Rubber composition
The existing rubber compositions have been solved in terms of fracture properties and recyclability by using a combination of polymers with hydroxyl and diene units in the rubber composition and a sulfur crosslinking agent to form a strong hydrogen bond and sulfur crosslinking structure. Inadequate, higher tensile strength and elongation are achieved and recyclability is improved.
Patent Information
- Application Number
- CN202380027423.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-01-11
- Publication Date
- 2024-11-05
AI Technical Summary
The existing rubber compositions are difficult to maintain tensile strength and elongation during breaking by hydrogen bond crosslinking, and have poor recovery.
Using a rubber composition containing a polymer having at least two hydroxyl groups and diene units and a sulfur crosslinking agent, a strong crosslinking structure is formed by hydrogen bonding and a sulfur crosslinking agent, and the content of the crosslinking agent is controlled to increase the breaking time. Tensile strength and elongation, and optimize the structure of the polymer to improve recyclability.
The tensile strength and elongation at break of the rubber composition are significantly improved while improving its recyclability, which performs better than rubber compositions crosslinked only by sulfur.
Smart Images

Figure BDA0005041753960000021 
Figure BDA0005041753960000022 
Figure BDA0005041753960000051
Abstract
Description
Technical Field
[0001] The present invention relates to rubber compositions. Background Art
[0002] Conventionally, rubber products such as tires are produced by crosslinking (vulcanizing) a rubber component (polymer) with sulfur to ensure sufficient physical properties such as tensile strength at break (TB) and elongation at break (EB) as indicators of durability.
[0003] Meanwhile, from the viewpoint of environmental issues and resource conservation, the technology of recycling used vulcanized rubber products has been studied. For example, Patent Document 1 mentioned below discloses an elastomer comprising an vicinal diol unit having a specific structure and a but-1-ene-1,4-diyl unit having a specific structure, and teaches that the elastomer has excellent toughness and recyclability.
[0004] Citation List
[0005] Patent Document 1: JP 2020-100718 A Summary of the invention
[0006] Problem that the invention aims to solve
[0007] However, the present inventors have found through studies that the elastomer described in Patent Document 1 is cross-linked by hydrogen bonds of diols, and the hydrogen bonds are easily dissociated, and physical properties such as tensile strength at break (TB) cannot be sufficiently maintained.
[0008] Therefore, an object of the present invention is to solve the above-mentioned problems of the prior art and to provide a rubber composition having improved tensile strength at break (TB) and elongation at break (EB).
[0009] Solutions for solving problems
[0010] The rubber composition of the present invention for solving the above-mentioned problems is mainly constituted as follows.
[0011] [1] A rubber composition comprising a rubber component (A) and a crosslinking agent (B),
[0012] wherein the rubber component (A) comprises a polymer (A1) having at least two hydroxyl groups and a diene unit, at least two hydroxyl groups in the polymer (A1) are bonded to adjacent carbon atoms, and
[0013] The content of the crosslinking agent (B) is 0.1 to 8 parts by mass based on 100 parts by mass of the rubber component (A), and is 0.1 to 80 parts by mass based on 100 parts by mass of the polymer (A1).
[0014] [2] The rubber composition according to [1], wherein the weight average molecular weight (Mw) of the polymer (A1) is 1,000 to 1,000,000.
[0015] [3] The rubber composition according to [1] or [2], wherein the polymer (A1) contains a monomer unit derived from a cycloocta-1,5-diene compound represented by the following general formula (1):
[0016] [Chemical formula 1]
[0017]
[0018] Where R 1 are independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms.
[0019] [4] The rubber composition according to any one of [1] to [3], wherein the polymer (A1) comprises a monomer unit derived from a 5-cyclooctene-1,2-diol compound represented by the following general formula (2):
[0020] [Chemical formula 2]
[0021]
[0022] Where R 2 are independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms.
[0023] [5] The rubber composition according to [4], wherein the content of the monomer unit derived from the 5-cyclooctene-1,2-diol compound represented by the above general formula (2) in the polymer (A1) is 5 to 50 mol%.
[0024] [6] The rubber composition according to any one of [1] to [5], wherein the crosslinking agent (B) contains at least sulfur.
[0025] Effects of the Invention
[0026] According to the present invention, a rubber composition having improved tensile strength at break (TB) and elongation at break (EB) can be provided. DETAILED DESCRIPTION
[0027] The rubber composition according to the present invention will be described in detail below by way of embodiments.
[0028] <Rubber Composition>
[0029] The rubber composition of the present invention comprises a rubber component (A) and a crosslinking agent (B). In the rubber composition of the present invention, the rubber component (A) comprises a polymer (A1) having at least two hydroxyl groups and a diene unit, wherein at least two hydroxyl groups in the polymer (A1) are bonded to adjacent carbon atoms, and the content of the crosslinking agent (B) is 0.1 to 8 parts by mass relative to 100 parts by mass of the rubber component (A), and is 0.1 to 80 parts by mass relative to 100 parts by mass of the polymer (A1).
[0030] In the rubber composition of the present invention, the polymer (A1) having a hydroxyl group forms a hydrogen bond via the hydroxyl group. Here, at least two hydroxyl groups in the polymer (A1) are bonded to adjacent carbon atoms, in other words, at least two hydroxyl groups are present in adjacent positions. Therefore, the hydroxyl group of one polymer (A1) and the hydroxyl group of another polymer (A1) can be strongly hydrogen-bonded by forming multiple hydrogen bonds in adjacent positions.
[0031] In addition, since the rubber composition of the present invention includes a crosslinking agent (B), the crosslinked rubber composition will have crosslinking due to hydrogen bonding and a crosslinking structure due to the crosslinking agent (B). Here, when the content of the crosslinking agent (B) is 0.1 parts by mass or more relative to 100 parts by mass of the rubber component (A) and 0.1 parts by mass or more relative to 100 parts by mass of the polymer (A1), the crosslinking structure due to the crosslinking agent (B) is fully formed. In addition, when the content of the crosslinking agent (B) is 8 parts by mass or less relative to 100 parts by mass of the rubber component (A) and 80 parts by mass or less relative to 100 parts by mass of the polymer (A1), moderate elongation is achieved.
[0032] In the rubber composition of the present invention, the rubber component (A) containing the polymer (A1) can be crosslinked with high strength due to the synergistic effect of the crosslinking caused by the hydrogen bond of the polymer (A1) having a hydroxyl group and the crosslinking structure caused by the crosslinking agent (B). As a result, the tensile strength at break (TB) can be significantly improved compared with the elastomer crosslinked only by hydrogen bonds as described in Patent Document 1, and both the tensile strength at break (TB) and the elongation at break (EB) can be significantly improved compared with the conventional rubber composition crosslinked only by sulfur.
[0033] In addition, in the rubber composition of the present invention, hydrogen bonds may be easily dissociated. In addition, since the content of the crosslinking agent (B) is 8 parts by mass or less relative to 100 parts by mass of the rubber component (A) and 80 parts by mass or less relative to 100 parts by mass of the polymer (A1), there is no excessive crosslinking structure caused by the crosslinking agent (B). Therefore, the rubber composition of the present invention is easier to recycle than a rubber composition crosslinked only by sulfur crosslinking.
[0034] --Rubber component (A)--
[0035] The rubber composition of the present invention comprises a rubber component (A), and the rubber component (A) provides rubber elasticity to the composition. The rubber component (A) comprises a polymer (A1) having at least two hydroxyl groups and a diene unit (hereinafter referred to as "polymer (A1)" or "polymer (A1) having hydroxyl groups"), and at least two hydroxyl groups in the polymer (A1) are bonded to adjacent carbon atoms.
[0036] At least two hydroxyl groups in polymer (A1) are bonded to adjacent carbon atoms. The structure in which at least two hydroxyl groups are bonded to adjacent carbon atoms allows the hydroxyl groups of one polymer (A) to form multiple hydrogen bonds with the hydroxyl groups of another polymer (A) at adjacent positions, which increases the strength of the crosslinked structure due to hydrogen bonds via the hydroxyl groups.
[0037] Note that the polymer (A1) having a hydroxyl group includes a site to which a plurality of carbon atoms are directly bonded, and the oxygen atoms in at least two hydroxyl groups are bonded to a carbon atom (a carbon atom at a site to which a plurality of carbon atoms are directly bonded). In addition, it can be said that the number of carbon atoms between the oxygen atom in one hydroxyl group and the oxygen atom in another hydroxyl group is two, or it can be said that an ortho-hydroxyl group is included.
[0038] In the polymer (A1), the hydroxyl group is bonded in an amount of preferably 10 to 100 mol%, more preferably 20 to 60 mol%, relative to the monomer units in the polymer (A1). When the hydroxyl group is bonded in an amount of 10 mol% or more relative to the monomer units in the polymer (A1), the strength of the cross-linked structure by hydrogen bonding via the hydroxyl group is improved, and the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition are further improved. In addition, when the hydroxyl group is bonded in an amount of 100 mol% or less relative to the monomer units in the polymer (A1), a polymer having sufficient elastomeric properties becomes more likely to be obtained.
[0039] It is preferred that two hydroxyl groups exist in one monomer unit, and in one embodiment, "hydroxyl groups are bonded in an amount of 10 to 100 mol% relative to the monomer units in polymer (A1)" means that two hydroxyl groups exist in 5 to 50 mol% of the monomer units in all monomer units.
[0040] The diene unit in the polymer (A1) having a hydroxyl group may be a conjugated diene unit (conjugated diene unit) or a non-conjugated diene unit (non-conjugated diene unit).
[0041] The conjugated diene unit is a monomer unit derived from a conjugated diene compound. The conjugated diene compound as a monomer preferably has 4 to 8 carbon atoms. Examples of such conjugated diene compounds include 1,3-butadiene, isoprene, 1,3-pentadiene and 2,3-dimethyl-1,3-butadiene. From the viewpoint of good elastomer properties, the conjugated diene compound as a monomer preferably contains 1,3-butadiene and / or isoprene.
[0042] The non-conjugated diene unit is a monomer unit derived from a non-conjugated diene compound. Examples of the non-conjugated diene compound as a monomer include a cycloocta-1,5-diene compound represented by the following general formula (1):
[0043] [Chemical formula 3]
[0044]
[0045] Where R 1 is independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms. Here, examples of the halogen atom include a fluorine atom, a chlorine atom and a bromine atom. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group and a neopentyl group.
[0046] As the cycloocta-1,5-diene compound of the general formula (1), a commercially available compound may be used, or a compound synthesized according to a known method may be used. 1 The compounds in which R is a hydrogen atom, a halogen atom, a methyl group or an ethyl group are preferred. 1 A compound in which R is a hydrogen atom or a methyl group is more preferred, and R 1 Compounds containing hydrogen atoms are particularly preferred. Specifically, examples of the cyclooct-1,5-diene compound of formula (1) include cyclooct-1,5-diene, 1-chlorocyclooct-1,5-diene, 1,5-dichlorocyclooct-1,5-diene, 1-methylcyclooct-1,5-diene, and 1,5-dimethylcyclooct-1,5-diene.
[0047] It is preferred that the polymer (A1) having a hydroxyl group contains a monomer unit derived from the cycloocta-1,5-diene compound represented by the above general formula (1). In this case, excellent rubber elasticity can be imparted to the rubber composition.
[0048] The proportion of the diene unit in the polymer (A1) is not particularly limited, and 50 mol% or more is preferred, 70 mol% or more is more preferred, and 95 mol% or less is preferred, 90 mol% or less is more preferred.
[0049] Polymer (A1) can include units derived from other monomers copolymerizable with diene compounds (which can be conjugated diene compounds or non-conjugated diene compounds). Examples of such units derived from other monomers include olefin units and aromatic vinyl units. The ratio of units derived from other monomers in polymer (A1) is not particularly limited and can be 0mol%. However, in one embodiment, 1mol% or more is preferred and 50mol% or less is preferred.
[0050] The olefin unit refers to a monomer unit derived from an olefin compound. The olefin compound as a monomer preferably has 2 to 10 carbon atoms. Specific examples of such olefin compounds include α-olefins such as ethylene, propylene, 1-pentene, 1-hexene, 1-heptene and 1-octene, and heteroatom-substituted olefin compounds such as vinyl pivalate, 1-phenylthioethylene and N-vinyl pyrrolidone.
[0051] The olefin compound may also have two or more hydroxyl groups. An example of the olefin compound having two or more hydroxyl groups is a 5-cyclooctene-1,2-diol compound represented by the following general formula (2):
[0052] [Chemical formula 4]
[0053]
[0054] Where R 2 is independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms. Here, examples of the halogen atom include a fluorine atom, a chlorine atom and a bromine atom. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group and a neopentyl group.
[0055] As the 5-cyclooctene-1,2-diol compound of the general formula (2), a commercially available compound may be used, or a compound synthesized according to a known method may be used. 2 The compounds in which R is a hydrogen atom, a halogen atom, a methyl group or an ethyl group are preferred. 2 A compound in which R is a hydrogen atom or a methyl group is more preferred, and R 2 Compounds which are hydrogen atoms are particularly preferred. Specifically, examples of the 5-cyclooctene-1,2-diol compound of the general formula (2) include 5-cyclooctene-1,2-diol and the like.
[0056] Preferably, the polymer (A1) having a hydroxyl group includes monomer units derived from the 5-cyclooctene-1,2-diol compound represented by the general formula (2) above. In the polymer comprising monomer units derived from the 5-cyclooctene-1,2-diol compound represented by the general formula (2), at least two hydroxyl groups are present in adjacent positions. Therefore, the hydroxyl group of a polymer and the hydroxyl group of another polymer form multiple hydrogen bonds in adjacent positions and can be strongly hydrogen-bonded. By compounding such polymers into a rubber composition, the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition can be further improved.
[0057] The proportion of the olefin unit in the polymer (A1) is not particularly limited and may be 0 mol%, but in one embodiment, 5 mol% or more is preferred, 10 mol% or more is more preferred, and 50 mol% or less is preferred, 30 mol% or less is more preferred.
[0058] The aromatic vinyl unit is a monomer unit derived from an aromatic vinyl compound. An aromatic vinyl compound refers to an aromatic compound substituted with at least a vinyl group. The aromatic vinyl compound as a monomer preferably has 8 to 10 carbon atoms. Specifically, examples of such aromatic vinyl compounds include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2-ethylstyrene, 3-ethylstyrene and 4-ethylstyrene.
[0059] The ratio of the aromatic vinyl unit in the polymer (A1) is not particularly limited and may be 0 mol %. However, in one embodiment, 1 mol % or more is preferred, and 50 mol % or less is preferred.
[0060] --First method for producing a polymer (A1) having a hydroxyl group--
[0061] The polymer (A1) having a hydroxyl group can be formed, for example, by ring-opening metathesis polymerization of a cyclooctane-1,5-diene compound represented by the above general formula (1) and a 5-cyclooctene-1,2-diol compound represented by the above general formula (2). As an example, when cyclooctane-1,5-diene is used as the compound represented by the general formula (1) and 5-cyclooctene-1,2-diol is used as the compound represented by the general formula (2), the reaction scheme of the ring-opening metathesis polymerization is shown below.
[0062] [Chemical formula 5]
[0063]
[0064] The molar ratio of the cyclooctane-1,5-diene compound represented by the general formula (1) to the 5-cyclooctene-1,2-diol compound represented by the general formula (2) [compound of the general formula (1) : compound of the general formula (2)] is preferably in the range of 95:5 to 50:50, and more preferably in the range of 90:10 to 70:30, and can be appropriately selected according to the purpose.
[0065] Here, in the polymer (A1) having a hydroxyl group, the content of the monomer unit derived from the 5-cyclooctene-1,2-diol compound represented by the general formula (2) is preferably 5 to 50 mol%. When the content of the monomer unit derived from the compound represented by the general formula (2) is 5 mol% or more, the amount of hydroxyl groups in the polymer (A1) increases, more hydrogen bonds are formed, crosslinking by hydrogen bonds can be formed more strongly, and the tensile strength at break (TB) and elongation at break (EB) of the rubber composition are further improved. When the content of the monomer unit derived from the compound represented by the general formula (2) is 50 mol% or less, the elongation characteristics of the polymer (A1) are improved and the elongation at break (EB) of the rubber composition is further improved. From the viewpoint of the tensile strength at break (TB) and elongation at break (EB) of the rubber composition, it is further preferred that the content of the monomer unit derived from the compound represented by the general formula (2) in the polymer (A1) having a hydroxyl group is 10 mol% or more. From the viewpoint of the elongation characteristics of the polymer (A1) and the elongation at break (EB) of the rubber composition, it is further preferred that the content is 30 mol% or less.
[0066] In the above-mentioned ring-opening metathesis polymerization, known catalysts can be used, for example, transition metal complexes such as titanium complexes, zirconium complexes, molybdenum complexes, ruthenium complexes, tantalum complexes, tungsten complexes and rhenium complexes can be used. Among them, transition metal-carbene complexes such as Grubbs first generation catalyst, Grubbs second generation catalyst and Hoveyda-Grubbs catalyst are preferred. Grubbs second generation catalyst is represented by the following structural formula:
[0067] [Chemical formula 6]
[0068]
[0069] And commercially available products may be used. The amount of the catalyst used is, for example, preferably 0.001 to 10 mol%, more preferably 0.01 to 1 mol%, and particularly preferably 0.01 to 0.1 mol% relative to 1 mol of the monomer of the raw material.
[0070] In the above ring-opening metathesis polymerization, the reaction temperature is preferably -50°C to 180°C, -20°C to 100°C is more preferred, and -10°C to 80°C is even more preferred. The reaction time is preferably 1 to 24 hours, and the reaction pressure may be pressurized, reduced pressure or atmospheric pressure, but atmospheric pressure is preferred. The reaction atmosphere is preferably an inert gas atmosphere such as nitrogen or argon.
[0071] The above-mentioned ring-opening metathesis polymerization can be carried out in a solvent. For example, as a solvent, an inert solvent for reaction is preferred, for example, an aliphatic halogenated solvent such as dichloromethane, chloroform and 1,2-dichloroethane; an ether solvent such as diethyl ether, tetrahydrofuran and dioxane; an aromatic hydrocarbon solvent such as benzene, toluene, xylene and mesitylene; an aromatic halogenated solvent such as monochlorobenzene and dichlorobenzene; and an aliphatic hydrocarbon solvent such as hexane, heptane, octane and cyclohexane.
[0072] --Second method for producing a polymer (A1) having a hydroxyl group--
[0073] The polymer (A1) having a hydroxyl group can also be formed by reacting a polymer chain with a compound having a hydroxyl group. Here, the polymer chain can be synthesized by polymerization or copolymerization of a diene compound or copolymerization of a diene compound and other monomers copolymerizable with the diene compound.
[0074] In addition, the compound having a hydroxyl group preferably has a functional group containing a sulfur atom or an unsaturated bond, etc. The compound having a hydroxyl group and a functional group containing a sulfur atom can be easily added to a polymer chain. In addition, the compound having a hydroxyl group and an unsaturated bond can also be easily added to a polymer chain.
[0075] Examples of the functional group containing a sulfur atom include a thiol group (also referred to as a "mercapto group"), a sulfide group (also referred to as a "thioether group"), and a thiol group is preferred. When a compound having a hydroxyl group has a thiol group as a functional group containing a sulfur atom, it is more easily added to a polymer chain.
[0076] Examples of the above unsaturated bond include a carbon-carbon double bond (C=C), a carbon-oxygen double bond (C=O), and a carbon-carbon triple bond (C≡C). Note that the carbon-carbon double bond may be part of an aromatic ring.
[0077] The compound having a hydroxyl group preferably has two or more hydroxyl groups. In the compound having two or more hydroxyl groups, at least two hydroxyl groups in the compound are preferably bonded to adjacent carbon atoms. In other words, the compound having two or more hydroxyl groups is preferably a vicinal diol having a functional group containing a sulfur atom or a vicinal diol having an unsaturated bond.
[0078] Examples of compounds having two or more hydroxyl groups include sulfur-containing compounds such as 1-mercapto-1,2-ethanediol, 3-mercapto-1,2-propylene glycol (also referred to as "thioglycerol" or "α-thioglycerol"), 2-mercapto-1,2-propylene glycol, 1-mercapto-1,2-propylene glycol, 3-mercapto-2-methyl-1,2-propylene glycol, 3-mercapto-2-ethyl-1,2-propylene glycol, 1-mercapto-2-methyl-1,2-propylene glycol, and 1-mercapto-2-ethyl-1,2-propylene glycol, and unsaturated compounds (aromatic compounds) such as catechol, methylcatechol, ethylcatechol, pyrogallol, and gallic acid. Among them, thioglycerol is preferred.
[0079] --Other methods for producing polymers (A1) having hydroxyl groups--
[0080] The method for producing the polymer (A1) having a hydroxyl group is not limited to the first production method or the second production method described above, and can be formed by other production methods. For example, a polymer in which two hydroxyl groups are bonded to adjacent carbon atoms can be produced by synthesizing a polymer chain having an epoxy group and ring-opening (hydrolyzing) the epoxy group.
[0081] The weight average molecular weight (Mw) of the polymer (A1) having a hydroxyl group is preferably 300 to 1,000,000, and more preferably 1,000 to 1,000,000. When the weight average molecular weight (Mw) is 1,000 or more, the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition are improved, and when the weight average molecular weight (Mw) is 1,000,000 or less, the processability of the rubber composition is improved.
[0082] In the present specification, the weight average molecular weight (Mw) of the polymer (A1) is measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0083] The rubber composition of the present invention comprises the above-mentioned polymer (A1) with hydroxyl as rubber component (A), and may further comprise the rubber component other than the polymer (A1) with hydroxyl. The example of such other rubber components includes natural rubber (NR), synthetic diene rubber and non-diene rubber. The example of synthetic diene rubber includes synthetic isoprene rubber (IR), styrene-butadiene rubber (SBR), butadiene rubber (BR), styrene-isoprene rubber (SIR), chloroprene rubber (CR), ethylene-butadiene copolymer and ethylene-styrene-butadiene copolymer. The example of non-diene rubber includes silicone rubber, fluororubber and polyurethane rubber.
[0084] In the rubber component (A) of the rubber composition, the proportion of the polymer (A1) having a hydroxyl group is preferably 10% by mass or more, more preferably 50% by mass or more, and may be 100% by mass.
[0085] --Crosslinking agent (B)--
[0086] The rubber composition of the present invention contains a crosslinking agent (B). When the rubber composition contains the crosslinking agent (B) and the polymer (A1) having a hydroxyl group, crosslinking due to hydrogen bonding and a crosslinking structure due to the crosslinking agent (B) exist in the crosslinked rubber composition.
[0087] The content of the crosslinking agent (B) is 0.1 to 8 parts by mass based on 100 parts by mass of the rubber component (A), and is 0.1 to 80 parts by mass based on 100 parts by mass of the polymer (A1) having a hydroxyl group.
[0088] When the content of the crosslinking agent (B) is 0.1 parts by mass or more relative to 100 parts by mass of the rubber component (A), the crosslinking structure due to the crosslinking agent (B) is fully formed and the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition are improved. When the content of the crosslinking agent (B) is 8 parts by mass or less relative to 100 parts by mass of the rubber component (A), moderate elongation can be achieved and the elongation at break (EB) of the rubber composition is improved. The content of the crosslinking agent (B) is preferably 0.5 parts by mass or more relative to 100 parts by mass of the rubber component (A) from the viewpoint of the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition, and is preferably 5 parts by mass or less relative to 100 parts by mass of the rubber component (A) from the viewpoint of the elongation characteristics and the elongation at break (EB) of the rubber composition.
[0089] In addition, when the content of the crosslinking agent (B) is 0.1 parts by mass or more relative to 100 parts by mass of the polymer (A1) having a hydroxyl group, the crosslinked structure due to the crosslinking agent (B) is fully formed and the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition are improved. When the content of the crosslinking agent (B) is 80 parts by mass or less relative to 100 parts by mass of the polymer (A1) having a hydroxyl group, moderate elongation can be achieved and the elongation at break (EB) of the rubber composition is improved. The content of the crosslinking agent (B) is preferably 0.5 parts by mass or more relative to 100 parts by mass of the polymer (A1) having a hydroxyl group from the viewpoint of the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition, and is preferably 50 parts by mass or less relative to 100 parts by mass of the polymer (A1) having a hydroxyl group from the viewpoint of the elongation characteristics and the elongation at break (EB) of the rubber composition.
[0090] Examples of the crosslinking agent (B) include sulfur, peroxides, etc. Examples of peroxides include organic peroxides, and specific examples thereof include tert-butyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, dicumyl peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, diisopropylbenzene hydroperoxide, tert-butylcumyl peroxide, di(2-tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, peroxybenzoic acid, benzoyl peroxide, 1,1-bis(1,1-dimethylethylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)-3,3 ,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 2,2-bis(4,4-di-(tert-butylperoxy)cyclohexyl)propane, 4,4-di-(tert-butylperoxy)valerate n-butyl, tert-butylperoxylaurate, tert-butylperoxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, tert-hexylperoxy-2-ethylhexanoate, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyacetate, cyclohexanone peroxide, acetylacetone peroxide, diisopropylperoxydicarbonate, and di(4-tert-butylcyclohexyl)peroxydicarbonate. Here, when sulfur is used as the crosslinking agent (B), sulfur crosslinks are formed, and when peroxide is used as the crosslinking agent (B), a crosslinking structure (CC bond, etc.) caused by the peroxide is formed.
[0091] The crosslinking agent (B) preferably contains at least sulfur. It is further preferred that sulfur is contained in an amount of 50% by mass or more of the crosslinking agent (B), and all of the crosslinking agent (B) may be sulfur. When the crosslinking agent (B) contains at least sulfur, sulfur crosslinking is formed as a crosslinking structure due to the crosslinking agent (B), and the tensile strength at break (TB) and elongation at break (EB) of the rubber composition are further improved.
[0092] --Metal ions of elements in Groups 3 to 12 of the periodic table--
[0093] The rubber composition may further contain metal ions of elements in Groups 3 to 12 of the periodic table. When such metal ions are contained, the hydroxyl groups in the polymer (A1) are complexed with the metal ions of elements in Groups 3 to 12 of the periodic table. Therefore, the polymer (A1) can be crosslinked with a higher strength than hydrogen bonding, thereby further improving the tensile strength at break (TB) and elongation at break (EB) of the rubber composition.
[0094] Examples of elements in Group 3 of the periodic table include scandium and yttrium.
[0095] Furthermore, examples of the elements in Group 4 of the periodic table include titanium and zirconium.
[0096] Furthermore, examples of the elements in Group 5 of the periodic table include vanadium and niobium.
[0097] Furthermore, examples of the elements in Group 6 of the periodic table include chromium, molybdenum, and tungsten.
[0098] Specifically, examples of the element in Group 7 of the periodic table include manganese and rhenium.
[0099] Furthermore, examples of the elements in Group 8 of the periodic table include iron, ruthenium, and osmium.
[0100] Furthermore, examples of the elements in Group 9 of the periodic table include cobalt, rhodium, and iridium.
[0101] Furthermore, examples of the elements in Group 10 of the periodic table include nickel, palladium, and platinum.
[0102] Furthermore, examples of the elements in Group 11 of the periodic table include copper and silver.
[0103] Furthermore, examples of the elements in Group 12 of the periodic table include zinc.
[0104] Metal ions of elements of Groups 3 to 12 of the periodic table tend to be strongly bonded to hydroxyl groups.
[0105] Note that the ion valence of the metal ion of the element of Groups 3 to 12 of the periodic table is not particularly limited and may be any valence that each element can take.
[0106] The metal ion is preferably a metal ion selected from elements in Groups 7 to 12 of the periodic table. When the metal ion is a metal ion of an element in Groups 7 to 12 of the periodic table, the bond with the hydroxyl group tends to be even stronger and a crosslink with higher strength can be formed.
[0107] The metal ions are preferably selected from metal ions of elements in the fourth and fifth periods of the periodic table. The metal ions of elements in the fourth and fifth periods of the periodic table have a high coordination force to the hydroxyl group, which increases the bond dissociation energy between the metal ions and the hydroxyl group and further increases the tensile strength at break (TB) and the elongation at break (EB) of the rubber composition.
[0108] It is particularly preferred that the metal ion is at least one selected from the group consisting of iron ions, copper ions, and zinc ions. Iron ions, copper ions, and zinc ions tend to bind particularly strongly to hydroxyl groups and can form even stronger cross-linked structures. Note that the valence of the iron ion is preferably divalent (Fe 2+ ) or trivalent (Fe 3+ ).
[0109] It is preferred to complex the metal ions with the hydroxyl groups of the polymer (A1) by adding a metal salt to the rubber composition. Note that the form of the metal salt to be added is not particularly limited, and may be, for example, a hydrate. The amount of the metal salt added is preferably in the range of 1 to 30 parts by mass, more preferably in the range of 1 to 15 parts by mass, even more preferably in the range of 1 to 10 parts by mass, and particularly preferably in the range of 1 to 5 parts by mass, relative to 100 parts by mass of the polymer (A1) having a hydroxyl group.
[0110] Examples of the above-mentioned metal salts include metal halides, metal sulfates and metal nitrates. Among them, metal halides are preferred. Metal halides are easier to handle and can more easily form crosslinks with higher strength.
[0111] In addition, examples of the above-mentioned metal halide include metal fluoride, metal chloride, metal bromide and metal iodide. Among them, metal chloride is preferred. Metal chloride is easy to handle and can more easily form a crosslink with high strength.
[0112] It is also preferred that the metal salt be a metal salt other than metal oxides, metal carbonates and fatty acid metal salts. Metal salts other than metal oxides, metal carbonates and fatty acid metal salts tend to form a coordinate bond with a hydroxyl group more easily (further tend to complex).
[0113] Specifically, examples of the metal salt include FeCl 2 , FeCl 2 ·4H 2 O, FeCl 3 , FeCl 3 ·6H 2 O, CuCl 2 , CuCl 2 ·2H 2 O, and ZnCl 2. One metal salt may be used alone, or two or more metal salts may be used in combination.
[0114] --other--
[0115] In addition to the above-mentioned rubber component (A), crosslinking agent (B) and metal ions (metal salts) of elements in Groups 3 to 12 of the periodic table, the rubber composition of the present invention may also contain compounding agents commonly used in the rubber industry, which may be appropriately selected and compounded within the scope of not impairing the purpose of the present invention. Examples of these compounding agents include, for example, fillers (such as carbon black and silica), softeners, waxes, stearic acid, antioxidants, silane coupling agents, zinc flowers (zinc oxide) and vulcanization accelerators, etc. Commercially available products are suitable for use as these compounding agents.
[0116] Examples of the wax include paraffin wax and microcrystalline wax. The content of the wax is not particularly limited, and is preferably in the range of 0.1 to 5 parts by mass, more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the rubber component (A).
[0117] The content of stearic acid is not particularly limited, and is preferably in the range of 0.1 to 5 parts by mass, more preferably in the range of 0.5 to 4 parts by mass, relative to 100 parts by mass of the rubber component (A).
[0118] Examples of antioxidants include N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6PPD), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (TMDQ), 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline (AW), and N,N'-diphenyl-p-phenylenediamine (DPPD). The amount of the antioxidant is not particularly limited, and is preferably in the range of 0.1 to 5 parts by mass, more preferably in the range of 1 to 4 parts by mass, relative to 100 parts by mass of the rubber component (A).
[0119] The content of zinc flower (zinc oxide) is not particularly limited, and is preferably in the range of 0.1 to 10 parts by mass, more preferably in the range of 1 to 5 parts by mass, relative to 100 parts by mass of the rubber component (A).
[0120] Examples of the vulcanization accelerator include sulfenamide vulcanization accelerators, guanidine vulcanization accelerators, thiazole vulcanization accelerators, thiuram vulcanization accelerators, and dithiocarbamate vulcanization accelerators. The amount of the vulcanization accelerator is not particularly limited, and is preferably in the range of 0.1 to 5 parts by mass, more preferably in the range of 0.2 to 3 parts by mass, relative to 100 parts by mass of the rubber component (A).
[0121] --Method for producing rubber composition--
[0122] The method for producing the rubber composition is not particularly limited, but the rubber composition can be produced, for example, by mixing the above-mentioned rubber component (A) and the crosslinking agent (B) with various components appropriately selected as needed, followed by kneading, heating, extrusion, etc. In addition, the obtained rubber composition can be crosslinked to produce a crosslinked rubber.
[0123] There is no particular restriction on the kneading conditions, and various conditions such as the input volume of the kneading device, the rotor rotation speed, the punching pressure, the kneading temperature, the kneading time and the type of the kneading device can be appropriately selected according to the purpose. Examples of the kneading device include a Banbury mixer, an internal mixer, a kneader and a roll, etc., which are generally used for kneading of rubber compositions.
[0124] The conditions for warming are not particularly limited either, and various conditions such as warming temperature, warming time, and warming equipment can be appropriately selected according to the purpose. Examples of the warming equipment include a warming roll machine or the like generally used for warming of a rubber composition.
[0125] There is no particular restriction on the conditions for extrusion, and various conditions such as extrusion time, extrusion speed, extrusion equipment and extrusion temperature can be appropriately selected according to the purpose. Examples of extrusion equipment include extruders commonly used for extrusion of rubber compositions, etc. The extrusion temperature can be appropriately determined.
[0126] There is no particular limitation on the equipment, method, conditions, etc. for crosslinking, which can be appropriately selected according to the purpose. Examples of equipment for crosslinking include a molding vulcanizer, etc., which are generally used for vulcanization of rubber compositions. The conditions for crosslinking are such that the temperature is, for example, about 100° C. to 190° C.
[0127] For example, in the first stage of kneading, the rubber component (A) [containing the polymer (A1) having a hydroxyl group] can be mixed and kneaded with various components appropriately selected as needed to produce a mixture containing the rubber component (A), and in the second stage and subsequent stages of kneading, the crosslinking agent (B) can be mixed and kneaded with various components appropriately selected as needed to produce a rubber composition. In addition, by crosslinking the rubber composition after forming it into a desired shape, a crosslinked rubber having a crosslinked structure due to hydrogen bonds and a crosslinked structure due to the crosslinking agent (B) can be formed.
[0128] --use--
[0129] The rubber composition of the present invention can be used for a variety of rubber products, such as tires, rubber tracks and vibration-isolating rubbers.
[0130] Example
[0131] The present invention will be described in more detail below with reference to Examples, although the present invention is not limited to these Examples.
[0132] <Analysis of polymer>
[0133] The weight average molecular weight (Mw) of the polymer is measured using the following method.
[0134] (1) Method for measuring weight average molecular weight (Mw)
[0135] The weight average molecular weight (Mw) of the polymer in terms of polystyrene was determined by gel permeation chromatography [GPC: HLC-8321GPC / HT manufactured by Tosoh Corporation, columns: two HT-806M columns manufactured by Showa Denko KK, detector: differential refractometer (RI)] using monodisperse polystyrene as a reference. Note that the measurement temperature was 40°C.
[0136] <Method for synthesizing a polymer having a hydroxyl group>
[0137] The polymer having a hydroxyl group was synthesized by ring-opening metathesis polymerization according to Macromolecules 2020, 53, 4121 using cycloocta-1,5-diene and 5-cyclooctene-1,2-diol as monomers.
[0138] In the synthesized polymer having a hydroxyl group, the ratio of the cycloocta-1,5-diene unit was 80 mol% and the ratio of the 5-cyclooctene-1,2-diol unit was 20 mol% with respect to all constituent units of the polymer. The weight average molecular weight (Mw) was 202,000.
[0139] <Production of Rubber Composition>
[0140] The rubber composition was produced according to the formulation summarized in Table 1. In the mixing, the first stage and the second stage of mixing were performed sequentially. The first stage of mixing was performed at 110° C. for 3 minutes, and the second stage of mixing was performed at 80° C. for 1 minute and 30 seconds. The tensile strength at break (TB) and the elongation at break (EB) of the obtained rubber composition were measured by the following method.
[0141] (2) Measurement methods of TB and EB
[0142] A JIS No. 7 dumbbell-shaped test piece was prepared from the rubber composition, and the tensile strength at break (TB) and the elongation at break (EB) were measured by performing a tensile test at room temperature (23° C.) according to JIS K6251. The tensile strength at break (TB) and the elongation at break (EB) of Comparative Example 1 were expressed as index values by taking the tensile strength at break (TB) and the elongation at break (EB) of Comparative Example 1 as 100. A larger index value indicates a larger tensile strength at break (TB) and the elongation at break (EB).
[0143] [Table 1]
[0144]
[0145] *1 Polymer having hydroxyl groups: Polymer having hydroxyl groups synthesized by the above method
[0146] *2Butadiene rubber: manufactured by Asahi Kasei Corporation, trade name "TUFDENE (registered trademark) 2000R"
[0147] *3 Stearic acid: manufactured by Kao Corporation, trade name "Lunak S-70V"
[0148] *4 Wax: manufactured by Seiko Chemical Co., Ltd., trade name "Suntight A"
[0149] *5 Antioxidant 6PPD: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, manufactured by OUCHI SHINKOCHEMICAL INDUSTRIAL CO., LTD., trade name "NOCRAC 6C"
[0150] *6 Zinc flower: Made by FUJIFILM Wako Pure Chemical Corporation
[0151] *7 Vulcanization accelerator DPG: 1,3-diphenylguanidine, manufactured by Sumitomo Chemical Co., Ltd., trade name "SOXINOL D"
[0152] *8 Vulcanization accelerator CBS: N-cyclohexyl-2-benzothiazolylsulfenamide, manufactured by Sanshin Chemical Industry Co. Ltd., trade name "Sanceler CM-G"
[0153] *9 Vulcanization accelerator DM: di-2-benzothiazole disulfide, manufactured by OUCHI SHINKO CHEMICAL INDUSTRIAL CO., LTD., trade name "NOCCELER DM-P"
[0154] *10 Sulfur: manufactured by FUJIFILM Wako Pure Chemical Corporation
[0155] As can be understood from Table 1, the rubber composition of Example 1 according to the present invention has significantly improved tensile strength at break (TB) and elongation at break (EB) compared to a general sulfur-crosslinked rubber composition (Comparative Example 1).
[0156] Industrial Applicability
[0157] The rubber composition of the present invention can be used for various rubber products such as tires, rubber tracks and vibration-isolating rubbers.
Claims
1. A rubber composition comprising a rubber component (A) and a crosslinking agent (B), in, The rubber component (A) comprises a polymer (A1) having at least two hydroxyl groups and a diene unit, At least two hydroxyl groups in the polymer (A1) are bonded to adjacent carbon atoms, and The content of the crosslinking agent (B) is 0.1 to 8 parts by mass relative to 100 parts by mass of the rubber component (A) and 0.1 to 80 parts by mass relative to 100 parts by mass of the polymer (A1).
2. The rubber composition according to claim 1, wherein The weight average molecular weight (Mw) of the polymer (A1) is 1,000 to 1,000,000.
3. The rubber composition according to claim 1 or 2, wherein: The polymer (A1) comprises a monomer unit derived from a cycloocta-1,5-diene compound represented by the following general formula (1): [Chemical formula 1] Where R 1 are independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms.
4. The rubber composition according to any one of claims 1 to 3, wherein The polymer (A1) comprises a monomer unit derived from a 5-cyclooctene-1,2-diol compound represented by the following general formula (2): [Chemical formula 2] Where R 2 are independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 5 carbon atoms.
5. The rubber composition according to claim 4, wherein In the polymer (A1), the content of the monomer unit derived from the 5-cyclooctene-1,2-diol compound represented by the general formula (2) is 5 to 50 mol%.
6. The rubber composition according to any one of claims 1 to 5, wherein The crosslinking agent (B) contains at least sulfur.