Positive electrode active material for nonaqueous electrolyte secondary battery
By using the composite oxide LixTMtmMyO2-fFf with a Fm-3m space group crystal structure as the positive electrode active substance in the non-aqueous electrolyte secondary battery, the problem of insufficient discharge voltage of the positive electrode active substance in the prior art is solved, and high discharge voltage and Capacity battery performance.
Patent Information
- Application Number
- CN202280093700.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-05
AI Technical Summary
The positive electrode active substances of existing nonaqueous electrolyte secondary batteries are difficult to achieve high discharge voltage, which affects the energy density and output performance of the battery.
The composite oxide with a Fm-3m space group crystal structure is used as the positive electrode active material, and the specific form is LixTMtmMyO2-fFf. The ratio of transition metal TM and non-transition metal M and the content of fluorine are controlled by mechanochemical method to ensure x+ tm+y is between 1.75≤2, f≤0.7, and Q is within the range of 0.8≤2×tm×{1-(1-f/2)5≤1.5.
The discharge voltage and discharge capacity of the nonaqueous electrolyte secondary battery are significantly improved, achieving more efficient electrochemical performance.
Smart Images

Figure CN118901152A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a technology of a positive electrode active material for a non-aqueous electrolyte secondary battery. Background Art
[0002] As a high-output, high-energy-density secondary battery, for example, a nonaqueous electrolyte secondary battery is widely used, which includes a positive electrode, a negative electrode, and a nonaqueous electrolyte and performs charge and discharge by transferring lithium ions etc. between the positive electrode and the negative electrode.
[0003] For example, Patent Document 1 discloses, as a positive electrode active material used in a non-aqueous electrolyte secondary battery, a composite oxide having a crystal structure belonging to the space group Fm-3m, containing lithium and molybdenum and containing substantially no chromium.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-202954 Summary of the invention
[0007] An object of the present disclosure is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge voltage.
[0008] The positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized in that it has a crystal structure belonging to the space group Fm-3m and is represented by the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the above general formula, TM is a transition metal, M is a non-transition metal, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and Q=2×tm×{1-(1-f / 2) 5}, 0.8≤Q≤1.5 is satisfied.
[0009] According to one aspect of the present disclosure, a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge voltage can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment.
[0011] Figure 2 This is a diagram showing the X-ray diffraction results of Example 1.
[0012] Figure 3 This is a diagram showing the X-ray diffraction results of Example 11.
[0013] Figure 4 3 is a diagram showing the X-ray diffraction result of Comparative Example 1.
[0014] Figure 5 It is a graph showing the charge and discharge curve of Example 1.
[0015] Figure 6 It is a graph showing the charge and discharge curve of Example 11.
[0016] Figure 7 3 is a graph showing the charge and discharge curve of Comparative Example 1. DETAILED DESCRIPTION
[0017] An example of a nonaqueous electrolyte secondary battery using the positive electrode active material for a nonaqueous electrolyte secondary battery disclosed in the present invention will be described below.
[0018] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment. Figure 1 The non-aqueous electrolyte secondary battery 10 shown in the figure comprises: a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a shell body 16 and a sealing body 17 for blocking the opening of the shell body 16. It should be noted that, instead of the wound electrode body 14, an electrode body of other forms such as a laminated electrode body in which a positive electrode and a negative electrode are alternately laminated with a separator interposed therebetween may be applied. In addition, as the battery case 15, examples include cylindrical, square, coin-shaped, button-shaped, and other metal cases, resin cases formed by laminating resin sheets (laminated batteries), and the like.
[0019] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may also contain a halogen-substituted product obtained by replacing at least a portion of the hydrogen in these solvents with a halogen atom such as fluorine. Examples of the electrolyte salt include lithium salts such as LiPF6. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte, and may also be a solid electrolyte using a gel-like polymer or the like.
[0020] The shell body 16 is, for example, a metal container in a cylindrical shape with a bottom. A gasket 28 is provided between the shell body 16 and the sealing body 17 to ensure the airtightness inside the battery. The shell body 16 has, for example, a bulging portion 22 in which a part of the side surface bulges inwardly and supports the sealing body 17. The bulging portion 22 is preferably formed in an annular shape along the circumferential direction of the shell body 16, and the sealing body 17 is supported by its upper surface.
[0021] The sealing body 17 has a structure in which a partially opened metal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cover 27 are stacked in sequence from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. When the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 to the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is cut off. When the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.
[0022] Figure 1 In the non-aqueous electrolyte secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode lead 21 attached to the negative electrode 12 extends to the bottom side of the case body 16 through the outside of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the partially opened metal plate 23 as the bottom plate of the sealing body 17 by welding or the like, and the cover 27 as the top plate of the sealing body 17 electrically connected to the partially opened metal plate 23 becomes the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the case body 16 by welding or the like, and the case body 16 becomes the negative terminal.
[0023] The positive electrode 11 , the negative electrode 12 , and the separator 13 are described in detail below.
[0024] <Positive electrode>
[0025] The positive electrode 11 includes a positive electrode current collector and a positive electrode composite material layer disposed on the positive electrode current collector. The positive electrode current collector may be made of a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a thin film having the metal disposed on the surface. The thickness of the positive electrode current collector is preferably in the range of 1 μm or more and 20 μm or less, for example.
[0026] The positive electrode composite material layer preferably contains a positive electrode active material, and further contains a binder, a conductive material, etc. The thickness of the positive electrode composite material layer is preferably in the range of, for example, 10 μm or more and 300 μm or less.
[0027] The positive electrode 11 is obtained, for example, by applying a positive electrode composite material slurry containing a positive electrode active material, a binder, a conductive material, etc., on a positive electrode current collector and drying the slurry to form a positive electrode composite material layer on the positive electrode current collector, and rolling the positive electrode composite material layer.
[0028] The positive electrode active material includes a composite oxide having a crystal structure belonging to the space group Fm-3m.
[0029] The crystal structure belonging to the space group Fm-3m means that in the diffraction pattern obtained by X-ray diffraction (XRD) measurement, there is a peak that can be attributed to the space group Fm-3m. It should be noted that the "-3" in the space group "Fm-3m" represents the object element of the 3-fold regression axis, and should be marked with "-" above the original "3". The X-ray diffraction pattern of the composite oxide can be measured by powder X-ray diffraction using an X-ray diffraction device (Rigaku's "MiniFlexII") and the line source is set to CuKα rays, the tube voltage is set to 40kV, and the tube current is set to 15mA. At this time, the diffracted X-rays are detected by a high-speed one-dimensional detector (D / teX Ultra2) through a metal plate with a thickness of 30μm and a Kβ local opening. In addition, the sampling width is set to 0.02°, the scanning speed is set to 10° / minute, the divergence slit width is set to 0.625°, the light receiving slit width is set to 13mm (OPEN), and the scattering slit width is set to 8mm. In addition, the crystal structure of the composite oxide can be determined based on the obtained X-ray diffraction pattern and by Rietveld analysis using the "RIETAN-FP" program (F. Izumi and K. Momma, Solid State Phenom., 130, 15-20 (2007).). It should be noted that the X-ray diffraction device is not limited to the above-mentioned device, nor is the X-ray source. The X-ray diffraction measurement conditions are not limited to the above-mentioned conditions. In addition, the analysis method of the obtained X-ray diffraction pattern is not limited to the above-mentioned method.
[0030] The composite oxide having a crystal structure belonging to the space group Fm-3m is represented by the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and Q=2×tm×{1-(1-f / 2) 5}, 0.8≤Q≤1.5 is satisfied. Here, Q represents the number of oxygens bound to the transition metal bound to fluorine. By using such a composite oxide, the discharge voltage of the positive electrode active material can be increased. It should be noted that the above-mentioned crystal structure may also have pores in which Li atoms, TM atoms, and M atoms are not configured. Here, having pores means that in the positive electrode active material just after manufacture or taken out by disassembling a discharged secondary battery, there are pores in the composite oxide that are not filled with Li atoms, TM atoms, and M atoms. The molar ratio of the pores is preferably greater than 0.05 and less than 0.25.
[0031] In the general formula, for example, from the viewpoint of obtaining a higher discharge voltage, x, tm, y, and f preferably satisfy 1.0<x≤1.4, 0.4≤tm<1.0, 0≤y≤0.2, and 0.2≤f≤0.6.
[0032] The composite oxide preferably contains Mn as a transition metal (TM), for example, in order to obtain a higher discharge voltage or to increase the discharge capacity. In the general formula, the molar ratio tm_Mn of Mn in tm is preferably 0.6<tm_Mn<0.8.
[0033] The composite oxide preferably contains Mn and a transition metal other than Mn, for example, from the aspect of being able to obtain a higher discharge voltage or from the aspect of improving the discharge capacity. As the transition metal other than Mn, for example, Ni, Co, Fe, Ti, Y, Zr, Nb, Mo, Sc, W, V, Gd, Ce, Ta, etc. can be listed, and Ce, Gd, and Nb are more preferred.
[0034] Examples of the non-transition metal (M) contained in the composite oxide include Al, Mg, Sb, Bi, Ca, Sr, Mg, K, Ga, Sn, and Zn, with Ga and Mg being more preferred.
[0035] The composite oxide preferably contains Mn, and further contains at least one of the five elements of Gd, Ce, Nb as transition metals (TM), and Mg and Ga as non-transition metals (M), and more preferably contains at least three of the five elements, for example, from the aspect of being able to obtain a higher discharge voltage or from the aspect of improving the discharge capacity. In addition, the molar ratio of Mg, Gd, Ce, Nb, and Ga in the composite oxide is preferably greater than 0 and less than 0.025.
[0036] The composition of the composite oxide can be confirmed by, for example, Rietveld analysis of parameters obtained by inductively coupled plasma optical emission spectrometry, X-ray photoelectron spectroscopy, and powder X-ray diffraction.
[0037] The method for producing the composite oxide is not particularly limited, and may be a known method in the synthesis of the positive electrode active material, for example, it may be obtained by treating a lithium source, an additive element source, a fluorine source, etc. using a mechanochemical method. A mechanochemical method (also referred to as mechanochemical treatment, etc.) refers to a synthesis method that utilizes a mechanochemical reaction. A mechanochemical reaction refers to a chemical reaction such as a crystallization reaction, a solid solution reaction, a phase change reaction, etc., which is locally generated by mechanical energy such as friction and compression during the crushing process of a solid substance. As an apparatus for performing a mechanochemical method, a ball mill, a bead mill, a vibration mill, a turbo pulverizer, a mechanical fusion device, a disc mill, and other pulverizers / dispersing machines may be cited. Among these, a ball mill is preferred. The mechanochemical treatment may be carried out in an atmosphere of an inert gas such as argon, or in an oxygen-containing atmosphere.
[0038] Lithium sources include lithium carbonate, lithium hydroxide, etc. The added element source is a compound containing a transition metal and a compound containing a non-transition metal, such as an oxide or hydroxide containing a transition metal, an oxide or hydroxide containing a non-transition metal, a composite oxide or hydroxide containing a transition metal and a non-transition metal, etc. The fluorine source is a fluoride such as lithium fluoride, molybdenum fluoride, magnesium fluoride, etc. It should be noted that lithium fluoride can be used as a lithium source, transition metal fluorides such as molybdenum fluoride can be used as a transition metal-containing compound of an added element source, and non-transition metal fluorides such as magnesium fluoride can also be used as a non-transition metal-containing compound of an added element source.
[0039] The composite oxide obtained by the mechanochemical treatment may be subjected to a heat treatment. The heating temperature is not particularly limited, and is, for example, in the range of 500° C. to 1000° C. In addition, the heating time is not particularly limited, and is, for example, 1 hour to 20 hours. The heating may be performed in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere.
[0040] The positive electrode active material may be composed of the above-mentioned composite oxide alone, or may contain other active materials other than the above-mentioned composite oxide. Examples of other active materials include Li x MO y (M represents at least one transition metal) represented by a composite oxide (Li having a layered α-NaFeO2 type crystal structure) x CoO2、Li x NiO2、Li x MnO2、Li x Ni α Co (1-α) O2、Li x Ni α Mn β Co (1-α-β) O2, etc., Li with spinel crystal structure xMn2O4、Li x Ni α Mn (2-α) O4, etc.), Li w M ’ x (XO y ) z (M' represents at least one transition metal, X represents, for example, P, Si, B, V, etc.) represented by a polyanion compound (LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc.).
[0041] The content of the composite oxide is preferably 50 mass % or more, more preferably 70 mass % or more, and further preferably 90 mass % or more relative to the total mass of the positive electrode active material. The composite oxide has a crystal structure belonging to the space group Fm-3m and is represented by the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and Q=2×tm×{1-(1-f / 2) 5}, 0.8≤Q≤1.5 is satisfied.
[0042] Examples of the conductive material contained in the positive electrode composite material layer include carbon black, acetylene black, Ketjen black, graphite and other carbon powders, etc. These may be used alone or in combination of two or more.
[0043] As the binding material included in the positive electrode composite material layer, for example, fluorine resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), PAN, polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR), CMC or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K etc.), polyvinyl alcohol (PVA) etc. can be used. These can be single 1 kind, and also can be used in combination of 2 or more kinds.
[0044] <Negative electrode>
[0045] The negative electrode 12 includes a negative electrode current collector such as a metal foil, and a negative electrode composite material layer formed on the negative electrode current collector. As the negative electrode current collector, a foil of a metal such as copper that is stable within the potential range of the negative electrode, a film having the metal disposed on the surface, etc. can be used. The negative electrode composite material layer includes, for example, a negative electrode active material, a binder, etc.
[0046] As the negative electrode active material contained in the negative electrode composite material layer, there is no particular limitation as long as it is a material that can absorb / release lithium ions, for example, carbon materials, elements that can form alloys with lithium, or compounds containing the elements, etc. can be listed. As carbon materials, graphites such as natural graphite, difficult graphitization carbon, and artificial graphite, coke, etc. can be used. As elements that can form alloys with lithium and compounds containing the elements, for example, silicon, tin, silicon oxide, tin oxide, etc. formed by combining them with oxygen can be listed. In addition, in addition to the above, materials such as lithium titanate whose charge and discharge potential relative to metallic lithium is higher than that of carbon materials, etc. can also be used. As the binding material contained in the negative electrode composite material layer, the same materials as those in the case of the positive electrode can be listed.
[0047] <Separator>
[0048] For example, a porous sheet having ion permeability and insulation is used as the separator 13. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator 13, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin, or a layer obtained by coating the surface of the separator 13 with aramid resin, etc.
[0049] Example
[0050] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0051] <Example 1>
[0052] [Preparation of positive electrode active material]
[0053] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gadolinium oxide (Gd2O3), and cerium oxide (CeO2) were weighed and mixed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Gd:Ce:F was 1.225:0.705:0.005:0.01:0.005:0.6. The mixed powder was put into a planetary ball mill (Premium-Line P7 manufactured by Fritsch, rotation speed: 600 rpm, container: 45 mL pot made of zirconia, balls: 200 g / min, 100 g / min, ... The treatment was carried out in an Ar atmosphere at room temperature for 35 hours (35 cycles of running for 1 hour and then stopping for 10 minutes). 1.225 Mn 0.705 Mg 0.005 G 0.01 Ce 0.005 O 1.4F 0.6 The composite oxide shown.
[0054] The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 2 The crystal structure was analyzed, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m. The conditions for the powder X-ray diffraction measurement were as described above (the same conditions were also used for other examples and comparative examples).
[0055] [Production of positive electrode]
[0056] The composite oxide was mixed in a ratio of 70 parts by mass, acetylene black was mixed in a ratio of 20 parts by mass, and polyvinylidene fluoride was mixed in a ratio of 10 parts by mass, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode composite material layer slurry. Next, the positive electrode composite material layer slurry was applied to an aluminum foil having a thickness of 15 μm and dried, and the obtained coating was rolled to prepare a positive electrode having a positive electrode composite material layer formed on both sides of the aluminum foil.
[0057] [Preparation of non-aqueous electrolyte]
[0058] A non-aqueous electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) in a mixed solvent of fluoroethylene carbonate (FEC) and methyl propionate (FMP) at a volume ratio of 1:3 at a concentration of 1 mol / L.
[0059] [Production of test battery cells]
[0060] Electrode leads were installed on the metal lithium as the positive electrode and the negative electrode, respectively. Then, an electrode body with a separator sandwiched between the positive electrode and the negative electrode was prepared, and the electrode body was placed in an aluminum laminate film, injected with the non-aqueous electrolyte, and sealed. This was used as the test battery cell (non-aqueous electrolyte secondary battery) of Example 1.
[0061] <Example 2>
[0062] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and niobium oxide (Nb2O5) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ga:Nb:F became 1.225:0.7:0.01:0.01:0.005:0.6. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F0.6 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0063] In addition, using Li 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F 0.6 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0064] <Example 3>
[0065] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Nb:Ce:F became 1.143:0.765:0.02:0.01:0.005:0.447. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0066] In addition, using Li 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0067] <Example 4>
[0068] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gadolinium oxide (Gd2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Gd:Nb:Ce:F of 1.168:0.755:0.005:0.01:0.005:0.447. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.168 Mn 0.755 G 0.005 Nb 0.01 Ce 0.005 O 1.553 F 0.447 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0069] In addition, using Li 1.168 Mn 0.755 G 0.005 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0070] <Example 5>
[0071] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Ga:Nb:Ce:F of 1.175:0.76:0.005:0.005:0.005:0.45. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.175 Mn 0.76 Ga 0.005 Nb 0.005 Ce 0.005 O 1.55 F 0.45 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0072] In addition, using Li 1.175 Mn 0.76 Ga 0.005 Nb 0.005Ce 0.005 O 1.55 F 0.45 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0073] <Example 6>
[0074] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Ga:Nb:Ce:F of 1.2:0.685:0.005:0.005:0.005:0.5. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0075] In addition, using Li 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0076] <Example 7>
[0077] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ga:Ce:F became 1.175:0.7:0.025:0.025:0.025:0.45. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0078] In addition, using Li 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0079] <Example 8>
[0080] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gadolinium oxide (Gd2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Gd:Nb:Ce:F became 1.192:0.73:0.005:0.01:0.005:0.298. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.192 Mn 0.73 G 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0081] In addition, using Li 1.192 Mn 0.73 G 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0082] <Example 9>
[0083] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and niobium oxide (Nb2O5) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ga:Nb:F became 1.2:0.735:0.005:0.005:0.005:0.3. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0084] In addition, using Li 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0085] <Example 10>
[0086] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gadolinium oxide (Gd2O3), and niobium oxide (Nb2O5) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Gd:Nb:F became 1.25:0.73:0.005:0.005:0.01:0.298. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.25 Mn 0.73 Mg 0.005 G 0.005 Nb 0.01 O 1.702 F 0.298 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0087] In addition, using Li 1.25 Mn 0.73 Mg 0.005 G 0.005 Nb0.01 O 1.702 F 0.298 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0088] <Example 11>
[0089] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Mg:Nb:Ce:F of 1.15:0.785:0.005:0.005:0.005:0.2. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.15 Mn 0.785 Mg 0.005 Nb 0.005 Ce 0.005 O 1.8 F 0.2 The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 3 As a result of analyzing the crystal structure, it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m. The conditions for the powder X-ray diffraction measurement are as described above.
[0090] In addition, using Li 1.15 Mn 0.785 Mg 0.005 Nb 0.005 Ce 0.005 O 1.8 F 0.2 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0091] <Comparative Example 1>
[0092] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Ga:Nb:Ce:F of 1.25:0.485:0.005:0.005:0.005:0.5. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 4 As a result of analyzing the crystal structure, it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0093] In addition, using Li 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0094] <Comparative Example 2>
[0095] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ce:F became 1.25:0.45:0.025:0.025:0.5. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0096] In addition, using Li 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0097] <Comparative Example 3>
[0098] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), and lithium peroxide (Li2O2) were weighed as starting sources of the composite oxide so that the molar ratio of Li:Mn:F became 1.667:0.333:1.333. The same operation as in Example 1 was performed except that LiF was weighed so as to obtain LiMnO2. 1.667 Mn 0.333 O 0.667 F 1.333The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belonged to Fm-3m.
[0099] In addition, using Li 1.667 Mn 0.333 O 0.667 F 1.333 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0100] <Comparative Example 4>
[0101] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), and titanium oxide (TiO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Ti:F became 1.2:0.6:0.2:0.2. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.2 Mn 0.6 Ti 0.2 O 1.8 F 0.2 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belonged to Fm-3m.
[0102] In addition, using Li 1.2 Mn 0.6 Ti 0.2 O 1.8 F 0.2 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0103] <Comparative Example 5>
[0104] The same operation as in Example 1 was performed except that LiMnO2 was used as the composite oxide to obtain a composite oxide represented by LiMnO2. The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belonged to Fm-3m.
[0105] Furthermore, a test battery cell was produced in the same manner as in Example 1 using a composite oxide represented by LiMnO 2 .
[0106] <Comparative Example 6>
[0107] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), and lithium peroxide (Li2O2) were weighed as starting sources of the composite oxide so that the molar ratio of Li:Mn:F became 1.1:0.6:0.7. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.1 Mn 0.6 O 1.3 F 0.7 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belonged to Fm-3m.
[0108] In addition, using Li 1.1 Mn 0.6 O 1.3 F 0.7 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0109] <Comparative Example 7>
[0110] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), and lithium peroxide (Li2O2) were weighed as starting sources of the composite oxide so that the molar ratio of Li:Mn:F became 1.14:0.86:0.7. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.14 Mn 0.86 O 1.3 F 0.7 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belonged to Fm-3m.
[0111] In addition, using Li 1.14 Mn 0.86 O 1.3 F 0.7 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0112] [Charge and discharge test]
[0113] For the test battery cells of each embodiment and each comparative example, constant current charging was performed at a constant current of 0.1C until the battery voltage reached 4.95V under a temperature environment of 25°C, and constant voltage charging was performed at 4.95V until the current value reached 0.05C. Then, constant current discharge was performed at a constant current of 0.1C until the battery voltage reached 2.5V. In addition, the value obtained by dividing the total amount of electricity during discharge by the total current was obtained as the discharge voltage. In addition, the discharge capacity (mAh / g) during the above-mentioned constant current discharge was obtained.
[0114] Table 1 summarizes the composition of the composite oxide of each example and each comparative example, the composition (Li x TM tm M y O 2-f F f : TM is a transition metal, M is a non-transition metal) the value of x+tm+y, the value of f and 2×tm×{1-(1-f / 2) 5}=Q value, and the results of discharge capacity and discharge voltage.
[0115] [Table 1]
[0116]
[0117] Compared with Comparative Examples 1 to 7, Examples 1 to 11 all showed high discharge voltages and high discharge capacities. From these results, it is believed that by using a crystal structure belonging to the space group Fm-3m and having the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the figure can obtain a high discharge voltage. In the above general formula, TM is a transition metal, M is a non-transition metal, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and Q=2×tm×{1-(1-f / 2) 5}, 0.8≤Q≤1.5 is satisfied.
[0118] Figure 5 , Figure 6 The charge and discharge curves of Example 1 and Example 11 are shown in the figures. According to these figures, the high discharge voltage in the examples described in the present invention is shown, and it is confirmed that a high discharge capacity can be obtained. The same charge and discharge curves can be obtained for other examples 2 to 10, so good results as shown in Table 1 can be obtained. On the other hand, Figure 7 The charge and discharge curve of Comparative Example 1 is shown. According to the figure, the discharge voltage is low and only a low discharge capacity is obtained in Comparative Example 1. The other Comparative Examples 2 to 7 also have the same charge and discharge curves, and the results are inferior to those of the examples shown in Table 1.
[0119] Description of Reference Numerals
[0120] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 bulge, 23 partially opened metal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cover, 28 gasket.
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, which has a crystal structure belonging to the space group Fm-3m and has the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the general formula, in which TM is a transition metal, M is a non-transition metal, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and Q=2×tm×{1-(1-f / 2) 5 }, 0.8≤Q≤1.5 is satisfied.
2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein In the general formula, x, tm, y and f satisfy 1.0<x≤1.4, 0.4≤tm<1.0, 0≤y≤0.2, 0.2≤f≤0.
6.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The composite oxide contains Mn as the transition metal (TM), In the general formula, in tm, the molar ratio of Mn tm_Mn is 0.6<tm_Mn<0.
8.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 3, wherein The composite oxide contains Mn and a transition metal other than Mn as the transition metal (TM).
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 3, wherein The composite oxide contains at least one element among five elements of Gd, Ce, and Nb as the transition metals (TM) and Mg and Ga as the non-transition metals (M).
6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 3, wherein The composite oxide contains at least three elements among five elements of Gd, Ce, and Nb as the transition metals (TM) and Mg and Ga as the non-transition metals (M).
7. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 5 or 6, wherein In the composite oxide, the molar ratio B of the Mg, the Gd, the Ce, the Nb and the Ga is 0<B≤0.025.