Photoinitiators that can be used to practice the present disclosure include those known for free radical photocuring (meth) acrylates. Exemplary photoinitiators include benzoin and its derivatives, such as α-methylbenzoin; α-phenylbenzoin; α-allylbenzoin; α-benzylbenzoin; benzoin ethers, such as benzil dimethyl ketal, benzoin methyl ether, benzoin ethyl ether, benzoin n-butyl ether; acetophenone and its derivatives, such as 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone and 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone.

[0092] The curable composition according to the present disclosure contains 0.5 wt % to 1 wt % of a 2-alkylimidazole (epoxy curing agent), such as, for example, 2-ethylimidazole and 2-ethyl-4-methylimidazole (e.g., sold as IMICURE EMI-2,4 by Air Products & Chemicals, Allentown, Pa.) and 2-propylimidazole (e.g., sold under the trade name CUREMOD 2-PI-60LIQ by Near Chemical Specialties Inc., Buffalo Grove, Illinois).

[0093] Based on the total weight of components a) to g), the curable composition according to the present disclosure includes 0 wt % to 5 wt % (i.e., it is optional) of a phenolic resin. In some embodiments, based on the total weight of components a) to g), 4 wt % to 5 wt %. Useful phenolic resins may include thermoplastic novolac resins and / or resol phenolic resins.

[0094] Usually, thermoplastic novolac resin is made by reacting phenolic monomers (for example phenol, cresol, xylenol, resorcinol, catechol, bisphenol A, naphthol or their combination) with aldehyde in the presence of an acid catalyst, wherein the molar ratio of aldehyde to phenol is less than one. The example of aldehyde for preparing thermoplastic novolac resin comprises formaldehyde, acetaldehyde, propionaldehyde, glyoxal and furfural. Usually, these thermoplastic novolac resins have a molecular weight in the range of 300 to 1500, although higher and lower molecular weights may also be available. In addition, the starting phenolic monomers may be substituted by various groups (such as alkyl, alkoxy, carboxyl and sulfo group), as long as at least two reactive sites are retained to form thermoplastic novolac resin.

[0095] Many thermoplastic phenolic resins are readily available from commercial suppliers, including, for example, Georgia Pacific Resins, Atlanta, Georgia (e.g., sold under the trade names "GP 2074," "GP 5300," "GP 5833," "RESI-FLAKE GP-2049," "RESI-FLAKE GP-2050," or "RESI-FLAKE GP-2211"); Bakelite AG, Frielendorf, Germany (e.g., sold under the trade name "RUTAPHEN 8656F"); Borden Chemical, Inc. (e.g., sold under the trade name "DURITE 423A" or "DURITE SD1731"). While thermoplastic phenolic resins are generally useful, resole phenolic resins may tend to interfere with the cure of curable compositions according to the present invention and, if included, should be used with caution.

[0096] The curable composition according to the present disclosure may also include an optional dual reactive polymerizable component, for example, a compound having at least one free radical polymerizable group and at least one cationically polymerizable group. The dual reactive compound may be made, for example, by introducing at least one ethylenically unsaturated group into a compound that already contains one or more epoxy groups, or vice versa.

[0097] The curable composition according to the present disclosure may contain various additives such as, for example, fillers, thickeners, toughening agents, grinding aids, pigments, fibers, tackifiers, lubricants, wetting agents, surfactants, defoamers, dyes, coupling agents, plasticizers, and suspending agents.

[0098] In applications where low viscosity is desired, such as, for example, as a backing treatment, the curable compositions according to the present disclosure can be substantially free of dissolved thermoplastic polymers (e.g., thermoplastic polymers having a weight average molecular weight of 5,000 or greater), as such materials tend to greatly increase viscosity, which can make the coating process difficult (e.g., saturating a porous backing).

[0099] The curable compositions according to the present disclosure can be applied to a variety of substrates using conventional methods such as, for example, roller coating (e.g., using a soft rubber roller), spraying, transfer coating, dip coating, screen printing, gravure coating, curtain coating, rod coating, blade coating, or die coating. The curable composition can be applied to the substrate in a uniform or patterned manner and can be continuous or discontinuous.

[0100] If a curable composition comprising solid components is utilized, such a composition can be prepared, for example, by mixing some or all of the various materials of the curable composition in a suitable container under stirring conditions to form the curable composition without thermally decomposing the components, and the mixing is also carried out at an elevated temperature (e.g., less than 100° C.) sufficient to liquefy at least some of the materials so that they can be effectively mixed.

[0101] The curable composition can be cured by exposure to thermal energy, actinic radiation, or more typically a combination thereof. In such cases, the curing of the curable composition generally begins after exposing it to an appropriate source of actinic radiation (e.g., ultraviolet radiation, visible radiation, or particulate radiation), and can continue for a period of time thereafter.

[0102] Useful forms of heat energy include, for example, thermal radiation and infrared radiation. Exemplary sources of heat energy include ovens, heated rollers, hot air blowers, infrared lamps, and combinations thereof.

[0103] The source of actinic radiation is generally selected based on the expected processing conditions and is selected to appropriately activate the photoinitiator. Exemplary useful sources of ultraviolet and visible radiation include mercury lamps, xenon lamps, carbon arc lamps, tungsten filament lamps, and sunlight. Ultraviolet radiation, especially from medium pressure mercury arc lamps or microwave driven H-type, D-type, or V-type mercury lamps, such as those available from Fusion UV Systems, Gaithersburg, Maryland, is particularly desirable.

[0104] Depending on the amount and type of reactive components involved, the energy source, the web speed, the distance from the energy source, and the thickness of the make layer precursor to be cured, the exposure time for actinic radiation is generally in the range of, for example, less than about 0.01 seconds to 1 minute or more to obtain, for example, 0.1 Joule / square centimeter (J / cm 2 ) to 10 J / cm2 total energy exposure. Filters and / or dichroic reflectors, for example, may also be used to reduce the thermal energy associated with the actinic radiation.

[0105] If electron beam radiation is used, the required dose is typically less than 1 Mrad to 100 Mrads or more.

[0106] The curable composition according to the present disclosure can be applied to a backing, for example, as a treated backing in the manufacture of a coated abrasive article. Such treated backings are typically prepared by applying a curable composition according to the present disclosure (i.e., a backing treatment precursor) to at least a portion of the backing and at least partially curing the curable composition. For example, if the backing has two opposing major surfaces, the curable composition can be applied in a manner that contacts only one of the major surfaces or in a manner that contacts both major surfaces (e.g., by saturating the fabric with the curable composition or simultaneously applying the curable composition to each major surface of the backing).

[0107] Useful backings include, for example, fabrics (such as nonwovens, for example, nonwoven fabrics including needle punching, melt spinning, spunbonding, hydroentangled or meltblown), knitted fabrics, stitch-bonded fabrics and woven fabrics (e.g., cloth); paper; mesh; polymer films (including primed films), such as polyolefin films (e.g., polypropylene including biaxially oriented polypropylene, polyester films, polyamide films, cellulose ester films); foils; foams (e.g., natural sponge materials or polyurethane foams); combinations of two or more of these materials; and treated forms thereof. The backing may also be a laminate of two materials (e.g., paper / film, cloth / paper, film / cloth).

[0108] Available fiber backing can be made of any known fiber, whether natural fiber, synthetic fiber, or blend of natural fiber and synthetic fiber. The example of available fiber material includes fiber or yarn comprising the following substances: polyester (for example, polyethylene terephthalate), polyamide (for example, hexamethylene adipamide, polycaprolactam), polypropylene, acrylic (formed by acrylonitrile polymer), cellulose acetate, polyvinylidene chloride-vinyl chloride copolymer, vinyl chloride-acrylonitrile copolymer, graphite, polyimide, silk, cotton, flax, jute, hemp or rayon. Available fiber can have natural material, or have recycled material or waste material recovered from clothing cutting, carpet manufacturing, fiber manufacturing or textile processing, for example. Available fiber can be homogenized or can be composite material, such as bicomponent fiber (for example, cospun sheath-core fiber). Fiber can be stretched and curled, but can also be continuous filament, such as those filaments formed by extrusion process.

[0109] The treated backing according to the present disclosure is generally flexible. The thickness of the backing is generally in the range of about 0.02 mm to about 5 mm, advantageously in the range of about 0.05 mm to about 2.5 mm, and more advantageously in the range of about 0.1 mm to about 0.4 mm, but thicknesses outside these ranges can also be used, for example, according to the intended use. The strength of the backing should be sufficient to resist tearing or other damage in use. The thickness and smoothness of the backing should also be suitable for providing the required thickness and smoothness of the coated abrasive article, wherein these characteristics of the coated abrasive article may vary depending on, for example, the intended application or use of the coated abrasive article.

[0110] The treated backing can have any basis weight. Treated backings comprising fabrics having a basis weight in the range of 100 g / m2 to 550 g / m2 generally have good flexibility and are well suited for inclusion in coated abrasive articles, however higher and lower basis weights may also have good flexibility. Examples of such treated backings include those comprising fabrics having a basis weight in the range of 200 g / m2 to 400 g / m2, and those having a basis weight in the range of 250 g / m2 to 370 g / m2.

[0111] The amount of curable composition applied to the backing can be any amount, again depending on the particular application.

[0112] The curable compositions and treated backings according to the present disclosure can also be used in the manufacture of coated abrasive articles, where they can provide good adhesion between the abrasive layer and the backing.

[0113] Figure 1 One such coated abrasive article is shown in FIG. Figure 1 , the exemplary coated abrasive article 100 includes a backing 112. The backing 112 may optionally be saturated with an impregnant 111. In addition, the backing 112 may be treated with an optional backsize layer 113 and / or an optional presize layer 115. In the case where the backing 112 is porous, the backsize layer 113 and the presize layer 115 penetrate into the backing and, in some cases, may even contact each other in the porous interior of the backing. An abrasive layer 114 covers the presize layer 115, and the abrasive layer includes a base size layer 116 in which abrasive gravels 118 are embedded, and a size layer 117 covering the base size layer 116 and the abrasive gravels 118. An optional top size layer 119 covers the size layer 117.

[0114] Another exemplary coated abrasive article according to the present disclosure Figure 2 Now see Figure 2, the coated abrasive article 200 includes a backing 212. The backing 212 is treated with at least one of an impregnant 211 or a presize layer 215. In addition, the backing 212 can be treated with an optional backsize layer 213. In the case where the backing 212 is porous, the backsize layer 213 and the presize layer 215 penetrate into the backing, and in some cases, may even contact each other in the porous interior of the backing. An abrasive layer 214 covers the presize layer 215, and the abrasive layer includes a plurality of abrasive gravels 218 distributed throughout the binder 209.

[0115] The reaction product according to the curable composition of the present disclosure can be used as a backing treatment material, for example, as one or more of an impregnating agent, a sub-gel layer, a pre-gel layer or a backing layer. The purpose of these materials is generally to seal the backing, protect the yarn or fiber in the backing, and / or promote the adhesion of other layers to the backing. If the backing is a fabric, at least one material in these materials is generally used. The addition of a pre-gel layer or a backing layer can cause a "smoother" surface on the front and / or back side of the backing in addition.

[0116] For use in coated abrasive articles, the backing typically has a thickness in the range of 0.02 mm to 5 mm, such as in the range of 0.05 mm to 2.5 mm, or in the range of 0.1 mm to 1 mm, although thicknesses outside of these ranges can be used.

[0117] The backing may also be a laminate of two materials (e.g., paper / film, cloth / paper, or film / cloth). The backing may also be a fiber-reinforced thermoplastic, such as described, for example, in U.S. Pat. No. 5,417,726 (Stout et al.), or an endless belt, such as described, for example, in U.S. Pat. No. 5,573,619 (Benedict et al.), the disclosure of which is incorporated herein by reference.

[0118] The backing can be a polymeric substrate (having hook rods protruding therefrom), such as, for example, a polymeric substrate described in U.S. Pat. No. 5,505,747 (Chesley et al.), or the backing can be a loop fabric, such as, for example, a loop fabric described in U.S. Pat. No. 5,565,011 (Follett et al.), the disclosure of which is incorporated herein by reference.

[0119] The choice of backing material may depend on the intended application of the coated abrasive article. The thickness and smoothness of the backing should also be suitable to provide the desired thickness and smoothness of the coated abrasive article, wherein these characteristics of the coated abrasive article may vary depending on, for example, the intended application or use of the coated abrasive article.

[0120] Antistatic materials can be included in any of these backing treatment materials. The addition of antistatic materials can reduce the tendency of coated abrasive articles to accumulate static electricity when sanding wood or wood-like materials. Additional details about antistatic backings and backing treatments can be found in, for example, U.S. Pat. Nos. 5,108,463 (Buchanan et al.), 5,137,542 (Buchanan et al.), 5,328,716 (Buchanan), and 5,560,753 (Buchanan et al.), the disclosures of which are incorporated herein by reference.

[0121] In some cases, it may be desirable to bond a pressure sensitive adhesive to the back side of the coated abrasive article so that the resulting coated abrasive article can be secured to a back-up pad. Exemplary pressure sensitive adhesives include latex crepe, rosin, acrylic polymers and copolymers including polyacrylates (e.g., poly(butyl acrylate)), vinyl ethers (e.g., poly(n-butyl vinyl ether)), alkyd adhesives, rubber adhesives (e.g., natural rubber, synthetic rubber, chlorinated rubber), and mixtures thereof.

[0122] To promote adhesion of the binder resin to the backing, one or more surfaces of the backing may be modified by known methods, including corona discharge, ultraviolet light exposure, electron beam exposure, flame discharge, and / or roughening.

[0123] The basis weight of the make coat used may vary depending on, for example, the intended use, the type of abrasive grain, and the nature of the coated abrasive article being prepared, but is generally in the range of 1 gram per square meter (i.e., g / m 2 In some embodiments, the curable primer layer precursor may be applied to the backing by any known coating method for applying the primer layer precursor to the backing, including, for example, roller coating, extrusion die coating, curtain coating, blade coating, gravure coating, and spray coating.

[0124] After the curable make layer precursor is applied to the backing and before the curable make layer precursor is solidified (eg, by curing), abrasive particles are deposited on the make layer.

[0125] Exemplary curable make coat precursors include phenolic resins, epoxy resins, acrylic monomers, cyanate resins, urethane resins, hide glue, and combinations thereof.

[0126] Exemplary abrasive particles that can be used include fused alumina-based materials such as alumina, ceramic alumina (which may contain one or more metal oxide modifiers and / or crystallization promoters or nucleating agents), and heat-treated alumina, silicon carbide, co-fused alumina-zirconia, diamond, cerium dioxide, titanium diboride, cubic boron nitride, boron carbide, garnet, flint, corundum, sol-gel derived abrasive particles, and blends thereof. Examples of sol-gel abrasive particles include those described in the following patents: U.S. Pat. Nos. 4,314,827 (Leitheiser et al.), 4,518,397 (Leitheiser et al.), 4,623,364 (Cottringer et al.), 4,744,802 (Schwabel), 4,770,671 (Monroe et al.), 4,881,951 (Wood et al.), 5,011,508 (Wood et al.), 5,011,509 (Wood et al.), 5,012,013 (Wood et al.), 5,013,014 (Wood et al.), 5,014,015 (Wood et al.), 5,014,016 (Wood et al.), 5,015,017 (Wood et al.), 5,016,013 ... , 5,429,647 (Larmie), 5,498,269 (Larmie), and 5,551,963 (Larmie), the disclosures of which are incorporated herein by reference. The abrasive particles can be in the form of, for example, individual particles, agglomerates, abrasive composite particles, and mixtures thereof.

[0127] Preferably, the abrasive particles (and in particular the abrasive particles) comprise ceramic abrasive particles, such as, for example, polycrystalline alpha alumina particles prepared by a sol-gel process. Ceramic comminuted abrasive particles composed of microcrystals of alpha alumina, magnesium aluminum spinel, and rare earth hexaaluminate can be prepared using sol-gel alpha alumina particle precursors according to the methods described in, for example, U.S. Pat. No. 5,213,591 (Celikkaya et al.) and U.S. Published Patent Applications 2009 / 0165394A1 (Culler et al.) and 2009 / 0169816A1 (Erickson et al.). Further details regarding methods of making sol-gel derived abrasive particles can be found, for example, in U.S. Pat. Nos. 4,314,827 (Leitheiser), 5,152,917 (Pieper et al.), 5,435,816 (Spurgeon et al.), 5,672,097 (Hoopman et al.), 5,946,991 (Hoopman et al.), 5,975,987 (Hoopman et al.), and 6,129,540 (Hoopman et al.), and U.S. Published Patent Application 2009 / 0165394 Al (Culler et al.).

[0128] In some preferred embodiments, the abrasive particles that can be used (especially in the case of abrasive particles) can be shaped abrasive particles, which can be found in U.S. Pat. Nos. 5,201,916 (Berg), 5,366,523 (Rowenhorst (Re 35,570)) and 5,984,988 (Berg). U.S. Pat. No. 8,034,137 (Erickson et al.) describes aluminum oxide abrasive particles that have been formed into a specific shape and then crushed to form fragments that retain a portion of their original shape features. In some embodiments, the abrasive particles are precisely shaped (i.e., the shape of the particles is at least partially determined by the shape of the cavity in the production tool used to make them). Details about such abrasive particles and methods of making them can be found, for example, in U.S. Pat. Nos. 8,142,531 (Adefris et al.), 8,142,891 (Culler et al.), 8,142,532 (Erickson et al.), 9,771,504 (Adefris); and U.S. Patent Application Publications 2012 / 0227333 (Adefris et al.), 2013 / 0040537 (Schwabel et al.), and 2013 / 0125477 (Adefris). A particularly useful precisely shaped abrasive particle shape is a platelet shape having three side walls, any of which can be straight or concave, and which can be vertical or inclined relative to the platelet base; for example, shapes as described in the references cited above.

[0129] The surface coating on the abrasive particles can be used to improve the adhesion between the abrasive particles and the binder material, or to facilitate the electrostatic deposition of the abrasive particles. In one embodiment, the surface coating described in U.S. Patent No. 5,352,254 (Celikkaya) can be used in an amount of 0.1% to 2% of the surface coating relative to the weight of the abrasive particles. Such surface coatings are described in U.S. Patent Nos. 5,213,591 (Celikkaya et al.), 5,011,508 (Wald et al.), 1,910,444 (Nicholson), 3,041,156 (Rowse et al.), 5,009,675 (Kunz et al.), 5,085,671 (Martin et al.), 4,997,461 (Markhoff-Matheny et al.) and 5,042,991 (Kunz et al.). In addition, the surface coating can prevent the shaped abrasive particles from being capped. "Capping" is a term that describes the phenomenon whereby metal particles from the workpiece being abraded become welded to the tops of the abrasive particles.Surface coatings that perform the above functions are known to those skilled in the art.

[0130] In some embodiments, the length and / or width of the abrasive particles may be selected to be in the range of 0.1 micrometers to 3.5 millimeters (mm), more typically in the range of 0.05 mm to 3.0 mm, and more typically in the range of 0.1 mm to 2.6 mm, although other lengths and widths may be used.

[0131] Abrasive particles may be selected to have a thickness ranging from 0.1 micrometers to 1.6 millimeters, more typically 1 micrometer to 1.2 millimeters, although other thicknesses may also be used. In some embodiments, the abrasive particles may have an aspect ratio (ratio of length to thickness) of at least 2, 3, 4, 5, 6 or more.

[0132] Abrasive particles may be independently sized according to specified nominal grades recognized by the abrasives industry.Exemplary abrasives industry recognized grading standards include those promulgated by ANSI (American National Standards Institute), FEPA (Federation of European Abrasive Manufacturers), and JIS (Japanese Industrial Standards). Such industry-accepted grading standards include, for example: ANSI 4, ANSI 6, ANSI 8, ANSI 16, ANSI 24, ANSI 30, ANSI 36, ANSI 40, ANSI 50, ANSI 60, ANSI 80, ANSI100, ANSI 120, ANSI 150, ANSI 180, ANSI 220, ANSI 240, ANSI 280, ANSI 320, ANSI 360, ANSI 400, and ANSI 600; FEPA P8, FEPA P12, FEPA P16, FEPA P24, FEPA P30, FEPA P36, FEPA P40, FEPA P50, FEPA P60, FEPA P80, FEPA P100, FEPA P120, FEPA P150, FEPA P P180, FEPAP220, FEPA P240, FEPA P320, FEPA P400, FEPA P500, FEPA P600, FEPA P800, FEPA P1000, FEPA P1200; FEPA F8, FEPA F12, FEPA F16 and FEPA F24; and JIS 8, JIS12, JIS16, JIS24, JIS 36. JIS 46, JIS 54, JIS 60, JIS 80, JIS100, JIS150, JIS180, JIS220, JIS240, JIS280, JIS 320, JIS 360, JIS 400, JIS 600, JIS 800, JIS1000, JIS1500, JIS2500, JIS More typically, the crushed alumina particles and the seedless sol-gel-prepared alumina-based abrasive particles are independently sized to ANSI 60 and 80 or FEPA F36, F46, F54 and F60 or FEPA P60 and P80 classification standards.

[0133] Alternatively, the abrasive particles can be made using a test sieve that meets the U.S. standard according to ASTM E-11 "Standard Specification for Wire Cloth and Sieves for Testing Purposes". ASTM E-11 specifies the design and construction requirements of test sieves, which use the media of a wire mesh woven sieve cloth mounted in a frame to classify materials according to a specified particle size. -18+20 is a typical designation, which means that the shaped abrasive particles can pass through a test sieve No. 18 that meets the ASTM E-11 specification, but can be retained on a test sieve No. 20 that meets the ASTM E-11 specification. In one embodiment, the shaped abrasive particles have a particle size such that most of the particles pass through an 18-mesh test sieve and can be retained on a 20-mesh, 25-mesh, 30-mesh, 35-mesh, 40-mesh, 45-mesh, or 50-mesh test sieve. In various embodiments, the nominal screening grades that the shaped abrasive particles can have include:

[0134] + 400, -400 + 450, -450 + 500, -50 + 600, -60 + 700, -70 + 800, -80 + 1000, -100 + 1200, -120 + 1400, -140 + 1700, -170 + 2000, -200 + 2300, -230 + 2700, -270 + 3250, -325 + 4000, -400 + 4500, -450 + 500, or -500 + 6350. Alternatively, a custom mesh size such as -90 + 1000 may be used. Exemplary agglomerates are described, for example, in U.S. Pat. Nos. 4,652,275 (Bloecher et al.) and 4,799,939 (Bloecher et al.), the disclosures of which are incorporated herein by reference. The present disclosure also encompasses agglomerated particles that are erodible using diluents as described, for example, in U.S. Pat. No. 5,078,753 (Broberg et al.), the disclosure of which is incorporated herein by reference. The abrasive composite particles include abrasive particles in a binder.

[0135] Exemplary abrasive composite particles are described, for example, in US Pat. No. 5,549,962 (Holmes et al.), the disclosure of which is incorporated herein by reference.

[0136] The coating weight of the abrasive grains may vary depending, for example, on the particular desired coated abrasive article, the method of applying the abrasive grains, and the particle size of the abrasive grains, but is generally in the range of 1 to 2000 g / m 2 within the range.

[0137] A size layer precursor is then applied to the at least partially cured make coat and abrasive particles, and the size layer precursor is then at least partially cured to provide a size layer. Exemplary size layer precursors include phenolic resins, epoxy resins, acrylic monomers, and combinations thereof. The size layer precursor can be applied by applying and curing a curable size layer precursor using any known coating method, including, for example, roll coating, extrusion die coating, curtain coating, or spray coating.

[0138] The basis weight of the size layer will necessarily vary depending upon the intended use, the type of abrasive grain, and the nature of the coated abrasive article being prepared, but the basis weight is typically between 1 and 5 g / m. 2 Up to 300 or even 800g / m 2 or above.

[0139] If present, the optional top size typically includes a grinding aid and / or an anti-filling material. The optional top size can be used to prevent or reduce the accumulation of dust (material ground off the workpiece) between the abrasive particles, which can significantly reduce the cutting ability of the coated abrasive disc. Useful top sizes typically include a grinding aid (e.g., potassium tetrafluoroborate), a metal salt of a fatty acid (e.g., zinc stearate or calcium stearate), a salt of a phosphate ester (e.g., potassium behenyl phosphate), a phosphate ester, a urea-formaldehyde resin, a mineral oil, a cross-linked silane, a cross-linked silicone, and / or a fluorochemical.

[0140] The optional supersize may be applied to the size layer using any known coating method including, for example, roll coating, extrusion die coating, curtain coating, or spray coating.

[0141] Useful supersizes are further described, for example, in U.S. Pat. No. 5,556,437 (Lee et al.). Typically, the amount of grinding aid incorporated into the coated abrasive product is from about 50 to about 400 gsm, more typically from about 80 to about 300 gsm. The supersize may contain a binder, such as, for example, those used to prepare a size coat or make coat, but it need not have any binder.

[0142] Further details regarding coated abrasive articles including abrasive grains and make, size, and optional topsize layers are well known and described in, for example, U.S. Pat. Nos. 4,734,104 (Broberg); 4,737,163 (Larkey); 5,203,884 (Buchanan et al.); 5,152,917 (Pieper et al.); 5,378,251 (Culler et al.); 5,417,726 (Stout et al.); 5,436,063 (Follett et al.); 5,496,386 (Brober g et al.), 5,609,706 (Benedict et al.), 5,520,711 (Helmin), 5,954,844 (Law et al.), 5,961,674 (Gagliardi et al.), 4,751,138 (Bange et al.), 5,766,277 (DeVoe et al.), 6,077,601 (DeVoe et al.), 6,228,133 (Thurber et al.), and 5,975,988 (Christianson), the disclosures of which are incorporated herein by reference.

[0143] In some embodiments of coated abrasive articles according to the present disclosure, the abrasive layer comprises a dispersion of abrasive particles and a binder, which is the reaction product of a curable composition according to the present disclosure (typically applied as a slurry). Slurry coating techniques are well known in the abrasive art and include, for example, those described in U.S. Pat. Nos. 5,378,251 (Culler et al.), 5,942,015 (Culler et al.), and 6,277,160 (Stubbs et al.); the disclosures of the above patents are incorporated herein by reference.

[0144] In some embodiments of coated abrasive articles according to the present disclosure, the abrasive layer comprises abrasive composites, which in some embodiments are precisely shaped.

[0145] Thus, in another exemplary embodiment, a coated abrasive article according to the present disclosure may have an abrasive layer comprising precisely shaped abrasive composites (eg, a structured abrasive article). Figure 3 , an exemplary coated abrasive article 300 has a backing 310, a backing treatment 320 (e.g., a presize layer or bonding layer) according to the present disclosure fixed to a major surface 315 of the backing 310, and an abrasive layer 330 fixed to the bonding layer 320. The abrasive layer 330 includes a plurality of precisely shaped abrasive composites 355. The abrasive composites include abrasive particles 360 dispersed in a binder 350.

[0146] In making such coated abrasive articles, a slurry comprising a curable binder precursor and abrasive particles can be applied to a tool having a plurality of precisely shaped cavities therein. The slurry is then at least partially polymerized and attached to a bonding layer by, for example, addition polymerization of an adhesive or slurry. Suitable binder precursors and abrasive particles include, for example, those listed above.

[0147] The abrasive composites can be any three-dimensional shape that forms at least one of a raised feature or a groove on the exposed surface of the abrasive layer. Useful shapes include, for example, cubes, prisms, pyramids (e.g., square pyramids or hexagonal pyramids), truncated pyramids, cones, crosses, hemispheres, and truncated cones. Combinations of abrasive composites of different shapes and / or sizes can also be used. The abrasive layer of the structured abrasive can be continuous or discontinuous.

[0148] For finishing applications, the density of the abrasive composites in the abrasive layer is generally in the range of at least 1,000, 10,000, or even at least 20,000 abrasive composites per square inch (e.g., at least 150, 1,500, or even 7,800 abrasive composites per square centimeter) up to and including 50,000, 70,000, or even up to 100,000 abrasive composites per square inch (up to and including 7,800, 11,000, or even up to 15,000 abrasive composites per square centimeter), although abrasive composites of greater or lesser density may also be used.

[0149] Further details regarding coated abrasive articles having an abrasive layer comprising precisely shaped abrasive composites can be found, for example, in U.S. Pat. Nos. 5,152,917 (Pieper et al.), 5,435,816 (Spurgeon et al.), 5,672,097 (Hoopman), 5,681,217 (Hoopman et al.), 5,851,247 (Stoetzel et al.), and 6,139,594 (Kincaid et al.), the disclosures of which are incorporated herein by reference.

[0150] The coated abrasive articles according to the present invention can be converted into, for example, belts, strips, rolls, discs (including perforated discs), and / or sheets. For belt applications, the two free ends of the abrasive sheet can be joined together to form a spliced ​​belt using known methods. Endless belts can also be formed as described, for example, in U.S. Pat. No. 5,573,619 (Benedict et al.), the disclosure of which is incorporated herein by reference.

[0151] Coated abrasive articles according to the present invention can be used to abrade a workpiece. One such method includes frictionally contacting at least a portion of an abrasive layer of the coated abrasive article with at least a portion of a surface of the workpiece, and moving at least one of the coated abrasive article or the workpiece relative to the other to abrade at least a portion of the surface.

[0152] Examples of workpiece materials include metals, metal alloys, exotic metal alloys, ceramics, glass, wood, wood-like materials, composite materials, painted surfaces, plastics, reinforced plastics, stone, and / or combinations thereof. The workpiece may be flat or have a shape or contour associated therewith. Exemplary workpieces include metal parts, plastic parts, particle board, camshafts, crankshafts, furniture, and turbine blades.

[0153] The coated abrasive article according to the present invention can be used manually and / or in conjunction with a machine. When abrading is performed, at least one of the coated abrasive article and the workpiece is usually moved relative to the other or both are moved relative to each other.

[0154] Grinding can be performed under wet or dry conditions. Exemplary liquids for wet grinding include water, water containing conventional rust-inhibiting compounds, lubricants, oils, soaps, and cutting fluids. The liquid may also contain defoamers, degreasers, and / or the like.

[0155] Select an implementation

[0156] In a first embodiment, the present disclosure provides a curable composition comprising a component, based on the total weight of components a) to g), comprising:

[0157] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0158] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0159] c) 5 to 45% by weight of polythiol;

[0160] d) 0 to 10% by weight of dicyandiamide;

[0161] e) 0.1% to 2% of a free radical photoinitiator;

[0162] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0163] g) 0% to 5% phenolic resin.

[0164] In a second embodiment, the present disclosure provides a curable composition according to the first embodiment, wherein the curable composition is substantially free of phenolic resin.

[0165] In a third embodiment, the present disclosure provides a curable composition according to the first or second embodiment, wherein the curable composition is substantially free of dissolved thermoplastic polymer.

[0166] In a fourth embodiment, the present disclosure provides a curable composition according to any one of the first to third embodiments, wherein the curable composition is substantially free of dicyandiamide.

[0167] In a fifth embodiment, the present disclosure provides a treated backing comprising a fabric having a backing treatment contacting at least a portion of the fabric, wherein the backing treatment comprises the reaction product of a curable composition comprising, based on the total weight of components a) through g):

[0168] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0169] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0170] c) 5 to 45% by weight of polythiol;

[0171] d) 0 to 10% by weight of dicyandiamide;

[0172] e) 0.1% to 2% of a free radical photoinitiator;

[0173] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0174] g) 0% to 5% phenolic resin.

[0175] In a sixth embodiment, the present disclosure provides a curable composition according to the fifth embodiment, wherein the backing treatment is substantially free of phenolic resin.

[0176] In a seventh embodiment, the present disclosure provides a curable composition according to the fifth or sixth embodiment, wherein the backing treatment is substantially free of dissolved thermoplastic polymer.

[0177] In an eighth embodiment, the present disclosure provides a curable composition according to any one of the fifth to seventh embodiments, wherein the backing treatment is substantially free of dicyandiamide.

[0178] In a ninth embodiment, the present disclosure provides a curable composition according to any one of the fifth to eighth embodiments, wherein the fabric has two opposing major surfaces, and wherein the backing treatment contacts both major surfaces.

[0179] In a tenth embodiment, the present disclosure provides a curable composition according to any one of the fifth to eighth embodiments, wherein the treated backing has two opposing major surfaces, and wherein the backing treatment contacts only one of the major surfaces.

[0180] In an eleventh embodiment, the present disclosure provides a curable composition according to any one of the fifth to tenth embodiments, wherein the fabric has a basis weight in a range of 200 grams per square meter to 400 grams per square meter.

[0181] In a twelfth embodiment, the present disclosure provides a method of making a treated backing, the method comprising:

[0182] Contacting at least a portion of the fabric with a curable composition preparable from components comprising, based on the total weight of components a) to g),

[0183] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0184] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0185] c) 5 to 45% by weight of polythiol;

[0186] d) 0 to 10% by weight of dicyandiamide;

[0187] e) 0.1% to 2% of a free radical photoinitiator;

[0188] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0189] g) 0% to 5% phenolic resin; and

[0190] The curable composition is at least partially cured.

[0191] In a thirteenth embodiment, the present disclosure provides a method according to the twelfth embodiment, wherein the curable composition is substantially free of phenolic resin.

[0192] In a fourteenth embodiment, the present disclosure provides a method according to the twelfth or thirteenth embodiment, wherein the curable composition is substantially free of dissolved thermoplastic polymer.

[0193] In a fifteenth embodiment, the present disclosure provides a method according to any one of the twelfth to fourteenth embodiments, wherein the curable composition is substantially free of dicyandiamide.

[0194] In a sixteenth embodiment, the present disclosure provides a method according to any one of the twelfth to fifteenth embodiments, wherein the fabric has two opposing major surfaces, and wherein the curable composition contacts the two major surfaces.

[0195] In a seventeenth embodiment, the present disclosure provides a method according to any one of the twelfth to sixteenth embodiments, wherein the fabric has two opposing major surfaces, and wherein the curable composition contacts only one of the two major surfaces.

[0196] In an eighteenth embodiment, the present disclosure provides a method according to any one of the twelfth to seventeenth embodiments, wherein the treated backing comprises a fabric having a basis weight in a range of 200 grams per square meter to 400 grams per square meter.

[0197] In a nineteenth embodiment, the present disclosure provides a coated abrasive article comprising an abrasive layer secured to a major surface of a treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder, wherein the treated backing comprises at least one of a presize layer, an impregnant or subsize layer, or a bonding layer, the treated backing comprising a reaction product of components, the components comprising, based on the total weight of components a) to g):

[0198] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0199] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0200] c) 5 to 45% by weight of polythiol;

[0201] d) 0 to 10% by weight of dicyandiamide;

[0202] e) 0.1% to 2% of a free radical photoinitiator;

[0203] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0204] g) 0% to 5% phenolic resin.

[0205] In a twentieth embodiment, the present disclosure provides a coated abrasive article according to the nineteenth embodiment, wherein the binder is substantially free of phenolic resin.

[0206] In a twenty-first embodiment, the present disclosure provides a coated abrasive article according to the nineteenth or twentieth embodiment, wherein the binder is substantially free of dissolved thermoplastic polymers.

[0207] In a twenty-second embodiment, the present disclosure provides a coated abrasive article according to any one of the nineteenth to twenty-first embodiments, wherein the binder is substantially free of dicyandiamide.

[0208] In a twenty-third embodiment, the present disclosure provides a coated abrasive article according to any one of the nineteenth to twenty-second embodiments, wherein the treated backing comprises a fabric having a basis weight in a range of 200 grams per square meter to 400 grams per square meter.

[0209] In a twenty-fourth embodiment, the present disclosure provides a coated abrasive product according to any one of the nineteenth to twenty-third embodiments, wherein the abrasive layer comprises: a base coat layer disposed on at least a portion of the treated backing, abrasive grains partially embedded in the base coat layer, and a secondary coat layer at least partially covering the base coat layer and the abrasive grains.

[0210] In a twenty-fifth embodiment, the present disclosure provides a coated abrasive article according to the twenty-fourth embodiment, further comprising a supersize disposed at least partially on the size layer.

[0211] In a twenty-sixth embodiment, the present disclosure provides a coated abrasive article according to any one of the nineteenth to twenty-third embodiments, wherein the abrasive particles are dispersed in a binder.

[0212] In a twenty-seventh embodiment, the present disclosure provides a coated abrasive article according to any of the twenty-sixth embodiment, wherein the abrasive layer comprises abrasive composites.

[0213] In a twenty-eighth embodiment, the present disclosure provides a coated abrasive article according to the twenty-sixth embodiment, wherein the abrasive layer comprises precisely shaped abrasive composites.

[0214] In a twenty-ninth embodiment, the present disclosure provides a method of grinding a workpiece, the method comprising:

[0215] Providing a coated abrasive article according to any one of the nineteenth to twenty-eighth embodiments;

[0216] frictionally contacting at least a portion of the abrasive layer with at least a portion of a surface of a workpiece; and

[0217] At least one of the coated abrasive article or the workpiece is moved relative to the other to abrade at least a portion of the surface.

[0218] In a thirtieth embodiment, the present disclosure provides a method of making a coated abrasive article, the method comprising:

[0219] A curable backing treatment precursor is disposed on at least a portion of the backing, the curable backing treatment precursor comprising the following components, based on the total weight of components a) to g):

[0220] a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F;

[0221] b) 6 to 12% by weight of at least trifunctional (meth)acrylate;

[0222] c) 5 to 45% by weight of polythiol;

[0223] d) 0 to 10% by weight of dicyandiamide;

[0224] e) 0.1% to 2% of a free radical photoinitiator;

[0225] f) 0.5 to 1% by weight of 2-alkylimidazole; and

[0226] g) 0% to 5% phenolic resin; and

[0227] at least partially curing the curable backing treatment precursor to provide a treated backing; and

[0228] An abrasive layer is secured to the major surface of the treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder.

[0229] In a thirty-first embodiment, the present disclosure provides a method according to the thirtieth embodiment, wherein the treated backing comprises at least one of a presize, a subsize, or an impregnant.

[0230] In a thirty-second embodiment, the present disclosure provides a method according to the thirtieth or thirty-first embodiment, wherein the curable backing treatment precursor is substantially free of phenolic resin.

[0231] In a thirty-third embodiment, the present disclosure provides a method according to any one of the thirtieth to thirty-second embodiments, wherein the curable backing treatment precursor is substantially free of dissolved thermoplastic polymer.

[0232] In a thirty-fourth embodiment, the present disclosure provides a method according to any one of the thirtieth to thirty-third embodiments, wherein the curable backing treatment precursor is substantially free of dicyandiamide.

[0233] In a thirty-fifth embodiment, the present disclosure provides a method according to any one of the thirtieth to thirty-fourth embodiments, wherein the backing comprises a fabric having a basis weight in a range of 200 grams per square meter to 400 grams per square meter.

[0234] In a thirty-sixth embodiment, the present disclosure provides a method according to any one of the thirtieth to thirty-fifth embodiments, wherein the abrasive layer comprises: a base glue layer disposed on at least a portion of the treated backing, abrasive particles partially embedded in the base glue layer, and a composite glue layer at least partially covering the base glue layer and the abrasive particles.

[0235] In a thirty-seventh embodiment, the present disclosure provides the method according to the thirty-sixth embodiment, the abrasive layer further comprising a supersize layer at least partially disposed on the size layer.

[0236] In a thirty-eighth embodiment, the present disclosure provides a method according to any one of the thirtieth to thirty-fifth embodiments, wherein the abrasive particles are dispersed in a binder.

[0237] In a thirty-ninth embodiment, the present disclosure provides a method according to the thirty-eighth embodiment, wherein the abrasive layer comprises abrasive composites.

[0238] In a fortieth embodiment, the present disclosure provides a method according to the thirty-eighth embodiment, wherein the abrasive layer comprises precisely shaped abrasive composites.

[0239] Objects and advantages of this invention are further illustrated by the following non-limiting examples, but the particular materials and amounts thereof recited in these examples, as well as other conditions and details, should not be construed to unduly limit this invention.

[0240] Example

[0241] Unless otherwise noted, all other reagents were obtained or purchased from fine chemical suppliers such as Sigma-Aldrich Company, St. Louis, Missouri, or may be synthesized by known methods.

[0242] Unit abbreviations used in the examples: gsm = grams per square meter, °C = degrees Celsius; cm = centimeter; mm = millimeter; μm = micrometer; fpm = feet per minute; and kV = kilovolt.

[0243] Table 1 below reports the materials used in the examples.

[0244] Table 1

[0245]

[0246]

[0247] Backing treatment

[0248] The cloth backing (HPC or PCC) was pre-cut into rectangular sheets of 11.4 cm × 25.4 cm. The treatment solution was preheated to 60°C and coated on the rich weft side (technical back) of the cloth piece using a draw-down scraper with a gap of 76.2 μm. The coated sample was immediately UV irradiated under an H bulb at 300WPI, 12fpm, and then finally cured in a lab Mathis oven at 140°C or 170°C for 2 minutes and 15 seconds based on the example requirements. The sample was back-coated with BCZ using a draw-down scraper with a gap of 76.2 μm on the rich warp side (technical face), and then dried in an oven under the following conditions: dried at 110°C for 1 min, and then dried at 130°C for 2 min. The backing flatness was visually inspected. All example backings showed improved flatness compared to the comparative examples.

[0249] Peel test

[0250] The fully treated backing was coated with MR1 using a spin-draw blade at a gap of 101.6 μm, and then BAO was drop-coated on top to saturate the surface. The samples were cured at 93°C and 103°C for one hour respectively. SZ1 was then targeted to the abrasive side at a coating weight of 544 gsm. After final curing at 103°C overnight, the coated abrasive samples were ready for peel testing.

[0251] A 17.8 cm x 7.6 cm x 6 mm thick wooden board was coated with a layer of TECHNOMELT 8633 hot melt adhesive (Henkel USA, Stamford, CT) dispensed by a hot melt adhesive gun. A 10 cm section of a 17.78 cm x 2.54 cm strip of coated abrasive to be tested was partially overlaid on the molten laminated composition, with the abrasive side facing the laminated composition. The abrasive strip was then pressed into position, and the assembly was then cooled to 25°C.

[0252] The board was mounted horizontally into the upper jaw of a tensile tester (a SINTECH 6W tensile tester from MTS Systems Corporation, Eden Prairie, Minnesota). The free end of the coated abrasive was then attached to the lower jaw of the tensile tester, and the lower jaw pulled the coated abrasive from the board at a rate of 0.5 mm / sec at a 90 degree angle. The force necessary to cause failure of the test specimen was reported, expressed in Newtons / cm (N / cm) of sample width. The tests were conducted at the indicated temperatures.

[0253] Example 1

[0254] 66.71 parts by weight of EPOXY were mixed with 8.50 parts by weight of TMPTA using a mechanical stirrer at room temperature until a homogeneous state was reached, and then 1.00 parts by weight of BDK was added during stirring. The mixture was heated to 60°C. After the BDK was completely dissolved, 4.45 parts by weight of NPR were added, and the mixture was mixed at 60°C until uniform. Then 11.56 parts by weight of PETMP, 7.12 parts by weight of DCDA and 0.67 parts by weight of 2-PI were added and mixed until uniform. The obtained solution was used to treat HPC and cured at 170°C for peeling test as described above, thereby producing SB-1-P170.

[0255] Example 2

[0256] 70.69 parts by weight of EPOXY and 8.50 parts by weight of TMPTA were mixed at room temperature using a mechanical stirrer until uniform, and then 1.00 parts by weight of BDK was added during stirring. The mixture was heated to 60°C. After BDK was completely dissolved, 11.56 parts by weight of PETMP, 7.54 parts by weight of DCDA and 0.71 parts by weight of 2-PI were added and mixed until uniform. The obtained solution was used to treat HPC and cured at 170°C for peeling test as described above, thereby producing SB-2-P170.

[0257] Example 3

[0258] The treatment solution was mixed by the same procedure as in Example 2, but with a different composition ratio: 75.14 parts by weight of EPOXY, 10.33 parts by weight of TMPTA, 5.65 parts by weight of PETMP, 0.15 parts by weight of BDK, 8.01 parts by weight of DCDA, and 0.75 parts by weight of 2-PI. The obtained solution was used to treat HPC and cured at 170° C. for the peel test as described above, thereby producing SB-3-P170.

[0259] Example 4

[0260] The treatment solution was mixed by the same procedure as in Example 2, but with a different composition ratio: 75.00 parts by weight of EPOXY, 10.33 parts by weight of TMPTA, 5.62 parts by weight of PETMP, 0.30 parts by weight of BDK, 8.00 parts by weight of DCDA, and 0.75 parts by weight of 2-PI. The obtained solution was used to treat HPC and cured at 170° C. for the peel test as described above, thereby producing SB-4-P170.

[0261] Example 5

[0262] 47.44 parts by weight of EPOXY and 11.21 parts by weight of TMPTA were mixed at room temperature using a mechanical stirrer until uniform, and then 0.33 parts by weight of BDK was added during stirring. The mixture was heated to 60°C. After BDK was completely dissolved, 40.27 parts by weight of PETMP and 0.75 parts by weight of 2-PI were added and mixed until uniform. The obtained solution was used to treat HPC and PCC, and cured at 140°C or 170°C for peeling tests as described above, thereby producing SB-5-P170, SB-5-P140 and SB-5-PC140, respectively.

[0263] Comparative Example A

[0264] 75.19 parts by weight of EPOXY was mixed with 10.03 parts by weight of TMPTA at room temperature using a mechanical stirrer until uniform, and then 1.00 parts by weight of BDK was added during stirring. The mixture was heated to 60°C. After the BDK was completely dissolved, 5.01 parts by weight of NPR were added, and the mixture was mixed at 60°C until uniform. Then 8.02 parts by weight of DCDA and 0.75 parts by weight of 2-PI were added and mixed until uniform. The obtained solution was used to treat HPC and cured at 170°C for peel testing as described above, thereby producing SB-P-Comp.

[0265] Comparative Example B

[0266] The comparative PCC backing was not pre-sized, but only back-sized as described above for the peel test, resulting in SB-PC-Comp.

[0267] Table 2 below reports the peel test results for Examples 1 to 6 and Comparative Examples A and B.

[0268] Table 2

[0269]

[0270] Various modifications and alterations of this invention may be made by those skilled in the art without departing from the scope and spirit of this invention, and it should be understood that this invention is not to be unduly limited to the illustrative embodiments set forth herein.

Claims

1. A curable composition comprising components, based on the total weight of components a) to g), wherein the components comprise: a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F; b) 6 to 12% by weight of at least trifunctional (meth)acrylate; c) 5 to 45% by weight of polythiol; d) 0 to 10% by weight of dicyandiamide; e) 0.1% to 2% of a free radical photoinitiator; f) 0.5 to 1% by weight of 2-alkylimidazole; and g) 0% to 5% phenolic resin.

2. The curable composition of claim 1, wherein the curable composition is substantially free of phenolic resin.

3. The curable composition of claim 1, wherein the curable composition is substantially free of dissolved thermoplastic polymer.

4. The curable composition of claim 1, wherein the curable composition is substantially free of dicyandiamide.

5. A treated backing comprising a fabric having a backing treatment contacting at least a portion of the fabric, wherein the backing treatment comprises the reaction product of a curable composition comprising, based on the total weight of components a) through g), a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F; b) 6 to 12% by weight of at least trifunctional (meth)acrylate; c) 5 to 45% by weight of polythiol; d) 0 to 10% by weight of dicyandiamide; e) 0.1% to 2% of a free radical photoinitiator; f) 0.5 to 1% by weight of 2-alkylimidazole; and g) 0% to 5% phenolic resin.

6. The treated backing of claim 5, wherein the backing treatment is substantially free of phenolic resin.

7. The treated backing of claim 5, wherein the backing treatment is substantially free of dissolved thermoplastic polymers.

8. The treated backing of claim 5, wherein the backing treatment is substantially free of dicyandiamide.

9. The treated backing of claim 5, wherein the fabric has two opposing major surfaces, and wherein the backing treatment contacts both major surfaces.

10. The treated backing of claim 5, wherein the treated backing has two opposing major surfaces, and wherein the backing treatment contacts only one of the major surfaces.

11. The treated backing of claim 5, wherein the fabric has a basis weight in the range of 200 g / m2 to 400 g / m2.

12. A method of making a treated backing, the method include: Contacting at least a portion of the fabric with a curable composition preparable from components comprising, based on the total weight of components a) to g), a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F; b) 6 to 12% by weight of at least trifunctional (meth)acrylate; c) 5 to 45% by weight of polythiol; d) 0 to 10% by weight of dicyandiamide; e) 0.1% to 2% of a free radical photoinitiator; f) 0.5 to 1% by weight of 2-alkylimidazole; as well as g) 0% to 5% phenolic resin; and The curable composition is at least partially cured.

13. The method of claim 12, wherein the curable composition is substantially free of phenolic resin.

14. The method of claim 12, wherein the curable composition is substantially free of dissolved thermoplastic polymer.

15. The method of claim 12, wherein the curable composition is substantially free of dicyandiamide.

16. The method of claim 12, wherein the fabric has two opposing major surfaces, and wherein the curable composition contacts both major surfaces.

17. The method of claim 12, wherein the fabric has two opposing major surfaces, and wherein the curable composition contacts only one of the two major surfaces.

18. The method of claim 12, wherein the treated backing comprises a fabric having a basis weight in a range of 200 g / m2 to 400 g / m2.

19. A coated abrasive article comprising an abrasive layer secured to a major surface of a treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder, wherein the treated backing comprises at least one of a presize layer, an impregnant or subsize layer, or a bonding layer, the treated backing comprising the reaction product of components, based on the total weight of components a) to g), comprising: a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F; b) 6 to 12% by weight of at least trifunctional (meth)acrylate; c) 5 to 45% by weight of polythiol; d) 0 to 10% by weight of dicyandiamide; e) 0.1% to 2% of a free radical photoinitiator; f) 0.5 to 1% by weight of 2-alkylimidazole; and g) 0% to 5% phenolic resin.

20. The coated abrasive article of claim 19, wherein the binder is substantially free of phenolic resins.

21. The coated abrasive article of claim 19, wherein the binder is substantially free of dissolved thermoplastic polymers.

22. The coated abrasive article of claim 19, wherein the binder is substantially free of dicyandiamide.

23. The coated abrasive article of claim 19, wherein the treated backing comprises a fabric having a basis weight in a range of 200 g / m2 to 400 g / m2.

24. The coated abrasive article of claim 19, wherein the abrasive layer include: A make layer is disposed on at least a portion of the treated backing, abrasive grains are partially embedded in the make layer, and a size layer at least partially covers the make layer and the abrasive grains.

25. The coated abrasive article of claim 24, further comprising a supersize disposed at least partially on the size coat.

26. The coated abrasive article of claim 19, wherein the abrasive particles are dispersed in a binder.

27. The coated abrasive article of claim 26, wherein the abrasive layer comprises abrasive composites.

28. The coated abrasive article of claim 26, wherein the abrasive layer comprises precisely shaped abrasive composites.

29. A method for grinding a workpiece, the method include: Providing a coated abrasive article according to claim 19; placing at least a portion of the abrasive layer in frictional contact with at least a portion of a surface of the workpiece; as well as At least one of the coated abrasive article or the workpiece is moved relative to the other to abrade at least a portion of the surface.

30. A method of making a coated abrasive article, the method include: A curable backing treatment precursor is disposed on at least a portion of the backing, based on a composition The curable backing treatment precursor comprises the following components, based on the total weight of a) to g): a) 45 to 80 wt % of an epoxy resin, which can be prepared by reacting epichlorohydrin with at least one of bisphenol A or bisphenol F; b) 6 to 12% by weight of at least trifunctional (meth)acrylate; c) 5 to 45% by weight of polythiol; d) 0 to 10% by weight of dicyandiamide; e) 0.1% to 2% of a free radical photoinitiator; f) 0.5 to 1% by weight of 2-alkylimidazole; as well as g) 0% to 5% phenolic resin; as well as at least partially curing the curable backing treatment precursor to provide a treated backing; as well as An abrasive layer is secured to the major surface of the treated backing, wherein the abrasive layer comprises abrasive particles retained in a binder.

31. The method of claim 30, wherein the treated backing comprises at least one of a presize, a subsize, or an impregnant.

32. The method of claim 30, wherein the curable backing treatment precursor is substantially free of phenolic resin.

33. The method of claim 30, wherein the curable backing treatment precursor is substantially free of dissolved thermoplastic polymer.

34. The method of claim 30, wherein the curable backing treatment precursor is substantially free of dicyandiamide.

35. The method of claim 30, wherein the backing comprises a fabric having a basis weight in a range of 200 g / m2 to 400 g / m2.

36. The method according to claim 30, wherein the abrasive layer include: A make layer is disposed on at least a portion of the treated backing, abrasive grains are partially embedded in the make layer, and a size layer at least partially covers the make layer and the abrasive grains.

37. The method of claim 36, wherein the abrasive layer further comprises a supersize layer at least partially disposed on the size coat.

38. The method of claim 30, wherein the abrasive particles are dispersed in a binder.

39. The method of claim 38, wherein the abrasive layer comprises abrasive composites.

40. The method of claim 38, wherein the abrasive layer comprises precisely shaped abrasive composites.