Substrate comprising base and integrated getter film for manufacturing microelectronic device
By using Zr-V-Al or Zr-V-Fe getter films in microelectronics, microphotoelectrics and micromechanical devices, combined with sputtering technology and PVD deposition, rapid and effective gas control at low temperatures is achieved, and absorption is solved The problem of high activation temperature of gas agent materials reduces manufacturing costs and complexity, and improves manufacturing efficiency and product quality.
Patent Information
- Application Number
- CN202380028543.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-05
AI Technical Summary
Prior Art In the manufacture of microelectronics, microphotoelectrics and micromechanical devices, high activation temperatures of getter materials may cause damage to the device components, and traditional methods increase system cost and complexity, making it difficult to effectively control gases at low temperatures, especially It is the absorption of carbon oxides and carbon dioxide.
Use getter films with 65-80 atomic % Zr, 15-25 atomic % V, 2-15 atomic % Al or Fe, and deposited by sputtering technology. The surface roughness is 2nm to 20nm and the thickness is 500nm to 10μm, the substrate thickness is 20μm to 5mm, combined with PVD deposition technology, low temperature (250℃ to 300℃) and short-term (no more than 20 minutes) activation is achieved, reducing energy consumption and internal surface degassing substances in the activation process.
It realizes rapid and efficient control of gas at low temperatures, reduces the absorption of carbon oxides and carbon dioxide, avoids power consumption in device damage and sealing processes, improves manufacturing efficiency and production, and reduces the use of cobalt and avoids toxicity problems. .
Smart Images

Figure BDA0005049038000000051
Abstract
Description
[0001] The invention relates to a substrate for producing a microelectronic device, a micro-optoelectronic device or a micromechanical device, comprising a base and an integrally coated getter film.
[0002] One of the main technical issues associated with microelectromechanical systems (MEMS), also known as integrated electronic circuits (ICs), is related to their packaging solutions, as many devices require a vacuum and / or a controlled atmosphere to function properly and maintain their lifetime, which can be as long as 15 or 20 years.
[0003] In some types of integrated circuits such as ferroelectric memories, controlling the diffusion of gases (especially hydrogen) is critical to avoid corrosion throughout the ferroelectric material.
[0004] In this area, IR sensors and microbolometers also require specific control and elimination of gases. For example, in the case of IR sensors, these gases can absorb part of the incident radiation or transfer heat by convection from the window to the pixel array that constitutes the sensing element of the device, with relevant consequences for the measurement accuracy and, in the worst case, cause the device to malfunction or not function at all.
[0005] The most common solution to maintain the internal pressure of a sealed device and simultaneously control and remove gases entering the MEMS device involves the use of getter materials. These materials are typically represented by metals such as zirconium, titanium, vanadium, niobium, tantalum, or alloys thereof that may further contain transition elements, rare earths, or aluminum, which have a strong chemical affinity for gases such as hydrogen, oxygen, water, carbon oxides, and in some cases nitrogen.
[0006] One of the main challenges associated with the need to have getter materials inside MEMS devices is represented by the small size required for these sensors; said problem can be solved, for example, by introducing a thin film getter inside the volume of the device.
[0007] The getter film can be deposited using a sputtering technique which is particularly advantageous when applied to the manufacture of supports with integrated getter materials to be used for the production of microelectronic devices, such as those described in patents US Pat. No. 7,180,163 and US Pat. No. 6,897,551 (both in the name of the applicant).
[0008] Furthermore, US20090301610 describes a method for depositing a thin film of a metal alloy on a substrate and the associated metal alloys.
[0009] It is important to point out that standard systems require a heating process to activate the getter material, which is typically in the range of 400°C to 900°C, depending on the getter composition. Unfortunately, these activation temperatures may lead to damage and destruction of some device components or the entire sensor, such as sealing joints, anti-reflection coatings, sensitive elements like CMOS, as well as undesired diffusion or migration of atoms from adjacent layers of different materials, or temperature-induced thermal stresses due to different thermal expansion coefficients between different materials.
[0010] In the prior art, one of the possible solutions to these problems is represented by separating the getter and the device into two compartments formed in the package, or by using local heating methods such as laser heating or electric Joule heating, resulting in increased cost and complexity of the obtained system.
[0011] Another possible solution is represented by the development of a low-temperature vacuum micro-packaging wafer-level or chip-to-wafer approach for VOx (mixed vanadium oxide) based microbolometer detectors, as described in "Low-temperature vacuum hermetic wafer-level package for uncooled microbolometer FPAs" (Proceedings of the SPIE, Vol. 6884, Paper 68840P), in which the microbolometer chip is exposed to a temperature not exceeding 140°C.
[0012] Furthermore, US8395229 relates to a MEMS microdevice integrated in a sealed housing, describing an active thin film getter for controlling the internal gas composition and pressure, wherein the MEMS-based microdevice allows local heating of the thin film getter material deposited on its surface. However, even with said specific configuration, it is known in the prior art that, due to the relative distances between the microdevice structure and its individual elements, it is not possible to avoid heating by radiation and the resulting damage to its surroundings if the getter is not shielded.
[0013] Another approach is then represented by the choice of the getter composition itself, as disclosed, for example, in EP0869195 in the name of the applicant, in which a non-evaporable getter alloy comprising zirconium, cobalt and one or more components selected from yttrium, lanthanum or rare earths is used to absorb various gases while maintaining a relatively low activation temperature. However, the main disadvantage of said composition is represented by the presence of cobalt as one of the main components, due to the known toxicity of cobalt to the human body.
[0014] It is therefore an object of the present invention to overcome the above-mentioned problems of the prior art and in particular to simplify the manufacture of MEMS devices.
[0015] The object of the present invention is therefore to provide a substrate comprising a base and an integrated getter film for the manufacture of microelectronic, micro-optoelectronic or micromechanical devices, wherein the getter film allows gas control and reduction (mainly carbonized species such as carbon oxides and carbon dioxide which are the main species inside the sealed device) while maintaining both low activation temperatures (particularly in the range of 250° C. to 300° C.) and reduced activation times (i.e. not more than 20 minutes) as required in the field of MEMS technology. It is important to point out that the temperature range also corresponds to the typical sealing temperatures of the packages.
[0016] Thus, device damage can be both avoided and the power budget of the sealing process reduced, resulting in a faster process and thus increased manufacturing throughput.Another important improvement associated with the lower activation temperature of the getter material is that outgassing species from the inner surface of the sealed device is also reduced.
[0017] In particular, the unexpected effect can be achieved when the getter film composition comprises Zr in an amount of 65 to 80 atomic %, V in an amount of 15 to 25 atomic %, a third element selected from Al and Fe in an amount of 2 to 15 atomic %, and the getter film structure is characterized by a surface roughness of 2 to 20 nm. As determined by the embodiments and comparative examples reported below, the morphological aspects of the getter film are particularly related to the surface interaction with the gas and its relative absorption value. The average roughness value has been measured by optical profilometer or atomic force microscopy (atomic force microscopy, AFM), and also taking into account the sputtering technology used, the average roughness value range can be 2 nm to 20 nm, preferably up to 8 nm. For thick films characterized by a thickness of 10 μm, high roughness values can be obtained.
[0018] In a preferred embodiment, the third element is Al in an amount of 2 to 15 atomic %; and in another embodiment, the third element is Fe in an amount of preferably 2 to 10 atomic %.
[0019] Furthermore, small amounts of impurities of other chemical elements may be present in the getter composition if their total percentage (meaning the sum of the atomic percentage contents of all these chemical elements) is less than 1 atomic % relative to the total getter composition.
[0020] According to the present invention, the thickness of the getter film is 500 nm to 10 μm, preferably 1 μm to 5 μm, and the thickness of the substrate is 20 μm to 5 mm.
[0021] In another embodiment, the substrate is made of silicon, germanium, soda-lime glass or borosilicate glass, quartz, metal or metal alloy (like Kovar or Nicrofer), and all these materials can be bare or completely or partially covered with other metal layers (like gold, aluminum), anti-reflective coatings, oxides.
[0022] According to the present invention, the getter film can be deposited by a sputtering deposition technique, which is the most suitable method for depositing (getter) films for large-scale production at an industrial level. This technique is a physical vapor deposition (PVD) that allows the deposition of thin films by bombarding a target material with ions and depositing it on a substrate.
[0023] Ion bombardment is achieved by generating a plasma near the target surface, where ions are accelerated towards the target by an electric field, and their impact on the target surface causes atoms to be ejected from the surface, traveling in the opposite direction, where a substrate is usually placed to collect the sputtered atoms from the target. The target material is the source of the atoms to be deposited, and it can be made of a single element or an alloy. The target is coupled to a backing plate, which has the function of providing power to the target and also has the function of dissipating the heat generated by the plasma due to the ion bombardment process. Therefore, the target material must withstand the stresses associated with thermal heating and cycling, as well as the stresses caused by the different thermal expansion between the target material and the backing plate, which is usually made of copper.
[0024] In a second aspect of the invention, the invention comprises a micromechanical device comprising a substrate, in which a getter film is integrated by PVD deposition techniques such as sputtering.Other different deposition techniques typical in the electronics and semiconductor industry may also be used, such as evaporation.
[0025] The substrate geometry can be flat, as in the case of silicon, germanium, or glass and quartz wafers or ceramics, or it can be made of a plurality of grooves or cavities produced from a flat support using a standard etching process or a deep reactive ion etching process. The cavity depth can typically range from about 10 μm to about 350 μm. When the substrate is made of grooves or cavities, the getter film layer can be deposited at the bottom of the cavity, or as an alternative, it can be deposited inside the entire cavity surface, i.e. the bottom and vertical surfaces, up to the top. The latter case maximizes the getter dose inside the cavity and, therefore, maximizes the absorption properties of the material.
[0026] In the case of a metal or ceramic substrate, the surface of the substrate may be flat, or it may be a 3D object, the shape of which may typically be a parallelepiped or rounded cup form. The getter film is deposited inside all available surfaces of the 3D object. The getter film may be deposited on the substrate, directly in contact with the substrate, or partially or completely deposited on different layers or materials present on the substrate. The getter film may be geometrically patterned on the substrate in a specific position and shape by photolithography or metal masking to intentionally overlap or non-overlap specific areas or materials present on the surface of the substrate.
[0027] In another configuration, the getter material can be deposited on a thin metal sheet, and then small sections of the sheet with the getter can be cut and inserted into the device without depositing the getter directly on the substrate.
[0028] The sheet material can be steel, stainless steel, Kovar or Nicrofer. The sheet thickness is typically in the range of 50 μm to 500 μm. To simplify the cutting of the sheet in smaller pieces, the sheet can be patterned in smaller pieces of different geometries using a chemical etching process. The smaller shaped pieces are typically fixed to the sheet frame at two points, and a single piece can be easily removed by cutting the two anchoring points. The getter material can be deposited on the patterned sheet, and it can be deposited on one or both sides of the block. In this configuration, the getter film can also be directly activated with electric current or laser heating after the sealing process of the device.
[0029] Hereinafter, the present invention will be described in more detail with reference to the following examples.
[0030] Samples S1 to S3 and Comparative Samples C1 to C6
[0031] The getter film is prepared by sputtering deposition inside a vacuum chamber, wherein a sputtering target made of ZrVAl material is mounted on a copper backing plate. The diameter of the sputtering target is 5 cm, and the substrate on which the getter film is deposited is a silicon disk of 2.5 cm diameter. The process gas for samples S1 to S3 and comparative samples C1 and C3 to C6 is argon, while the process gas for C2 is krypton. The gas flow rate is 30 sccm or 40 sccm, while the gas pressure is 30 mTorr. The sputtering power is 120 W to 150 W, the distance between the target surface and the substrate is in the range of 50 mm, and the resulting getter film thickness is about 2.0 μm.
[0032] The functional properties of the material are characterized by the amount of gas that the getter can absorb at room temperature after being activated at a specific temperature for a specific time. The test is carried out according to standard ASTM F798-82. The test gas is carbon monoxide CO and the getter is activated in a vacuum at 250°C for 15 minutes before exposing the material to CO gas.
[0033] The resulting absorbed gas amounts reported in Table 1 were normalized to the getter surface.
[0034]
[0035] Table 1
[0036] The reported results indicate that samples S1 to S3 prepared according to the present invention exhibited significant CO absorption and the corresponding reduction of said gas species thereby, while maintaining reduced activation time and temperature.
[0037] On the contrary, comparative samples C1, C2 and C5 activated in the same way and having comparable roughness, but featuring different getter film compositions, show lower gas absorption values and the resulting reduction in efficiency. At the same time, comparative examples C4 and C6 disclose the key role of the specific range of surface roughness of the present invention, since substrates characterized by roughness values below 2 nm show a significant reduction in gas absorption. Moreover, comparative sample C3, reporting a typical getter composition according to the prior art containing cobalt, achieves lower gas absorption despite having the same roughness as S3, in addition to the toxicity problems associated with the use of said metal.
Claims
1. A substrate for manufacturing a microelectronic device comprising a base and an integrated getter film, wherein the getter film consists of: - Zr in an amount of 65 atomic % to 80 atomic %, -15 atomic % to 25 atomic % of V, and - a third element selected from Al and Fe in an amount of 2 to 15 atomic % relative to the total getter composition, and impurities of other chemical elements that may be present in the getter composition in a total percentage of less than 1 atomic %, Characterized in that the surface roughness of the getter film is 2nm to 20nm, preferably 2nm to 8nm. 2 . The substrate according to claim 1 , wherein the third element is Fe, and an amount of Fe is 2 atomic % to 10 atomic %.
3. The substrate according to any of the preceding claims, wherein the getter film has a thickness of 500 nm to 10 μm, preferably 1 μm to 5 μm.
4. The substrate according to any one of the preceding claims, wherein the base has a thickness of 20 μm to 5 mm.
5. The substrate according to any one of the preceding claims, wherein the base is made of a material selected from the group consisting of silicon, germanium, ceramic, soda-lime glass or borosilicate glass, quartz, metallic elements, Kovar, steel, stainless steel or Nicrofer.
6. The substrate according to any of the preceding claims, wherein the surface of the base is a flat surface or a 3D object in the form of a parallelepiped or a rounded cup, preferably with a cavity depth of about 10 μm to about 350 μm.
7. The substrate according to any one of the preceding claims, wherein the getter film is deposited using a sputtering technique.
8. The substrate according to any of the preceding claims, wherein the material of the base is completely or partially covered with one or more metal layers selected from gold, aluminum, anti-reflective coatings, oxides.
9. The substrate according to any one of the preceding claims, wherein the getter film is geometrically patterned in specific positions and shapes on the substrate.
10. A micromechanical device comprising the substrate according to any one of claims 1 to 9.
11. Use of a substrate according to any one of claims 1 to 9 as a component in a micromechanical device.