Carbide slag modified biochar for purifying heavy metal sewage and preparation method of carbide slag modified biochar

By combining calcium carbide slag with biomass during the pyrolysis process and using catalysts to improve the porosity and adsorption capacity of biochar, the problem of insufficient adsorption effect of existing biochar on various metal ions is solved, and efficient removal is achieved The sewage treatment of heavy metals reduces the cost of sewage treatment.

CN118904286AInactive Publication Date: 2024-11-08SHAOYANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027152.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing biochar is not effective in treating sewage with multiple metal ions, and the calcium carbide slag resources are not effectively utilized, resulting in high sewage treatment costs.

Method used

By dissolving calcium carbide slag in hydrochloric acid and sodium hydroxide solution for reaction, the calcium carbide slag extract is extracted and combined with biomass during the pyrolysis process, the porosity and adsorption capacity of biochar are improved by using catalysts, through intercalation and surface Modification enhances its adsorption properties to heavy metals.

Benefits of technology

It realizes effective modification of calcium carbide slag, improves the adsorption performance of biochar, can efficiently remove heavy metals, such as chromium and copper in sewage, reduces sewage treatment costs, and has a simple process and good environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904286A_ABST
    Figure CN118904286A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sewage treatment, and relates to carbide slag modified biochar for purifying heavy metal sewage and a preparation method of the carbide slag modified biochar. The method comprises the following steps: adding a carbide slag extract substance into biochar, acidifying and alkalizing carbide slag, adding Mg, Ca, Al, Fe and other metal elements into the biochar through intercalation and surface modification under different proportions, and performing the crosslinking effect of the metal elements to improve the purification performance of the biochar on heavy metal sewage. The carbide slag modified biochar prepared by the method has abundant pores, has better adsorbability, can be used as an adsorbent, and has the adsorption capacity of 95% or more on heavy metal chromium, copper and other elements especially in purification of chromium and copper-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage treatment, and more specifically relates to carbide slag modified biochar for purifying heavy metal sewage and a preparation method thereof. Background Art

[0002] Biochar made from biomass has rich pore structure, strong adsorption performance and good renewability. It has been widely used in sewage treatment and has become the most promising adsorption material. However, pure biochar often has poor adsorption effect, especially in sewage with multiple metal ions. One biochar can often only remove one metal ion.

[0003] It is reported that my country's annual production of calcium carbide slag is as high as 43 million tons, and the cumulative amount has exceeded 100 million tons, which contains 54% to 72% Ca(OH) 2 , 23%~31% SiO 2 、Al 2 O 3 , Fe 2 O 3 Mg 2 O 3 .

[0004] If carbide slag can be used to modify biochar, its interlayer adsorption capacity can be improved, making it easy to adsorb a variety of heavy metal ions, it can not only turn carbide slag into treasure, but also reduce the cost of sewage treatment. It is a green and environmentally friendly technology. Summary of the invention

[0005] The purpose of the present invention is to provide a carbide slag modified biochar for purifying heavy metal wastewater and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art, realize the transformation of carbide slag into treasure, enhance the interlayer adsorption capacity of biochar, and reduce the cost of sewage treatment.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention is to provide a method for preparing carbide slag modified biochar for purifying heavy metal wastewater, the steps comprising:

[0008] Dissolving carbide slag in hydrochloric acid solution, stirring and reacting, and then performing solid-liquid separation to obtain carbide slag solution;

[0009] Adding sodium hydroxide (NaOH) solution to the carbide slag solution, stirring for reaction, filtering out the precipitate to obtain a precipitate product, which is the carbide slag extract;

[0010] After adding the carbide slag extract to the pretreated biomass, the biomass is placed in a pyrolysis furnace for pyrolysis to prepare biochar;

[0011] Add activation liquid to the biochar to continue activation treatment, and obtain the carbide slag modified biochar through centrifugation, washing and drying.

[0012] Ca(OH) in carbide slag extract at high temperature 2 、Fe(OH) 3 、Al(OH) 3 Mg(OH) 2 Decomposes into Fe 2 O 3 、CaO、Al 2 O 3 , MgO, using Al 2 O 3 As a catalyst carrier, it can better support and disperse Fe 2 O 3 , CaO, MgO catalysts, giving full play to Fe 2 O 3 The ferromagnetic function of MgO can oxidize and decompose biomass, increase the chemical reaction rate of biomass pyrolysis, and reduce the activation energy required for biomass pyrolysis reaction. It can give full play to the catalytic effect of MgO on methane and carbon dioxide, converting them into useful fuels, and make the porosity of biochar higher and the pores richer. It can give full play to the catalytic effect of CaO on CO 2 The solidification of the gas reduces the greenhouse gas effect produced by biomass pyrolysis. The synergistic catalytic effect produced by the interface interaction between MgO and the other three catalysts is used to further improve the catalytic activity and stability.

[0013] At the same time, these catalysts can also effectively promote the adsorption of heavy metals in wastewater by attaching to biochar through intercalation and surface modification. During the pyrolysis of biomass, after the water and volatiles are separated, many irregular pores will appear on the surface and inside of the biomass, and carboxyl functional groups will be attached to the surface; in addition, in a high temperature environment filled with various biomass volatiles, Fe 2 O 3 、CaO、Al 2 O 3 , hydroxyl functional groups are easily formed on the surface of MgO, and carboxyl and hydroxyl functional groups are prone to condensation reactions in an acidic environment, thereby prompting these metal oxides to adhere to or intercalate in biochar. When purifying sewage, these metal oxides will remove heavy metals in the sewage through adsorption and surface effects.

[0014] Furthermore, the particle size of the carbide slag is 0.01 to 0.1 mm.

[0015] Furthermore, the concentration of the hydrochloric acid solution is 0.5-6 mol / L.

[0016] Furthermore, the concentration of the NaOH solution is 1-6 mol / L.

[0017] The carbide slag particle size defined in the present invention can promote the carbide slag to react fully with the hydrochloric acid solution to generate calcium chloride, ferric chloride, aluminum chloride and magnesium chloride, and the concentration of the hydrochloric acid solution can make the reaction milder and safer. The strong acid molecules are inserted into the interlayer of the carbide slag powder to convert the carbide slag powder into calcium chloride, ferric chloride, aluminum chloride and magnesium oxide solution and dissolve in water, and the strong acid is used to change the intermolecular force of the carbide slag to increase the solubility of the metal particles therein, which is to increase the conversion of the carbide slag solution into Ca(Cl) 2 、Fe(Cl) 2 、Al(Cl) 3 、Mg(Cl) 2 Effective measures of solution.

[0018] Furthermore, the mass / volume ratio of the carbide slag to the hydrochloric acid solution is 4g / 60-100mL.

[0019] The carbide slag first reacts with hydrochloric acid, which reacts with CaO, FeO, Al 2 O 3 , MgO, etc. to generate the corresponding chloride (such as CaCl 2 、FeCl 2 、AlCl 3 MgCl 2 ), the metal elements in carbide slag can be dissolved and extracted by pickling, while possible impurities can be removed.

[0020] Furthermore, the reaction temperature is 45-65°C.

[0021] Furthermore, the stirring time is 45 to 65 minutes.

[0022] The carbide slag solution defined by the present invention is rich in calcium chloride, ferric chloride, aluminum chloride and magnesium chloride, and the concentration of the sodium hydroxide solution is selected to make the reaction more thorough and safer. The strong base molecules react with the chloride ions in the solution to produce sodium chloride salt, so that the carbide slag solution is converted into calcium hydroxide, ferric hydroxide, aluminum hydroxide and magnesium hydroxide precipitation and separated out from water, which is an effective measure for separating and extracting Ca, Fe, Al and Mg ions from the carbide slag solution.

[0023] Furthermore, the volume ratio of the carbide slag solution to the sodium hydroxide solution is 1:1-2.

[0024] Furthermore, the stirring reaction is carried out at a temperature of 30 to 45° C. and for a time of 50 to 60 minutes.

[0025] Add sodium hydroxide (NaOH) solution to react with the chloride generated above to form an insoluble hydroxide precipitate (such as Ca(OH) 2 、Fe(OH) 3 、Al(OH) 3 Mg(OH) 2 ). The precipitate is filtered out, retaining the metal elements in the carbide slag, providing raw materials for subsequent biochar modification.

[0026] Furthermore, the biomass is bamboo chips and / or wood chips.

[0027] The pretreated biomass in the present invention is obtained by crushing, washing with deionized water (material-liquid ratio 30g / 200mL, 60°C, 100min), drying (60-70°C, 180min), and removing impurities in the biomass to obtain biomass with a certain particle size.

[0028] Furthermore, the particle size of the pretreated biomass is 1 to 3 mm;

[0029] The biomass pyrolysis to prepare biochar as defined in the present invention is completed in a fixed bed pyrolysis furnace, and the pyrolysis furnace adopts a self-pressurized pyrolysis method, and the selection of the pyrolysis final temperature, the heating rate, and the pyrolysis pressure can make the porosity of the biochar higher. The precipitate of calcium hydroxide, iron hydroxide, aluminum hydroxide, and magnesium hydroxide is mixed with biomass in a certain ratio for pyrolysis, so that the porosity of the biochar is higher, and the attachment of these metal ions on the biochar enables the biochar to have the ability to adsorb multiple metal ions in sewage.

[0030] The pyrolysis furnace adopts a self-pressurized pyrolysis method. By increasing the pyrolysis pressure and temperature at the same time, the biomass is cracked and volatile components are released. The hydrocarbons in the biomass are further decomposed into H under the catalytic action of carbide slag extract, pressure and temperature. 2 ,CO,CO 2 , CH 4 These gases flow in the pores of biochar under increased pressure, carrying carbide slag extracts, so that the metal elements in these carbide slag extracts are more and more widely distributed in the pores of biochar. The catalytic effect of carbide slag extracts further expands and enriches the pores of biochar, thereby improving the porosity and adsorption capacity of biochar.

[0031] Furthermore, the final pyrolysis temperature of the pyrolysis furnace is 500-600°C, the heating rate is 10-15°C / min, and the final pressure is 0.3MPa.

[0032] Pretreated biomass (such as bamboo chips, sawdust) will produce biochar during pyrolysis, which is a porous material with a large surface area and adsorption capacity. During the pyrolysis process, the added precipitation product (hydroxide) will interact with the biochar, and the metal ions will be fixed on the surface or in the pores of the biochar, enhancing its adsorption capacity for heavy metals.

[0033] Furthermore, the mass ratio of the precipitation product to the biomass is 1 to 2:20.

[0034] The modified biochar has higher porosity and more active sites, and can more effectively adsorb heavy metal ions such as chromium (Cr), copper (Cu), etc. In practical applications, the modified biochar can be put into sewage containing heavy metals to remove these harmful elements through physical adsorption and chemical binding.

[0035] Furthermore, the activation solution is NaOH solution or hydrogen peroxide.

[0036] Preferably, the concentration of the NaOH solution is 1-6 mol / L; the concentration of the hydrogen peroxide is 3%-7%.

[0037] Treatment in activation liquid can effectively remove the ash produced by the biomass pyrolysis process, making the pores of biochar more transparent and able to better exert its adsorption effect. At the same time, the corrosive effect of NaOH solution and hydrogen peroxide can be used to further increase the porosity of biochar, improve the pore structure of biochar, and improve the adsorption performance of biochar.

[0038] Furthermore, the activation treatment time is 100 to 120 minutes.

[0039] The second technical solution of the present invention is to provide a carbide slag modified biochar prepared by the above preparation method.

[0040] The third technical solution of the present invention is to provide an application of the above-mentioned carbide slag modified biochar in purifying heavy metal-containing wastewater.

[0041] Furthermore, the treatment temperature of the carbide slag modified biochar when used in purifying heavy metal-containing wastewater is 55-60°C.

[0042] Furthermore, the treatment time of the carbide slag modified biochar in purifying heavy metal-containing wastewater is 50 to 60 minutes.

[0043] The present invention discloses the following technical effects:

[0044] The present invention modifies biochar by carbide slag, adds metal elements Mg, Ca, Al, Fe and the like contained in the carbide slag to the biochar through intercalation and surface modification, and utilizes the cross-linking effect between these metal elements to improve the purification performance of the modified biochar for heavy metal wastewater.

[0045] The carbide slag modified biochar of the present invention has the advantages of simple preparation process, low cost, good environmental protection, good practicality, excellent adsorption performance and the like.

[0046] The carbide slag modified biochar prepared by the present invention has abundant pores and good adsorption properties, and can be used as an adsorbent, especially in purifying chromium- and copper-containing wastewater, and the adsorption capacity for heavy metal elements such as chromium and copper can reach more than 95%.

[0047] The carbide slag modified biochar preparation of the present invention is crushed into nanometers and evenly mixed with chromium- and copper-containing sewage, thereby improving the removal efficiency of heavy metals in sewage. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0049] Figure 1 This is a physical picture of the carbide slag powder in step S1 of Example 1;

[0050] Figure 2 This is a physical picture of the carbide slag solution prepared in step S2 of Example 1;

[0051] Figure 3 This is a physical picture of the precipitated product obtained by solid-liquid separation in step S3 of Example 1;

[0052] Figure 4 The SEM images of carbide slag modified biochar prepared in Examples 8 to 11, wherein a is Example 8, b is Example 9, c is Example 10, and d is Example 11;

[0053] Figure 5 The SEM images of carbide slag modified biochars prepared in Examples 12 to 15, wherein a is Example 12, b is Example 13, c is Example 14, and d is Example 15;

[0054] Figure 6 This is a diagram showing the removal effect after adding different carbide slag-modified biochars in Example 1, wherein from left to right are 0g, 1g, 1.5g and 2g of carbide slag-modified biochars. DETAILED DESCRIPTION

[0055] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0056] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0057] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0058] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0059] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0060] Unless otherwise specified, the normal temperature described in the present invention is 25°C.

[0061] The hydrochloric acid solution and the bentonite solution are mixed by glass rod drainage, which can reduce splashing caused by violent mixing, reduce personal injury, and further improve the safety of the preparation process.

[0062] Example 1

[0063] Preparation of carbide slag modified bentonite:

[0064] S1, 4g of carbide slag powder (0.01-0.1mm, Figure 1) was placed in a dried 200 mL beaker, 60 mL of hydrochloric acid (concentration 0.5 mol / L) was measured and added into the beaker by drainage with a glass rod, and the mixture was placed in a stirrer and stirred for 55 min. The system temperature was controlled at 50 °C and stirred for 1 h.

[0065] S2, repeat the centrifugation, take out the upper filtrate with a centrifuge tube, and separate the SiO 2 The insoluble slag is filtered out to prepare carbide slag solution ( Figure 2 ), which is rich in Ca(Cl) 2 、Fe(Cl) 2 、Al(Cl) 3 、Mg(Cl) 2 ;

[0066] S3, take 50mL of carbide slag solution and put it into a dried 100mL beaker, measure 50mL of sodium hydroxide (concentration is 2mol / L) and add it into the beaker by glass rod drainage, put it into the stirrer and stir for 50min, control the system temperature at 45℃, and separate the solid and liquid to obtain the precipitated product ( Figure 3 , rich in Ca(OH) 2 Mg(OH) 2 、Fe(OH) 2 、Al(OH) 3 ), known as carbide slag extract;

[0067] S4, drying the carbide slag extract and crushing it to obtain an additive, and putting it into a flask for later use;

[0068] S5. The biomass (wood chips) was crushed, washed with deionized water (solid-liquid ratio 30 g / 200 mL, 60° C., 100 min), and dried (60-70° C., 180 min) to obtain pretreated biomass with a particle size of 1-3 mm. The pretreated biomass and deionized water were mixed in a mass ratio of 1:50, stirred on an automatic stirrer for 50 min, heated at 50° C. and stirred evenly. After the pretreated biomass was filtered and dried for later use;

[0069] S6, take 0.3g of the additive, mix it with 10g of the dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, adopt a self-pressurized pyrolysis method, adjust the heating rate to 10°C / min, the pyrolysis final temperature to 500°C, and the pyrolysis final pressure to 0.3MPa, and pyrolyze to obtain biochar;

[0070] S7. Put the biochar into a dry 500mL beaker, measure 150mL of sodium hydroxide (concentration is 2mol / L) and add it into the beaker by drainage with a glass rod, put it into the stirrer and stir for 45min, control the system temperature at 65℃, keep stirring for 1h, separate the solid and liquid, and obtain carbide slag modified biochar after drying.

[0071] Take 150mL of the stock solution containing trivalent and hexavalent chromium (trivalent chromium concentration is 300mg / L, hexavalent chromium concentration is 300mg / L), put 0g, 1g, 1.5g and 2.5g of carbide slag modified biochar into the solution, heat the mixed solution to 65℃, stir for 60min, react for 2h, let it stand to room temperature, centrifuge and collect the supernatant. The results are as follows: Figure 6 shown.

[0072] Example 2

[0073] Compared with Example 1, the only difference is that the concentration of the hydrochloric acid added in step S1 is 3 mol / L.

[0074] Example 3

[0075] Compared with Example 1, the only difference is that the concentration of sodium hydroxide added dropwise in step S3 is 4 mol / L.

[0076] Example 4

[0077] Compared with Example 1, the only difference is that the final pyrolysis temperature in step S6 is 600°C.

[0078] Example 5

[0079] Compared with Example 1, the only difference is that the NaOH solution in step S7 is 0.8 mol / L.

[0080] Example 6

[0081] Compared with Example 1, the only difference is that the additive in step S6 is 0.15 g.

[0082] Example 7

[0083] Compared with Example 1, the only difference is that the wood chips are replaced with bamboo chips of equal mass.

[0084] Example 8

[0085] Compared with Example 1, the difference lies in step S6, which is specifically as follows:

[0086] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 400℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0087] Example 9

[0088] Compared with Example 1, the difference lies in step S6, which is specifically as follows:

[0089] Take 2g of additive, mix it evenly with 8g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, adopt a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 600℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0090] Example 10

[0091] Compared with Example 1, the difference lies in step S6, which is specifically as follows:

[0092] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, adopt a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 300℃, the final pyrolysis pressure to 0.2MPa, and prepare biochar by pyrolysis.

[0093] Embodiment 11

[0094] Compared with Example 1, the difference lies in step S6, which is specifically as follows:

[0095] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 350℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0096] Example 12

[0097] Compared with Example 7, the difference lies in step S6, which is specifically as follows:

[0098] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 500℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0099] Embodiment 13

[0100] Compared with Example 7, the difference lies in step S6, which is specifically as follows:

[0101] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 600℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0102] Embodiment 14

[0103] Compared with Example 7, the difference lies in step S6, which is specifically as follows:

[0104] Take 1g of additive, mix it evenly with 9g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 400℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0105] Embodiment 15

[0106] Compared with Example 7, the difference lies in step S6, which is specifically as follows:

[0107] Take 0.5g of additive, mix it evenly with 9.5g of dried pretreated biomass, put them together into a fixed bed pyrolysis furnace, use a self-pressurized pyrolysis method, adjust the heating rate to 10℃ / min, the final pyrolysis temperature to 600℃, the final pyrolysis pressure to 0.3MPa, and prepare biochar by pyrolysis.

[0108] Test example

[0109] Figure 1 This is a physical picture of the carbide slag powder in step S1 of Example 1.

[0110] Figure 2 This is a physical picture of the carbide slag solution prepared in step S2 of Example 1.

[0111] Figure 3 This is a physical picture of the precipitated product obtained by solid-liquid separation in step S3 of Example 1.

[0112] Figure 4 These are SEM images of carbide slag-modified biochars prepared in Examples 8 to 11, wherein a is Example 8, b is Example 9, c is Example 10, and d is Example 11.

[0113] Figure 5These are SEM images of carbide slag modified biochars prepared in Examples 12 to 15, wherein a is Example 12, b is Example 13, c is Example 14, and d is Example 15.

[0114] Figure 6 This is a diagram showing the removal effect after adding different carbide slag-modified biochars in Example 1, wherein from left to right are 0g, 1g, 1.5g and 2g of carbide slag-modified biochars.

[0115] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0116] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing carbide slag modified biochar for purifying heavy metal wastewater, characterized in that the steps include: Dissolving carbide slag in hydrochloric acid solution, stirring and reacting, and then performing solid-liquid separation to obtain a carbide slag solution; Adding sodium hydroxide solution to the carbide slag solution, stirring for reaction, filtering out the precipitate to obtain a precipitate product, which is the carbide slag extract; After adding the carbide slag extract to the pretreated biomass, the biomass is placed in a pyrolysis furnace for pyrolysis to prepare biochar; Add activation liquid to the biochar to continue activation treatment, and obtain the carbide slag modified biochar through centrifugation, washing and drying.

2. The preparation method according to claim 1, characterized in that: The particle size of the carbide slag is 0.01-0.1 mm; the concentration of the hydrochloric acid solution is 0.5-6 mol / L; and the concentration of the sodium hydroxide solution is 1-6 mol / L.

3. The preparation method according to claim 1, characterized in that: The mass / volume ratio of the carbide slag to the hydrochloric acid solution is 4g / 60-100mL.

4. The preparation method according to claim 1, characterized in that: The biomass is bamboo chips and / or wood chips; the reaction temperature is 45-65° C.; and the stirring time is 45-65 min.

5. The preparation method according to claim 1, characterized in that: The volume ratio of the carbide slag solution to the sodium hydroxide solution is 1:1-2.

6. The preparation method according to claim 1, characterized in that: The stirring reaction is carried out at a temperature of 30 to 45° C. and for a time of 50 to 60 minutes.

7. The preparation method according to claim 1, characterized in that: The final pyrolysis temperature of the pyrolysis furnace is 500-600° C., the heating rate is 10-15° C. / min, and the final pressure is 0.3-0.4 MPa; the mass ratio of the precipitation product to the biomass is 1-2:

20.

8. The preparation method according to claim 1, characterized in that: The activation solution is NaOH solution or hydrogen peroxide; the activation treatment time is 100 to 120 minutes.

9. A carbide slag modified biochar prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the carbide slag modified biochar as claimed in claim 9 in purifying wastewater containing heavy metals.