Composite component and method of making same

By introducing concentration gradient additives into the functional areas of composite material components, the problems of difficulty in distribution of additives and low structural integrity of composite material components in the prior art are solved, and efficient and economical manufacturing and long-term functional improvement are achieved. It is suitable for Components of complex geometric shapes.

CN118900763APending Publication Date: 2024-11-05SGL CARBON SE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380032698.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-03-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

During the manufacturing process of existing composite components, there are problems such as difficulty in uniform distribution of additive concentrations, difficulty in local control and regulation, low structural integrity, high cost, short-term functionality and difficulty in achieving complex geometric shapes, especially under thermal stress, layer separation is prone to occur. and the fall off of the flame retardant layer.

Method used

Using composite components containing fiber and matrix materials, the material properties are affected by introducing additives with concentration gradients in the functional area, providing locally different functional performances, and improving structural integrity and manufacturing through overall curing and one-piece design efficiency.

Benefits of technology

Long-term functional improvements in composite components, enhanced structural integrity, reduced costs, simplified manufacturing process, and avoided functional degradation under layer separation and thermal stress, enabling efficient manufacturing of components with complex geometries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900763A_ABST
    Figure CN118900763A_ABST
Patent Text Reader

Abstract

The invention relates to a composite material component, a motor vehicle component or a building component comprising the composite material component, a method for manufacturing the composite material component and the use of the composite material component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite component, a motor vehicle component or a building component comprising the composite component, a method for producing the composite component and the use of the composite component. Background Art

[0002] Composite components are already known in the prior art, with which different functions can be implemented in technical products, for example flame retardant effects.

[0003] For example, US 2005 / 0170238 A1 discloses a battery housing formed by a flame retardant polymer composition made of high density polyethylene, which can contain glass fiber reinforcement and fire resistant additives. During the manufacturing process, the fire resistant additive is mixed with the polyethylene to be protected in the form of a melt, and then the material is pressed into the desired shape. A disadvantage here is that the additive concentration is uniformly distributed in space and the concentration cannot be locally controlled / regulated.

[0004] US 2020 / 0152926 A1 describes a cover for a battery pack of an electric vehicle, the frame of which is made of a layered composite material. The first layer of the composite material comprises a so-called "shear panel" having a fiber-reinforced composite material layer intended to counteract shear deformation during impact. As a separate element, the layered composite material comprises a second functional layer that is fire-resistant and wear-resistant, which is deposited on the shear panel and faces the battery when the shear panel is connected to the vehicle frame.

[0005] However, a disadvantage of this arrangement is that, because of the severe deviations in the material structure, the separate fire-resistant second layer is susceptible to cracking and burning and can easily separate from the layered composite material, in particular under thermal stress. As a rule, the functionality of the composite component caused by the corresponding functional layer cannot be guaranteed in the long term. In addition, such layered composite materials usually require large amounts of additives, which can lead to increased costs for the product.

[0006] In addition to the fact that the methods for manufacturing such layered composites are laborious and complex, the realization of complex geometries is simply not possible or can only be achieved to a very limited extent. For example, in order to provide multi-dimensional components, flat blanks must be cut into sheets, which increases costs and limits the precision of the components. In order to overcome these disadvantages, a lot of effort is needed in terms of production and quality assurance.

[0007] Furthermore, because such layered composites have a lower structural integrity, thicker and / or heavier designs are often required to maintain a comparable level of functionality. Furthermore, typical joining methods, such as gluing or coating, often result in an inadequate joining of the different parts, for example due to poor adhesion properties of the disparate materials. Such assemblies are a risk in particular for automotive applications, since the corresponding layers can loosen and fall off during normal driving. In applications for battery housings, flame retardant layers can fall off the surface to be protected when exposed to fire. When battery cells overheat, poor abrasion behavior is often observed in the event of particle bombardment.

[0008] Purpose of the Invention

[0009] Against this background, the object of the present invention is therefore to provide a composite component which avoids the above-mentioned disadvantages of the prior art, in particular enables the composite component to have an improved and longer-term functionality and can be produced in a simple, cost-effective and process-reliable manner. In addition, it should be possible to improve the control of the material properties. Summary of the invention

[0010] According to the present invention, this object is achieved by a composite material component, which comprises or consists of the following components:

[0011] a) fibrous materials;

[0012] b) matrix material; and

[0013] c) a functional region in which an additive is arranged, which additive causes or influences material properties, in particular optical, thermal, mechanical and / or electromagnetic material properties, in the functional region, wherein

[0014] The functional region has a concentration gradient of the additive, so that the material properties caused by or affected by the additive exhibit locally different degrees in the functional region.

[0015] The composite component comprises one or more regions, at least one of which is a functional region of additives having a concentration gradient. Thus, the functional region has a degree of functionality that differs locally. Preferably, the functional region has a matrix material and / or a fiber material. In another preferred embodiment, the functional region does not have a fiber material.

[0016] The functional region can also contain pores, ie air and / or gas inclusions, which however preferably do not exceed 5% by volume of the total volume of the functional region.

[0017] The functional region can preferably form the entire composite component, ie the composite component has only one region, namely the functional region, which is formed by the composite component. However, the composite component can also have other regions, in particular other functional regions.

[0018] The composite component preferably consists exclusively of the region comprising fiber material and matrix material.

[0019] For the sake of linguistic simplicity, what is mentioned below is "a" fiber material and / or "a" region and / or "a" functional region and / or "a" matrix material and / or "a" additive and / or "a" concentration gradient. However, this should not be understood as a numerical limitation. In the following, the use of the singular should always be interpreted as it can also be "one or more" corresponding components.

[0020] A "composite component" is understood to mean a material consisting of a combination of two or more connected materials, for example a fiber material and a matrix material, whose material properties differ from those of its individual components and which can be used as a component of a technical product. Such a component can be, for example, a plate or a housing of a machine. However, the term also includes composite components that can form a technical product itself. The composite component according to the invention is a fiber composite material, such as GRP or CFRP.

[0021] The composite component can have one or more regions, at least one of which is a functional region. The functional region provides the composite component with the functions required for the application purpose, such as shielding or fire protection, by providing or influencing specific material properties. To this end, the functional region contains additives and optional fiber materials and / or optional matrix materials, or consists of the above components. In this case, the fiber material of the composite component is not an additive in the sense of the present invention, that is, the additive is an additive different from the fiber material and causes or influences the material properties in the functional region, in particular the optical material, thermal material, mechanical material and / or electromagnetic material properties.

[0022] The composite component can be manufactured by connecting different workpieces or coating workpieces. However, the composite component is preferably designed in an integral manner, i.e. in one piece. The composite component is particularly preferably obtained by integral curing during its production. The functional area can be manufactured by connecting different workpieces or coating workpieces. However, the functional area is preferably designed in an integral manner, i.e. in one piece. Particularly preferably, the functional area is obtained by integral curing during its production.

[0023] The volume fraction of the functional region relative to the total volume of the composite component is preferably ≥2 volume %, more preferably ≥5 volume %, even more preferably ≥10 volume %, even more preferably ≥20 volume %, even more preferably ≥40 volume %, and most preferably ≥60 volume %.

[0024] Preferably, apart from the incorporated additives and the incorporated fiber material, the matrix material of one, several or all regions of the composite component has a substantially homogeneous chemical composition, i.e., apart from the incorporated additives and the incorporated fiber material, material boundaries do not exist at all or only exist in adjacent regions of the composite component.

[0025] As mentioned above, additives are components contained in addition to fiber materials and matrix materials in composite components, which components cause or influence, especially enhance or weaken the material properties of the functional area, especially optical, thermal, mechanical and / or electromagnetic properties. This means that one or more material properties of the functional area are newly developed, enhanced or reduced compared to the functional area without the corresponding additive. Additives and / or fiber materials are at least partially, preferably substantially embedded in the matrix material. In this case, it is basically meant that at least 70 volume %, preferably at least 75 volume %, more preferably at least 80 volume %, more preferably at least 85 volume %, more preferably at least 90 volume % and most preferably at least 95 volume % of the fiber material is completely surrounded by the matrix material. Very particularly preferably, additives and / or fiber materials are completely embedded in the matrix material.

[0026] The functional area has an additive with a concentration gradient, so that it contains non-intersecting volume elements (i.e., volume elements with no volume intersection) with different concentrations of additives, so that the properties caused by or affected by the additives are strongly manifested in the functional area in a locally different manner. The volume of the non-intersecting volume elements is preferably ≥1%, more preferably ≥2%, and even more preferably ≥5%, but also preferably ≤10% of the total volume of the functional area and / or the composite component. The concentration gradient represents a preferably continuous local variation of the concentration of the additive in the functional area, preferably in the optional matrix material of the functional area. Continuous should be understood to refer to the continuous distribution of the concentration values ​​of the concentration function, i.e., the concentration gradient. The concentration gradient is preferably predefined, i.e., a distribution with concentration values ​​and / or directions predetermined by the method measures implemented during the manufacturing method. In the context of the present invention, concentration should be understood to refer to mass concentration, i.e., the mass of the additive in the composite component per unit volume (e.g., g / L).

[0027] The area of ​​the composite component and the spatial dimensions of the composite component itself are not restricted within the scope of the present invention. The composite component can preferably be a board, for example a fireproof board. The area of ​​the composite component can preferably be a layer. In this case, the composite component is particularly preferably a layered composite material or contains such a composite material. A layer is understood to mean a material or material mixture that is preferably a flat surface, which preferably has a material boundary with other areas of the composite component.

[0028] The term "material properties of the functional region" includes all material properties of the material or material mixture forming the functional region. The term encompasses both physical properties such as thermal conductivity or expansion coefficient and chemical material properties such as flammability or antimicrobial effect.

[0029] In a preferred embodiment of the invention, the material property induced by the additive in the functional area or influenced by the additive is a physical material property, preferably an optical, thermal, mechanical, acoustic, electrodynamic, thermodynamic and / or electromagnetic property. Particularly preferably, the physical material property is selected from the group consisting of: expansion coefficient, heat capacity, thermal conductivity / thermal conductivity, ductility, elasticity, strength, hardness, wear resistance, toughness, permeability (especially magnetic permeability), absorption and emission behavior, reflection and transparency.

[0030] In a preferred embodiment of the invention, the material property induced by the additive in the functional area or influenced by the additive is a chemical property. The chemical material property is preferably selected from the group consisting of: antimicrobial effect, flammability, corrosion resistance, solubility and acidity constant.

[0031] In a preferred embodiment of the invention, the material property induced by the additive in the functional area or influenced by the additive is a physiological material property. The physiological material property is preferably selected from the group consisting of: odor, taste and toxicity, in particular ecotoxicity.

[0032] A “fibrous material” is a material which has or consists of a linear, thread-like structure, which is therefore preferably part of a more complex surface structure such as a woven fabric, a nonwoven fabric, a laid scrim or a knitted fabric.

[0033] The matrix material of the composite material component according to the invention is used to embed at least partially, preferably completely, in the fiber material and optionally also to embed at least partially, preferably completely, in the additive and / or optionally to dissolve the additive at least partially, preferably completely. It holds the fibers of the fiber material in their position and transmits and distributes stresses between them. It is preferably a polymer material, in particular a thermosetting polymer material. It is preferably a polymer material made of a resin and a curing agent. In the preparation process, preferably accelerators, activators and release agents are used, which are therefore preferably part of the matrix material in the sense of the present invention.

[0034] For example, by integrating additives that cause or influence material properties, composite components with structural integrity and high mechanical stability can be obtained, while having other functions such as flame retardant activity. Using concentration gradients, the spatial distribution of material properties can be adapted to the specific application of the composite component, thereby eliminating the need for complex component structures that require increased manufacturing efforts. For example, flame retardant additives can be concentrated in subsections of functional areas that are particularly susceptible to fire or high thermal stresses. Another example is the accumulation of metal particles in subsections of functional areas, thereby affecting the electromagnetic properties of the composite component.

[0035] It is particularly preferred that the functional region has an integral character with another region, particularly preferably with all other regions of the composite component, ie an integral design of the composite component.

[0036] Composite components with fiber materials and additives have preferred monolithic properties, which avoids the breaking, detachment or separation of regions with different functions, especially layers, which is particularly common in specific 3D geometries, especially in very thin layers. Difficulties related to different thermal expansion of the individual layers can also be avoided. Avoiding the use of connecting elements (such as adhesives or rivets) also leads to a simple and stable structure.

[0037] Compared to the composite materials known from the prior art, which consist of a composite material layer and an additional functional layer, the functional region according to the invention can also be produced in a one-step process without subsequent connection or coating. This not only saves manufacturing costs, but also greatly simplifies the qualification of the components. In addition, the targeted control of the addition of additives can also reduce the total amount of additives required, which is particularly advantageous from an economic and ecological point of view.

[0038] The composite component is preferably composed of the functional region according to the invention. However, in another preferred embodiment of the invention, the composite component has other regions, in particular other functional regions. For example, the composite component can have two or more functional regions according to the invention with different additives.

[0039] In a preferred embodiment of the invention, the composite component has a multilayer sandwich structure, wherein preferably at least one, more preferably all, outermost layers are the functional region according to the invention, or the layers as a whole form the functional region. This means that, in the latter case, the functional region is formed by several layers, wherein each layer preferably has a substantially spatially constant concentration of additives, and preferably each layer is designed as a whole. The functional region formed by one or more layers can be connected to the rest of the composite component by positive locking or material bonding.

[0040] Furthermore, it is also possible to connect the monolithic design with the multilayer design, for example by combining a monolithic functional region formed by layers with a concentration gradient with a functional region formed by several layers of different concentrations.

[0041] Preferably, all regions of the composite component have the same matrix material. This makes the composite component particularly mechanically stable.

[0042] In a preferred embodiment, the volume ratio of matrix material to fiber material in the composite component is 8:1 to 1:10, preferably 5:1 to 1:8, particularly preferably 2:1 to 1:5.

[0043] In a preferred embodiment, the weight ratio of matrix material to fiber material in the composite component is from 5:1 to 1:20, preferably from 3:1 to 1:10, particularly preferably from 1:1 to 1:8.

[0044] In a preferred embodiment, the volume ratio of matrix material to additives in the composite component is from 100:1 to 1:5, preferably from 50:1 to 1:3, particularly preferably from 2:1 to 1:2.

[0045] In a preferred embodiment, the weight ratio of matrix material to additives in the composite component is from 100:1 to 1:10, preferably from 50:1 to 1:6, particularly preferably from 4:1 to 1:4.

[0046] In a preferred embodiment, the weight proportion of the fiber material to the total weight of the composite component is 10 to 95% by weight, preferably 20 to 90% by weight, more preferably 30 to 85% by weight, still more preferably 40 to 80% by weight, and most preferably 50 to 75% by weight.

[0047] In a preferred embodiment, the weight proportion of the additive to the total weight of the composite component is 0.05 to 50 wt%, preferably 0.1 to 25 wt%, more preferably 0.3 to 15 wt%, still more preferably 1.0 to 10 wt%, most preferably 2.0 to 5 wt%.

[0048] In a preferred embodiment, the volume ratio of matrix material to fiber material in the functional region is 8:1 to 1:15, preferably 2:1 to 1:10, particularly preferably 1:1 to 1:10.

[0049] In a preferred embodiment, the weight ratio of matrix material to fiber material in the functional region is 5:1 to 1:30, preferably 2:1 to 1:20, particularly preferably 1:1 to 1:15.

[0050] In a preferred embodiment, the volume ratio of matrix material to additive in the functional region is 100:1 to 1:20, preferably 50:1 to 1:6, particularly preferably 2:1 to 1:4.

[0051] In a preferred embodiment, the weight ratio of matrix material to additive in the functional region is from 100:1 to 1:20, preferably from 50:1 to 1:12, particularly preferably from 4:1 to 1:8.

[0052] In a preferred embodiment, the weight proportion of the optionally included fiber material to the total weight of the functional area is 20 to 80 wt %, preferably 25 to 70 wt %, more preferably 35 to 65 wt %, still more preferably 30 to 60 wt %, most preferably 30 to 55 wt %.

[0053] In a preferred embodiment, the weight proportion of the additive to the total weight of the functional region is 0.1 to 40 wt %, preferably 0.2 to 30 wt %, more preferably 0.5 to 20 wt %, still more preferably 1.0 to 10 wt %, most preferably 1.0 to 5 wt %.

[0054] The proportions of resin, fibers and pores are preferably determined as described in ISO 14127 (first edition, 2008).

[0055] The concentration gradient consists of a plurality of points. A "point" of the concentration gradient represents the concentration value of the additive in a non-intersecting volume element of the functional area, i.e. a point arranged centrally in a volume element is assigned the corresponding concentration value of the volume element. By connecting the points of different concentrations, it is possible to determine and set the spatial distribution of the concentration gradient, for example relative to the component extension, and thus determine its length L K .

[0056] The volume elements associated with the points of the concentration gradient are preferably obtained and defined in such a way that a part of the volume of the composite component (e.g. a functional area), preferably the entire volume of the composite component, is divided into volume elements of equal volume (i.e. a volume deviation of ≤5%, preferably ≤2%), and the concentration of the additive in each volume element is determined. The corresponding methods for analyzing the additive content of different additives are known to the person skilled in the art and are described in detail in conventional manuals, such as Taschenbuch der Kunststoff-Additive [Handbook of Plastic Additives], 3rd edition, Gächter, Müller, Carl Hanser Verlag, 1989, Chapter 20. The analysis can be carried out, for example, by incineration and / or dissolution of the component, as described in ISO 14127 (1st edition, 2008). The concentration values ​​associated with the points of the concentration gradient can thereby be determined. By comparing the concentration values ​​of the additive of different non-intersecting volume elements (e.g. layers or cubes), it can be determined whether there is a concentration difference, i.e. whether there is a concentration gradient with two or more points. The points associated with the corresponding concentration values ​​and thus representing the concentration in the volume element are arranged at the volume centroid of the volume element. The length L is obtained by connecting the points of different concentrations. K The point is preferably always connected from one point to the nearest point in space, i.e. on the shortest path. The volume of one of the disjoint volume elements is preferably the total volume V of the composite component. KB ≥1 / 50, more preferably ≥1 / 20×V KB , and more preferably ≥1 / 10×V KB , but preferably ≤1 / 5×V KB . In order to achieve a simple and feasible analysis, the composite material component is preferably divided into no more than 200, preferably no more than 100, more preferably no more than 50, and even more preferably no more than 10 volume elements of equal volume, and the concentration can be determined from these volume elements. The concentration gradient is preferably designed so that the concentration difference between two points arranged continuously along the length of the concentration gradient and representing different volume elements is ≥5%, more preferably ≥10%, even more preferably ≥15%, and even more preferably ≥20%, based on the higher concentration value in each case. This preferably applies to all adjacent concentration points of the concentration gradient. The concentration gradient preferably only has points with an additive concentration>0 and / or the functional area only contains volume elements with additives.

[0057] Preferably, the concentration value of the volume element with the highest concentration divided by the concentration value of the volume element with the lowest concentration is ≥2, preferably ≥5, more preferably ≥10, more preferably ≥20, most preferably ≥30 and / or its point spacing is ≥0.01×B E , preferably ≥0.05×BE .

[0058] In other preferred embodiments, a volume element represented by a point is obtained, which is defined by a layer of thickness D, which is removed from the composite component in each case by, for example, milling, and its concentration is then determined. The volumes of the removed layers are substantially the same (i.e., the volume deviation is ≤5%, preferably ≤2%). By comparing the concentrations of additives in different removed layers (i.e., non-intersecting volume elements), it is possible to determine whether there is a concentration difference, i.e., whether there is a concentration gradient. The thickness D of the measured layer is preferably ≤1 / 3 of the length of the concentration gradient, more preferably ≤1 / 5, still more preferably ≤1 / 10, most preferably ≤1 / 20, but it is also preferred that D ≥ 1 / 100 of the length of the concentration gradient. The volume of the layer is preferably the total volume V of the composite component. KB ≥1 / 50, more preferably ≥1 / 20×V KB , and more preferably ≥1 / 10×V KB , but preferably ≤1 / 5×V KB The layer density is preferably ≥0.05 mm, more preferably ≥0.1 mm, more preferably ≥3 mm, still more preferably ≥5 mm, but also preferably ≤5 cm. Preferably, the layer density D is ≥0.0001×B E , preferably D ≥ 0.0004 × B E , preferably D ≥ 0.0006 × B E , more preferably D ≥ 0.0008 × B E , and more preferably D ≥ 0.001 × B E , and more preferably D ≥ 0.005 × B E , the most preferred D ≥ 0.01 × B E ; but it is also preferred that D≤0.01×B E .

[0059] The concentration gradient is preferably designed such that the concentration difference between two points arranged consecutively along the length of the concentration gradient and representing different volume elements is ≥ 5%, more preferably ≥ 10%, even more preferably ≥ 15%, even more preferably ≥ 20%, based on the higher concentration value in each case. This preferably applies to all adjacent concentration points of the concentration gradient.

[0060] For example, a concentration gradient can be formed from 10 concentration values ​​representing the concentrations of 10 removed layers with a respective layer thickness of 1 mm, wherein the respective points representing the concentrations in the respective layers always have a concentration difference of at least 20%. The above-described layer-by-layer removal for determining the concentration gradient is particularly suitable for the case of sheet-like composite components such as fireproof panels.

[0061] Particularly in the case of complex structures or if the functional area is small relative to the composite component, the gradient can also be obtained and defined by cutting out cube-shaped elements from the composite component, the side length of the cube-shaped elements preferably being ≤ 1 / 3 of the length of the concentration gradient, more preferably ≤ 1 / 5, still more preferably ≤ 1 / 10, most preferably ≤ 1 / 20, but also preferably ≥ 1 / 100 of the length of the concentration gradient. The volumes of the cubes are substantially equal (i.e. the volume deviation is ≤ 5%, preferably ≤ 2%). The volume of the cubes is preferably ≥ the total volume V of the composite component. KB 1 / 50, more preferably ≥1 / 20×V KB , and more preferably ≥1 / 10×V KB , but preferably ≤1 / 5×V KB The side length of the corresponding cube is preferably ≥0.5 mm, more preferably ≥1 mm, more preferably ≥3 mm, still more preferably ≥5 mm, but also preferably ≤5 cm. Preferably, the side length of the cube is ≥0.0001×B E , preferably ≥0.0004×B E , more preferably ≥0.0006×B E , more preferably ≥ 0.0008 × B E , and more preferably ≥ 0.001 × B E , and more preferably ≥ 0.005 × B E , preferably ≥ 0.01 × B E ; However, the side length is also preferably ≤0.01×B E For example, a concentration gradient can be formed by 10 concentration values ​​representing the concentration of 10 cut-out cubes with a side length of 1 mm, wherein the corresponding points arranged in the middle of the cubes representing the concentration in the corresponding cubes always have a concentration difference of at least 20%.

[0062] The concentration gradient is preferably designed such that the concentration difference between two points arranged consecutively along the length of the concentration gradient and representing different volume elements is ≥ 5%, more preferably ≥ 10%, even more preferably ≥ 15%, even more preferably ≥ 20%, based on the higher concentration value in each case. This preferably applies to all adjacent concentration points of the concentration gradient.

[0063] In a preferred embodiment of the present invention, the concentration values ​​of the concentration gradient are distributed along its space, i.e., its length L K In a preferred embodiment of the invention, the concentration gradient increases or decreases continuously at least partially, preferably completely. K More than 10%, preferably more than 20%, more preferably more than 40%, more preferably more than 60%, and most preferably more than 75% of the concentration gradient has a continuous concentration value distribution. Because the concentration value distribution of the concentration gradient is continuous, segregation effects and predetermined breaking points in the functional area are avoided, thereby improving the strength and resistance of the material.

[0064] In a preferred embodiment, the concentration gradient is K The concentration gradient has at least partially, preferably completely, a monotonically increasing curve of concentration values, i.e., the concentration at each measuring point is higher than the concentration at the previous measuring point. In another preferred embodiment, the concentration gradient has a length L K The concentration at least partially, preferably completely, has a monotonically decreasing curve, ie the concentration at each measuring point is lower than at the preceding measuring point.

[0065] The concentration gradient is K The above embodiment has a distribution of concentration values, which is at least partially, preferably completely, selected from the group consisting of linear increase, stepwise increase, stepwise decrease, non-linear increase, linear decrease, exponential decrease, exponential increase and non-linear decrease.

[0066] In a preferred embodiment of the invention, the composite component has a maximum component extension B E , which is defined by the maximum distance between two points of the component, and the concentration gradient has a length L K , where L K ≥0.05×B E , preferably L K ≥0.2×B E , more preferably L K ≥0.3×B E , more preferably L K ≥0.4×B E , and more preferably L K ≥0.6×B E , most preferably L K ≥0.75×B E .

[0067] In a preferred embodiment of the present invention, the functional area has a maximum functional area extension FB E , which is defined by the maximum distance between two points of the functional region, and the concentration gradient has a length L K , where L K ≥0.05×FB E , preferably L K ≥0.2×FB E , more preferably L K ≥0.3×FB E , more preferably L K ≥0.4×FB E , and more preferably L K ≥0.6×FB E , most preferably L K ≥0.75×FB E .

[0068] Since the continuous concentration gradient preferably extends as widely as possible, a transition between regions of different concentrations of additive that is as uniform as possible is achieved. As a result, the composite component has enhanced structural integrity and strength.

[0069] The composite component is preferably a board such as a fireproof board. In this case, the concentration gradient is preferably along the height H of the board. B Preferably, the concentration gradient, particularly for this case, has a length L K , where L K ≥0.05×H B , preferably L K ≥0.2×H B , more preferably L K ≥0.3×H B , more preferably L K ≥0.4×H B , and more preferably L K ≥0.6×H B , the most preferred K ≥0.75×H B In other preferred embodiments, the concentration gradient is along the length L of the plate. B Preferably, the concentration gradient, particularly for this case, has a length L K , where L K ≥0.001×L B , preferably L K ≥0.004×L B , more preferably L K ≥0.006×L B , more preferably L K ≥0.008×L B , and more preferably L K ≥0.012×L B , the most preferred K ≥0.015×L B In other exemplary embodiments, the concentration gradient is along the width B of the plate. B Preferably, the concentration gradient, particularly for this case, has a length L K , where L K ≥0.001×B B , preferably L K ≥0.004×B B , more preferably L K ≥0.006×B B , more preferably L K ≥0.008×B B , and more preferably L K ≥0.01×B B, the most preferred K ≥0.012×B B In the above-mentioned embodiments, the concentration gradient preferably has only points with an additive concentration > 0, i.e. the distribution of the concentration values ​​along the gradient differs completely from zero in spatial distribution, and / or the functional area and the optional composite component are designed as one piece, preferably solidified as one piece. Combinations of the above-mentioned preferred embodiments are also possible and preferred, in which the concentration gradient has components along 2 or 3 plate axes (length, width, height) in each case.

[0070] The concentration gradient preferably has at least three points with different concentration values, preferably at least five points, even more preferably at least ten points, even more preferably at least 20 points, most preferably at least 50 points, wherein the points are preferably evenly spaced. The concentration gradient is then preferably designed such that the concentration difference between two points arranged consecutively along the length of the concentration gradient and representing different volume elements, based on the higher concentration value in each case, is ≥5%, more preferably ≥10%, even more preferably ≥15%, even more preferably ≥20%. This preferably applies to all adjacent concentration points of the concentration gradient. Particularly preferably, in this case, the concentration gradient has the above-mentioned concentration gradient with respect to the component extension B E and / or functional area extension FB E and / or a length L defined by one of the above distributions K Preferably, none of the concentration points forming the gradient are arranged within the optional fiber material.

[0071] Preferably, the concentration gradient is arranged completely within the functional area and particularly preferably corresponds to the functional area extension FB E concentration gradient.

[0072] In a preferred embodiment of the invention, the concentration gradient has a distribution of concentration values ​​with at least two differently designed partial regions. For example, the distribution of concentration values ​​of the concentration gradient can first decrease linearly and then increase stepwise. This makes it possible to achieve complex concentration distributions in the composite component. Preferably, the concentration gradient has partial regions with different inclinations.

[0073] In a preferred embodiment of the present invention, the concentration gradient has a maximum concentration point C max and the lowest concentration point C min , where C max / C min ≥2, preferably ≥5, more preferably ≥10, even more preferably ≥20, most preferably ≥30. Higher local differences in the material properties caused or influenced by the additive in the functional layer can be achieved by a correspondingly steep gradient in the concentration values.

[0074] Particularly preferred is the point C where the concentration gradient is at its highest concentration. max and the lowest concentration point Cmin With minimum distance L Cmax->min An embodiment in which L Cmax->min ≥0.05×B E , preferably L Cmax->min ≥0.2×B E , more preferably L Cmax->min ≥0.3×B E , more preferably L Cmax->min ≥0.4×B E , and more preferably L Cmax->min ≥0.5×B E .

[0075] However, for other applications it is also advantageous that, despite the presence of a gradient in the functional area, the local concentration differences are limited. Therefore, in another preferred embodiment of the present invention, C max / C min ≤2, preferably ≤5, even more preferably ≤10, even more preferably ≤20, most preferably ≤30.

[0076] In a preferred embodiment of the present invention, C max / C min The range of is 1.5-50, preferably 3-30, still more preferably 5-25, still more preferably 5-20, and most preferably 7-15.

[0077] In the above preferred embodiments, the composite component particularly preferably has a maximum component extension B E , which is defined by the maximum distance between two points of the component, and the concentration gradient preferably has a length L K , where L K ≥0.05×B E , preferably L K ≥0.2×B E , more preferably L K ≥0.3×B E , more preferably L K ≥0.4×B E , and more preferably L K ≥0.6×B E , the most preferred K ≥0.75×B E .

[0078] Preferably, the concentration gradient is designed such that the concentration of the additive increases on one, more than one or all surfaces of the composite component and decreases towards the interior, or vice versa.

[0079] Therefore, in a preferred embodiment of the invention, the concentration gradient is at least partially parallel to or extends to an orthogonal projection of one of the outer surfaces of the functional area; in this case, it is particularly preferred that the concentration of the additive increases at least partially, preferably continuously, towards one outer surface. In the meaning of the invention, an orthogonal projection is an image of a point on a plane forming one outer surface of the composite component, such that the connecting line between the point and its image forms a right angle with the plane. The distance between the image and the starting point of all points on the plane is then the shortest.

[0080] The concentration gradient is preferably designed so that the gradient C max The highest concentration point is arranged at or close to all points closest to the outer surface, that is, the distance from all points closest to the outer surface does not exceed 0.1×B E "External surface" is understood to mean a surface which is not adjacent to other regions of the composite component and thus delimits the composite component to the outside. In a preferred embodiment of the invention, the functional area has two or more concentration gradients, wherein the two or more concentration gradients are preferably designed such that the concentration of the additive increases towards the same external surface.

[0081] This arrangement is particularly preferred because additives are often used to control material properties that have a specific functional relationship with the outer surface. For example, additives can be used to improve impact resistance and are therefore particularly preferably concentrated at or near an outer surface. This embodiment is particularly preferred, particularly when the additives are to be subjected to further heat treatment such as carbonization after introduction into the composite component.

[0082] In another preferred embodiment, the concentration gradient is designed so that the point of highest concentration is arranged in the center of the component, i.e. at a distance ≥ 0.1×B from the nearest or all outer surfaces. E , preferably ≥0.2×B E In the case of a block-shaped or cuboid component, the above-mentioned spacing preferably exists relative to two or more outer surfaces.

[0083] In a preferred embodiment of the invention, the functional area is a fire protection area and for this purpose has a flame retardant as an additive in order to reduce the flammability of the functional layer.

[0084] In this case, the flame retardant is particularly preferably selected from: halogenated and / or nitrogen-based flame retardants, inorganic flame retardants such as graphite salts, aluminum hydroxide, antimony trioxide, ammonium polyphosphate, aluminum diethylphosphinate, mica, muscovite, guanidine, triazine, sulfates, borates, cyanurates, their salts, and mixtures thereof.

[0085] In other preferred embodiments, the additives are selected from: antioxidants; light stabilizers, in particular UV stabilizers; plasticizers, foaming agents, electrical conductors, thermal conductors, dyes; fillers for improving mechanical properties such as impact modifiers or rubber or thermoplastic particles; and mixtures of the above substances.

[0086] The additive can be present in the matrix material in dissolved or dispersed form. If it is dispersed, it is preferably present in the form of powder, flakes, tubes or a mixture of the above forms.

[0087] If the additive is a flame retardant, it is preferably selected from active flame retardants, ie cooling flame retardants, or passive flame retardants, ie insulating flame retardants. Particularly preferably, the flame retardant is an intumescent flame retardant.

[0088] Like any other regions, the functional region can have further additives. In particular, the functional region can have a plurality of different additives with different, preferably continuous, concentration gradients.

[0089] In a preferred embodiment of the present invention, the matrix material comprises or is a polymer matrix material, which particularly preferably has one or more thermosetting materials. Preferably, the matrix material is a polymer matrix material selected from the group consisting of polyurethane; polyvinyl chloride, in particular polyvinyl chloride rigid foam; and phenolic resins and epoxy resins.

[0090] In a preferred embodiment of the invention, the fiber material at least partially, preferably completely, has a surface structure, preferably a textile surface structure.

[0091] Particularly preferably, the surface structure is selected from a laid scrim, a knitted fabric, a woven fabric, a braid, a nonwoven or a mixture thereof.

[0092] According to the invention, a nonwoven is understood to mean a structure of fibers of finite length, continuous fibers (filaments) or cut yarns of any type and any origin, which are connected in some way to form a fiber layer and are connected to each other in some way. It does not include the crossing or entanglement of the yarns, as occurs in the manufacture of weaving, knitting, weaving, lace weaving, plaiting and tufting products. This definition corresponds to standard DIN EN ISO 9092. According to the invention, the term nonwoven also covers felt materials. However, films and papers do not belong to nonwovens.

[0093] In the context of the present invention, plaiting is understood to mean the regular interweaving of a plurality of strands made of a flexible material. The difference from weaving is that in plaiting the threads are not fed at right angles to the main manufacturing direction of the product.

[0094] According to the invention, a woven fabric is understood to mean a textile fabric consisting of two thread systems, namely warp (warp) and weft (weft), which intersect in a pattern at an angle of exactly or approximately 90°, as seen from the fabric surface. The two systems can each consist of a variety of warp or weft types (e.g. basic warp, pile warp and filling warp; basic weft, hemming weft and filling weft). The warp threads extend in the longitudinal direction of the woven fabric, parallel to the selvedge, and the weft threads extend in the transverse direction, parallel to the fabric edge. The threads are connected to the woven fabric primarily by friction engagement. In order for the woven fabric to be sufficiently non-slip, the warp threads and weft threads usually have to be woven relatively tightly. Therefore, with a few exceptions, the woven fabric also has a closed fabric appearance. This definition corresponds to standard DIN 61100, part 1.

[0095] According to the invention, the terms "woven fabric" and "nonwoven fabric" also include textile materials which have been tufted. Tufting is a method of anchoring yarns into a woven or nonwoven fabric using a machine operated by compressed air and / or electricity.

[0096] According to the invention, knitted fabrics are understood to mean textile materials produced from a thread system by knitting. These materials include crocheted materials and knitted materials.

[0097] According to the invention, a laid scrim is understood to mean a fabric consisting of one or more layers of parallel stretched threads. The threads are usually fixed at the intersections. The fixing is carried out by material bonding or mechanical friction and / or positive locking. The laid scrim is preferably selected from uniaxial or unidirectional, biaxial or multiaxial scrims.

[0098] Preferably, the fiber material has an anisotropic structure, ie, in the functional layer according to the invention, the fibers have a specific fiber orientation, thereby enabling an anisotropic mechanical behavior of the layered composite material to be produced.

[0099] The fiber material is preferably selected from the group consisting of glass fibers, carbon fibers, ceramic fibers, basalt fibers, boron fibers, steel fibers; polymer fibers, such as synthetic fibers, in particular aramid fibers and nylon fibers or natural fibers, in particular natural polymer fibers. Natural fibers are understood to mean fibers which originate from natural sources such as plants, animals or minerals and which can be used directly without further chemical conversion reactions. Examples according to the invention are flax or ramie fibers and protein fibers or cotton. According to the invention, regenerated fibers, i.e. fibers which are produced by chemical processes from naturally occurring renewable raw materials, can also be used.

[0100] In a preferred embodiment of the invention, all additives located in the composite component are present substantially in the functional region, i.e. ≥70% by weight, preferably ≥80% by weight, even more preferably ≥90% by weight and most preferably completely in a spatially delimited first subdivision of the functional region. The first subdivision preferably at least partially, preferably completely surrounds at least one outer surface of the composite component. If the composite component has more than one functional region, the above weight proportions and the following volume fractions preferably relate to one or more than one functional region.

[0101] In a preferred embodiment of the present invention, the volume V of the first sub-portion in which the additive of the functional region is substantially located T1 Total volume of functional area V FB A considerable portion of. Preferably V T1 ≥0.1×V FB , more preferably V T1 ≥0.3×V FB , and more preferably V T1 ≥0.5×V FB , and more preferably V T1 ≥0.7×V FB , the most preferred T1 ≥0.9×V FB .

[0102] In a preferred embodiment of the present invention, which is preferably combined with the above preferred embodiment, the functional area has a second subsection where no additive is present. The volume V of the second subsection T2 Preferably V T2 ≤0.7×V FB , more preferably V T2 ≤0.5×V FB , more preferably V T2 ≤0.3×V FB , and more preferably V T2 ≤0.2×V FB , the most preferred T2 ≤0.1×V FB .

[0103] In a further particularly preferred embodiment, all additives present in the composite component are arranged substantially, preferably completely, in the functional region.

[0104] In a preferred embodiment of the invention, the volume V of the subsection in which the additive of the functional region is substantially located T1 Relative to the total volume V of the functional area FB Smaller. Preferred V T1 ≤0.7×V FB , more preferably V T1 ≤0.5×VFB , more preferably V T1 ≤0.3×V FB , and more preferably V T1 ≤0.2×V FB , the most preferred T1 ≤0.1×V FB .

[0105] In a preferred embodiment of the present invention, which is preferably combined with the above preferred embodiment, the functional area has a second subsection where no additive is present. The volume V of the second subsection T2 Preferably V T2 ≥0.1×V FB , more preferably V T2 ≥0.2×V FB , more preferably V T2 ≥0.3×V FB , and more preferably V T2 ≥0.5×V FB , the most preferred is V T2 ≥0.7×V FB .

[0106] Preferably, the volume of the functional area accounts for more than 50% of the volume of the composite component, more preferably more than 65%, more preferably more than 75%, more preferably more than 90%, most preferably more than 95% or even 100%. For these cases, the composite component is particularly preferably designed as a single piece, preferably cured as a single piece.

[0107] In a preferred embodiment of the present invention, the volume V of the first sub-portion in which the functional region additive is substantially located T1 Total volume of composite components V KB A considerable portion of. Preferably V T1 ≥0.1×V KB , more preferably V T1 ≥0.3×V KB , and more preferably V T1 ≥0.5×V KB , and more preferably V T1 ≥0.7×V KB , the most preferred T1 ≥0.9×V KB .

[0108] In a preferred embodiment of the present invention, which is preferably combined with the above preferred embodiment, the functional area has a second subsection where no additive is present. The volume V of the second subsection T2 Preferably V T2 ≤0.7×V KB , more preferably V T2≤0.5×V KB , more preferably V T2 ≤0.3×V KB , and preferably V T2 ≤0.2×V KB , the most preferred is V T2 ≤0.1×V KB .

[0109] In a preferred embodiment of the invention, the volume V of the subsection in which the additive of the functional region is substantially located T1 Relative to the total volume V of the composite component KB Smaller. Preferred V T1 ≤0.7×V KB , more preferably V T1 ≤0.5×V KB , more preferably V T1 ≤0.3×V KB , and more preferably V T1 ≤0.2×V KB , the most preferred T1 ≤0.1×V KB .

[0110] In a preferred embodiment of the present invention, which is preferably combined with the above preferred embodiment, the functional area has a second subsection where no additive is present. The volume V of the second subsection T2 Preferably V T2 ≥0.1×V KB , more preferably V T2 ≥0.2×V KB , more preferably V T2 ≥0.3×V KB , and more preferably V T2 ≥0.5×V KB , the most preferred is V T2 ≥0.7×V KB .

[0111] Preferably, the volume of the functional area accounts for more than 50% of the volume of the composite component, more preferably more than 65%, more preferably more than 75%, more preferably more than 90%, and most preferably more than 95%. For this case, the composite component is particularly preferably designed as a single piece, preferably cured as a single piece.

[0112] In a particularly preferred embodiment, the functional region has only a volume portion containing the additive, namely V T1 =V FB , and / or composite components are composed of functional regions, i.e. V FB =V KB .

[0113] Particularly preferably, the additive is present in a volume V FB The content of the precipitate is ≥70 wt %, preferably ≥80 wt %, still more preferably ≥90 wt %, still more preferably ≥95 wt %, and most preferably completely exists in the volume V FB middle.

[0114] The composite component according to the invention is preferably a composite component of a motor vehicle component, a building component, an aircraft or spacecraft or a rail vehicle or a part of the aforementioned components.

[0115] In a preferred embodiment, the motor vehicle component formed by the composite component or of which the composite component is a part is a component of a battery housing, particularly preferably a floor panel or a cover panel. Further preferred motor vehicle components are selected from the group consisting of: luggage compartment floors, dashboards, door and roof claddings, underbody protection parts, structural components, wheel covers, engine compartment components, brake and clutch linings and discs, sound insulation materials, shear panels and seals.

[0116] In other preferred embodiments of the present invention, the composite material component is a part of an aircraft or spacecraft such as an airplane. In this context, preferred parts are tail rotor blades, main rotor hub plates, engine components, fuel tanks, fuselage structures, fire protection elements such as fire protection layers, rotating parts, turbine blades and wings.

[0117] In a further preferred embodiment of the invention, the composite component is a building component, for example for a wind turbine. In this context, preferred components are: rotor blades of a wind turbine, in particular structural and skin components of the "nacelle", wiring, pipes; walls and roofs.

[0118] The present invention also relates to a method for manufacturing one of the above-mentioned composite material components, comprising the following steps:

[0119] I) providing a composition for forming a composite component in a forming tool such as a die, the composition comprising or consisting of:

[0120] a) fibrous materials;

[0121] b) one or more precursor compounds of the matrix material;

[0122] c) additives, preferably flame retardants;

[0123] II) applying a predetermined pressure and a predetermined temperature to the composition to obtain a composite component, the predetermined pressure being preferably applied by pressing.

[0124] Step I) preferably comprises one, more or all of the following sub-steps:

[0125] a) providing one or more layers of fiber material in a forming tool, for example by a hand layup process;

[0126] b) providing one or more precursor compounds of the matrix material;

[0127] c) providing one or more additives, preferably dissolved in one or more precursor compounds;

[0128] d) contacting one or more precursor compounds of the matrix material with the fiber material, preferably by spraying;

[0129] e) At least partial reaction of the system of one or more precursor compounds, such as resin, hardener and optionally release agent, to give the matrix material (=curing).

[0130] In the method according to the invention, the additive can generally be introduced into the functional region by the following method measures:

[0131] i) the fiber material used can be provided with additives, for example by applying an additive solution or applying an additive powder, which additives can optionally be provided together with a binder for better adhesion to the fiber material;

[0132] ii) the additive is preferably introduced into one or more precursor compounds in dissolved and / or dispersed form;

[0133] iii) introducing the additive into a forming tool which is unfilled or partially or completely filled with one or more precursor compounds.

[0134] Locally changing the material properties by changing the distribution of additives in the matrix material can be achieved, for example, by the following operations:

[0135] i) different local accumulations of additives on the fiber material or the prepreg introduced into the forming tool;

[0136] ii) varying the concentration of additives present in dissolved and / or dispersed form in one or more precursor compounds during introduction into the forming tool;

[0137] iii) locally and gradually introducing the additive into the at least partially filled forming tool before, during or after the reaction of the one or more precursor compounds.

[0138] The predetermined pressure in step II) of the method defined in claim 15 is preferably in the range of 1 bar to 1000 bar, particularly preferably 5 bar to 500 bar, still more preferably 10 bar to 100 bar, most preferably 20 bar to 50 bar.

[0139] The predetermined temperature in step II) of the method defined in claim 15 is preferably in the range of 10°C to 900°C, particularly preferably 15°C to 700°C, still more preferably 20°C to 500°C, most preferably 25°C to 200°C.

[0140] Particularly preferably, the method for producing a composite component according to the invention is a wet pressing method. In this method, a liquid reaction resin is processed as a precursor compound together with the reinforcing fibers in a two-part mold. The upper mold part and the lower mold part are closed by a press.

[0141] During the wet pressing process, the resin is usually poured onto the fiber mat in one go or according to a fixed pouring time schedule. In this step, the additives can be added at different time points, wherein the concentration of the additives is preferably varied.

[0142] In most cases, polyurethane, epoxy or polyamide systems are used, which are formed from two or more precursor compounds which are mixed in a special mixing head to form a reactive liquid plastic material. Flat plate moulds or other dispenser systems are preferably used for planar application on the fibre mat.

[0143] The fiber mat is preferably laid out as a fiber blanket. This method is characterized by a particularly high efficiency.

[0144] Under the pressure of the press, the plastic is distributed throughout the mold by the mold closing process and wets the reinforcement fibers. At the same time or afterwards, the plastic / resin cures - usually at high temperatures. If the plastic cures, this will provide dimensional stability to the component and enable demoulding after the mold is opened.

[0145] The additives are preferably introduced into the functional layer by mixing into one or more precursor compounds of the matrix material. By varying the proportions of the additives, a concentration gradient can be generated when the matrix material is fed into the forming tool.

[0146] In the method for manufacturing a composite component according to the invention, the fiber mat can be preformed to form a so-called preform, in particular when the geometric complexity increases.

[0147] The invention also relates to the use of a composite component as defined in the claims and sections herein as a motor vehicle component, a building component, a composite part for an aircraft or spacecraft, a rail vehicle component or a part of the aforementioned components.

[0148] Particular preference is given to use as a component of a battery housing, in particular for lithium-ion batteries.

[0149] The invention also relates to the use of concentration gradients of additives in composite components, preferably designed in one piece, to obtain locally varying material properties of the composite component, in particular locally varying flammability or locally varying shielding properties.

[0150] The invention also relates to the use of concentration gradients of additives within a matrix material in a composite component to obtain locally varying material properties of the composite component. BRIEF DESCRIPTION OF THE DRAWINGS

[0151] The present invention will be described in more detail below with reference to exemplary embodiments shown in the accompanying drawings.

[0152] Figure 1 A composite component 1 is shown, which is formed in one piece and consists of a functional region, which contains a fiber material, a matrix material and an additive. The fiber material is illustrated as a horizontal line. In order to simplify the illustration, the fiber material embedded in the matrix material is not explicitly shown. The concentration of an added additive, such as a flame retardant additive, increases continuously in the direction of the arrow. This is reflected by the increasing shadow of the composite component.

[0153] Figure 2 A composite component 1 formed from several sheets is shown, wherein the layers 2, 3 and 4 containing the additive each have a different but constant intra-layer concentration. The concentration of the additive is higher in layer 2 than in layer 3, which in turn is higher than in layer 4. This results in a higher concentration of the additive towards the upper outer surface of the composite component, resulting in an increased development of properties caused by or affected by the additive.

[0154] Figure 3 A composite component 1 is shown in which the additive is arranged in a subsection of the functional area.

[0155] Figure 4 A composite component 1 is shown in which two different additives are arranged in two different subsections. DETAILED DESCRIPTION

[0156] Figure 1 By way of example, a composite component according to the invention is schematically shown, which can be used, for example, as a cover or base of a battery housing for an electric vehicle. Depending on the arrangement of the battery cells in the housing, if a battery fire occurs, specific areas of the cover are exposed to particularly high temperatures and these parts of the cover require a particularly high concentration of flame retardant additives.

[0157] To manufacture this composite component, multiple layers of carbon fiber multiaxial fabric are cut to the size of the cover or base to be manufactured and then stacked on top of each other. During the design process, the total grammage of the textile and the distribution of the proportions of different fiber directions (e.g. below 0°, ±45° and 90° relative to the longitudinal axis of the vehicle) are determined based on the mechanical and other stresses on the cover. In a simple basic structure, the proportions in the travel directions of 0°, -45°, 45° and 90° are equal, resulting in a so-called quasi-isotropic laminate.

[0158] The resin-hardener mixture of epoxy resin is evenly distributed over the layer stack. In areas that are subject to particularly high temperatures, for example in the middle of the subsequent component, a high concentration of a fireproofing additive such as aluminum hydroxide is mixed into the resin, while in the edge areas where stress is less, only a low concentration of the additive is added. This creates a concentration gradient of the additive. The layer stack is now placed in a press and compressed between two mold halves that have the geometry of the subsequent component. The resin (including the additive in the middle area) is pressed into the layer stack and the reinforcing fibers are embedded in the resin-additive mixture. Sufficient press closing force ensures that the layer stack is compressed to the appropriate component thickness. The increased temperature of the mold halves accelerates the reaction of the resin and hardener components of the epoxy resin, causing them to react within a short time to form a matrix material.

[0159] The component is then removed from the mold and sent to the final processing steps.

[0160] Reference numerals

[0161] 1: Composite components

[0162] 2: Additive concentration is C a Layer

[0163] 3: Additive concentration is C b Layer

[0164] 4: Additive concentration is C c Layer

[0165] 5: First subdivision with first additive

[0166] 6: Second Division with Second Additive

Claims

1. A composite material component, comprising the following components: a) fibrous materials; b) matrix material; and c) a functional region in which an additive is arranged, which additive causes or influences material properties, in particular optical, thermal, mechanical and / or electromagnetic material properties, in said functional region, It is characterized in that The functional region has a concentration gradient of the additive, so that the material property caused by or affected by the additive is exhibited to different degrees in the functional region. 2 . The composite component according to claim 1 , wherein the concentration gradient is designed such that the concentration of the additive increases at least partially, preferably completely, in the direction of one of the functional regions and / or the outer surface of the composite component. 3 . The composite component according to claim 1 , wherein the concentration values ​​of the concentration gradient continuously increase or decrease at least in sections, preferably completely, along the spatial distribution of the concentration gradient. 4 . The composite component according to claim 1 , wherein the concentration gradient has at least two portions with different concentration value distributions in the two portions.

5. The composite component according to any one of the preceding claims, wherein the concentration gradient is designed such that it contains a point of maximum concentration C max and the lowest concentration point C min , where C max / C min ≥5, preferably ≥10. 6 . The composite component according to claim 1 , wherein the concentration gradient is at least partially parallel to or extends to an orthogonal projection of one of the functional regions and / or the outer surface of the composite component.

7. A composite component according to any one of the preceding claims, wherein the functional region is a fire protection region, the additive is a flame retardant, and the material property caused by or affected by the additive is flammability.

8. The composite component according to claim 7, wherein the flame retardant is selected from: halogenated and / or nitrogen-based flame retardants, inorganic flame retardants such as graphite salts, aluminum hydroxide, antimony trioxide, ammonium polyphosphate, aluminum diethylphosphinate, mica, muscovite, or mixtures thereof.

9. The composite component according to any of the preceding claims, wherein the additive is dispersed in the matrix material, preferably in the form of a powder, flakes, tubes or a mixture thereof. 10 . The composite component according to claim 1 , wherein the matrix material contains or is a polymer matrix material, which is particularly preferably a thermosetting material.

11. A composite component according to any of the preceding claims, wherein the fiber material at least partially, preferably completely, has a preferred textile surface structure, the textile surface structure being selected from a laid scrim, a woven fabric, a non-woven fabric or a mixture thereof, wherein the fiber material is preferably selected from: glass fibers, carbon fibers, basalt fibers, ceramic fibers, steel fibers, polymer fibers, such as synthetic fibers, in particular aromatic polyamide and nylon fibers, or natural polymer fibers such as flax fibers, ramie fibers or protein fibers. 12 . The composite component according to claim 1 , wherein the functional region at least partially surrounds at least one outer surface of the composite component. 13 . The composite component according to claim 1 , wherein the composite component is designed in one piece and / or the functional area accounts for ≥ 30%, preferably ≥ 50%, of the volume of the composite component.

14. A motor vehicle component or a building component comprising the composite component according to any one of the preceding claims, wherein the motor vehicle component is preferably a component of a battery housing, particularly preferably a floor panel or a cover panel.

15. A method of manufacturing a composite component according to any one of the preceding claims, the method comprising the steps of: I) providing a composition for forming a composite component in a forming tool such as a die, the composition comprising or consisting of: a) fibrous materials; b) a precursor compound of a matrix material; and c) additives, preferably flame retardants; II) applying a predetermined pressure and a predetermined temperature to the composition to obtain the composite component.

16. The method according to claim 15, wherein the method is a wet pressing method.

17. Use of a composite component according to any of the preceding claims as or in a motor vehicle component, preferably as part of a battery housing.

Citation Information

Patent Citations

  • Metal matrix composite materials containing carbon nanotube-infused fiber materials and methods for production thereof

    CN102639321A

  • Polymer material containing flame retardant adopting gradient concentration distribution

    CN106009539A

  • Epoxy composition

    CN113544198A