Preparation method of aluminum silicate wool composite purification material

By preparing a lanthanum vanadate-alumina composite coating on an aluminosilicate cotton substrate, the problem of adsorbents being difficult to regenerate after saturation in the home environment was solved, achieving the effect of continuous adsorption and decomposition of organic gases.

CN118904313APending Publication Date: 2024-11-08SHENYANG LIGONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411339126.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In a home environment, adsorbents are difficult to regenerate once saturated, making it challenging to adsorb organic gases.

Method used

A lanthanum vanadate-alumina composite active coating was prepared on an aluminosilicate cotton matrix by a sol-gel method to coat alumina and a hydrothermal method to coat lanthanum vanadate, forming a uniform and dense composite material.

Benefits of technology

This material can continuously adsorb and decompose organic gases in the air without special regeneration treatment, and can effectively purify organic gases in the air for a long time.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of an aluminum silicate wool composite purification material, and belongs to the field of air pollution purification materials. The method comprises the following preparation steps: activating aluminum silicate wool, coating aluminum oxide by a sol-gel method and coating lanthanum vanadate by a hydrothermal method. The lanthanum vanadate-aluminum oxide composite active coating is prepared by two steps of coating aluminum oxide on an aluminum silicate wool matrix activated by hydrochloric acid treatment through a sol-gel method and coating lanthanum vanadate through a hydrothermal method. The material retains the softness of aluminum silicate wool, can adsorb various organic gases in air, can decompose the organic gases under illumination, and can efficiently purify the organic gases in air for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of air pollution purification materials, and specifically relates to a preparation method of an aluminum silicate wool composite purification material. Background Art

[0002] Due to industrial and home decoration reasons, the concentration of organic gases in the air exceeds the acceptable level for the human body, which causes air pollution and harms human health. The organic gases in confined spaces are particularly harmful and must be removed by effective methods. Using adsorbents to remove organic matter from the air by physical adsorption is a common method. Commonly used adsorbents include activated carbon and various porous substances.

[0003] The biggest difficulty in using adsorbents is adsorption saturation. All adsorbents have a maximum adsorption capacity. After exceeding a certain capacity, they will no longer continue to adsorb organic matter. The common way to solve this problem is to regenerate the adsorbent, but this is only applicable to industrial environments. Ordinary households do not have the conditions to regenerate adsorbents. Therefore, how to quickly, conveniently and efficiently regenerate adsorbents has become a very important technical issue. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing an aluminum silicate wool composite purification material, which can be used to purify organic gases in the air.

[0005] The technical solution adopted by the present invention is:

[0006] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0007] Step 1: Activate aluminum silicate wool

[0008] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.25-0.35 mol / L hydrochloric acid solution, heat to 70°C and reflux for 90 min;

[0009] (2) taking out the acid-treated aluminum silicate wool, washing it with pure water, drying it in an oven at 150° C. for 12 h, and then calcining it in an electric furnace at 820 to 850° C. for 3 h to obtain activated aluminum silicate wool;

[0010] Step 2: Sol-gel coating of alumina

[0011] (1) Add 0.15-0.25 mL of concentrated hydrochloric acid and 2.2-2.5 g of sodium dihydrogen phosphate to 35 mL of pure water, and stir to form solution A;

[0012] (2) Add 7.8-8.3 g of aluminum isopropoxide, 1.8-2.1 g of Tween 60, and 3.3-3.6 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0013] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0014] (4) taking out the aluminum silicate wool, leaving it to stand at room temperature for 60 minutes, drying it in an oven at 150° C. for 8 hours, and calcining it in an electric furnace at 450 to 480° C. for 3 hours to obtain aluminum silicate wool coated with alumina;

[0015] Step 3: Hydrothermal coating of lanthanum vanadate

[0016] (1) Add 6.2-6.5 g of lanthanum nitrate, 7.6-8.1 g of ammonium metavanadate and 3.2-3.3 g of ammonium bicarbonate to 200 mL of pure water and stir to form a solution C;

[0017] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0018] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150° C. for 12 h, and then calcined in an electric furnace at 550-620° C. for 3 h to obtain an aluminum silicate wool composite purification material.

[0019] Furthermore, the aluminum silicate wool in step (1) is a flocculent fiber made by melting hard clay clinker in a resistance furnace and blowing it. The main parameters of the aluminum silicate wool are: fiber diameter 15 microns, fiber length 8 mm, density 90 kg / m 3 , withstanding temperature of 900℃.

[0020] Furthermore, the aluminum silicate wool composite purification material uses aluminum silicate wool as a matrix material, and prepares a lanthanum vanadate-aluminum oxide composite active coating through two steps of coating alumina by a sol-gel method and coating lanthanum vanadate by a hydrothermal method; wherein the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.3% to 5.5%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 3.8% to 4.1%.

[0021] Compared with the prior art, the preparation method of the aluminum silicate wool composite purification material of the present invention has the following advantages:

[0022] The present invention prepares a lanthanum vanadate-aluminum oxide composite active coating on an aluminum silicate wool substrate activated by hydrochloric acid treatment by two steps of coating aluminum oxide by a sol-gel method and coating lanthanum vanadate by a hydrothermal method. The composite active coating is evenly distributed on the aluminum silicate wool substrate and is tightly combined. The aluminum silicate wool composite purification material retains the softness of the aluminum silicate wool, and can therefore be used in air purification equipment of various shapes. The material can adsorb various organic gases in the air and decompose the organic gases under light, thereby continuously adsorbing and decomposing the organic gases in the air without the need for a special regeneration process. The aluminum silicate wool composite purification material can purify the organic gases in the air over a long period of time and with high efficiency. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples where no specific conditions are indicated are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0024] Example 1

[0025] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0026] Step 1: Activate aluminum silicate wool

[0027] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.25 mol / L hydrochloric acid solution, heat to 70 °C and reflux for 90 min;

[0028] (2) The acid-treated aluminum silicate wool was taken out, washed with pure water, dried in an oven at 150° C. for 12 h, and then calcined in an electric furnace at 820° C. for 3 h to obtain activated aluminum silicate wool.

[0029] Step 2: Sol-gel coating of alumina

[0030] (1) Add 0.15 mL of concentrated hydrochloric acid and 2.2 g of sodium dihydrogen phosphate to 35 mL of pure water in sequence and stir to form solution A;

[0031] (2) Add 7.8 g of aluminum isopropoxide, 1.8 g of Tween 60 and 3.3 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0032] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0033] (4) The aluminum silicate wool was taken out, allowed to stand at room temperature for 60 minutes, then dried in an oven at 150°C for 8 hours, and then calcined in an electric furnace at 450°C for 3 hours to obtain aluminum silicate wool coated with alumina.

[0034] Step 3: Hydrothermal coating of lanthanum vanadate

[0035] (1) Add 6.2 g of lanthanum nitrate, 7.6 g of ammonium metavanadate and 3.2 g of ammonium bicarbonate to 200 mL of pure water and stir to form solution C;

[0036] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0037] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150°C for 12 hours, and then calcined in an electric furnace at 550°C for 3 hours to obtain an aluminum silicate wool composite purification material. Among them, the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.3%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 3.8%.

[0038] Example 2

[0039] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0040] Step 1: Activate aluminum silicate wool

[0041] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.27 mol / L hydrochloric acid solution, heat to 70 °C and reflux for 90 min;

[0042] (2) The acid-treated aluminum silicate wool was taken out, washed with pure water, dried in an oven at 150°C for 12 h, and then calcined in an electric furnace at 825°C for 3 h to obtain activated aluminum silicate wool.

[0043] Step 2: Sol-gel coating of alumina

[0044] (1) Add 0.16 mL of concentrated hydrochloric acid and 2.2 g of sodium dihydrogen phosphate to 35 mL of pure water in sequence and stir to form solution A;

[0045] (2) Add 7.9 g of aluminum isopropoxide, 1.8 g of Tween 60 and 3.3 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0046] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0047] (4) The aluminum silicate wool was taken out, allowed to stand at room temperature for 60 minutes, then dried in an oven at 150°C for 8 hours, and then calcined in an electric furnace at 455°C for 3 hours to obtain aluminum silicate wool coated with alumina.

[0048] Step 3: Hydrothermal coating of lanthanum vanadate

[0049] (1) Add 6.2 g of lanthanum nitrate, 7.7 g of ammonium metavanadate and 3.2 g of ammonium bicarbonate to 200 mL of pure water and stir to form solution C;

[0050] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0051] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150°C for 12 hours, and then calcined in an electric furnace at 560°C for 3 hours to obtain an aluminum silicate wool composite purification material. Among them, the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.3%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 3.8%.

[0052] Example 3

[0053] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0054] Step 1: Activate aluminum silicate wool

[0055] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.30 mol / L hydrochloric acid solution, heat to 70 °C and reflux for 90 min;

[0056] (2) The acid-treated aluminum silicate wool was taken out, washed with pure water, dried in an oven at 150° C. for 12 h, and then calcined in an electric furnace at 835° C. for 3 h to obtain activated aluminum silicate wool.

[0057] Step 2: Sol-gel coating of alumina

[0058] (1) Add 0.20 mL of concentrated hydrochloric acid and 2.3 g of sodium dihydrogen phosphate to 35 mL of pure water in sequence and stir to form solution A;

[0059] (2) Add 8.0 g of aluminum isopropoxide, 1.9 g of Tween 60 and 3.4 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0060] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0061] (4) The aluminum silicate wool was taken out, allowed to stand at room temperature for 60 minutes, then dried in an oven at 150°C for 8 hours, and then calcined in an electric furnace at 465°C for 3 hours to obtain aluminum silicate wool coated with alumina.

[0062] Step 3: Hydrothermal coating of lanthanum vanadate

[0063] (1) Add 6.3 g of lanthanum nitrate, 7.8 g of ammonium metavanadate and 3.2 g of ammonium bicarbonate to 200 mL of pure water and stir to form solution C;

[0064] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0065] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150°C for 12 hours, and then calcined in an electric furnace at 580°C for 3 hours to obtain an aluminum silicate wool composite purification material. Among them, the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.4%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 3.9%.

[0066] Example 4

[0067] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0068] Step 1: Activate aluminum silicate wool

[0069] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.32 mol / L hydrochloric acid solution, heat to 70 °C and reflux for 90 min;

[0070] (2) The acid-treated aluminum silicate wool was taken out, washed with pure water, dried in an oven at 150° C. for 12 h, and then calcined in an electric furnace at 840° C. for 3 h to obtain activated aluminum silicate wool.

[0071] Step 2: Sol-gel coating of alumina

[0072] (1) Add 0.22 mL of concentrated hydrochloric acid and 2.4 g of sodium dihydrogen phosphate to 35 mL of pure water in sequence and stir to form solution A;

[0073] (2) Add 8.1 g of aluminum isopropoxide, 2.0 g of Tween 60 and 3.5 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0074] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0075] (4) The aluminum silicate wool was taken out, allowed to stand at room temperature for 60 minutes, then dried in an oven at 150°C for 8 hours, and then calcined in an electric furnace at 470°C for 3 hours to obtain aluminum silicate wool coated with alumina.

[0076] Step 3: Hydrothermal coating of lanthanum vanadate

[0077] (1) Add 6.4 g of lanthanum nitrate, 7.9 g of ammonium metavanadate and 3.3 g of ammonium bicarbonate to 200 mL of pure water and stir to form solution C;

[0078] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0079] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150°C for 12 hours, and then calcined in an electric furnace at 610°C for 3 hours to obtain an aluminum silicate wool composite purification material. Among them, the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.4%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 4.0%.

[0080] Example 5

[0081] A method for preparing an aluminum silicate wool composite purification material comprises the following process steps:

[0082] Step 1: Activate aluminum silicate wool

[0083] (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.35 mol / L hydrochloric acid solution, heat to 70 °C and reflux for 90 min;

[0084] (2) The acid-treated aluminum silicate wool was taken out, washed with pure water, dried in an oven at 150°C for 12 h, and then calcined in an electric furnace at 850°C for 3 h to obtain activated aluminum silicate wool.

[0085] Step 2: Sol-gel coating of alumina

[0086] (1) Add 0.25 mL of concentrated hydrochloric acid and 2.5 g of sodium dihydrogen phosphate to 35 mL of pure water, and stir to form solution A;

[0087] (2) Add 8.3 g of aluminum isopropoxide, 2.1 g of Tween 60 and 3.6 mL of glycerol to 220 mL of ethanol and stir to form solution B;

[0088] (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min;

[0089] (4) The aluminum silicate wool was taken out, allowed to stand at room temperature for 60 minutes, then dried in an oven at 150° C. for 8 hours, and then calcined in an electric furnace at 480° C. for 3 hours to obtain aluminum silicate wool coated with alumina.

[0090] Step 3: Hydrothermal coating of lanthanum vanadate

[0091] (1) Add 6.5 g of lanthanum nitrate, 8.1 g of ammonium metavanadate and 3.3 g of ammonium bicarbonate to 200 mL of pure water and stir to form solution C;

[0092] (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h;

[0093] (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150°C for 12 hours, and then calcined in an electric furnace at 620°C for 3 hours to obtain an aluminum silicate wool composite purification material. Among them, the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.5%; the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 4.1%.

[0094] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing an aluminum silicate wool composite purification material, characterized in that: The process includes the following steps: Step 1: Activate aluminum silicate wool (1) Soak 10 g of aluminum silicate wool in 500 mL of 0.25-0.35 mol / L hydrochloric acid solution, heat to 70°C and reflux for 90 min; (2) taking out the acid-treated aluminum silicate wool, washing it with pure water, drying it in an oven at 150° C. for 12 h, and then calcining it in an electric furnace at 820 to 850° C. for 3 h to obtain activated aluminum silicate wool; Step 2: Sol-gel coating of alumina (1) Add 0.15-0.25 mL of concentrated hydrochloric acid and 2.2-2.5 g of sodium dihydrogen phosphate to 35 mL of pure water, and stir to form solution A; (2) Add 7.8-8.3 g of aluminum isopropoxide, 1.8-2.1 g of Tween 60, and 3.3-3.6 mL of glycerol to 220 mL of ethanol and stir to form solution B; (3) Mix solution A and solution B and heat to 35° C., add the activated aluminum silicate wool prepared in step 1, stir and keep warm for 60 min; (4) taking out the aluminum silicate wool, leaving it to stand at room temperature for 60 minutes, drying it in an oven at 150° C. for 8 hours, and calcining it in an electric furnace at 450 to 480° C. for 3 hours to obtain aluminum silicate wool coated with alumina; Step 3: Hydrothermal coating of lanthanum vanadate (1) Add 6.2-6.5 g of lanthanum nitrate, 7.6-8.1 g of ammonium metavanadate and 3.2-3.3 g of ammonium bicarbonate to 200 mL of pure water and stir to form a solution C; (2) placing solution C into a hydrothermal reactor, adding the alumina-coated aluminum silicate wool prepared in step 2, and heating the reactor to 185° C. for 36 h; (3) The aluminum silicate wool treated by hydrothermal treatment is taken out, dried in an oven at 150° C. for 12 h, and then calcined in an electric furnace at 550-620° C. for 3 h to obtain an aluminum silicate wool composite purification material.

2. The method for preparing an aluminum silicate wool composite purification material according to claim 1, characterized in that: The aluminum silicate wool in step (1) is made of hard clay clinker as raw material, melted in a resistance furnace, and blown into flocculent fibers. The main parameters of the aluminum silicate wool are: fiber diameter 15 microns, fiber length 8 mm, density 90 kg / m 3 , withstanding temperature of 900℃.

3. The method for preparing an aluminum silicate wool composite purification material according to claim 1, characterized in that: The aluminum silicate wool composite purification material uses aluminum silicate wool as a matrix material, and prepares a lanthanum vanadate-aluminum oxide composite active coating by two steps of coating aluminum oxide by a sol-gel method and coating lanthanum vanadate by a hydrothermal method; wherein the mass percentage of lanthanum vanadate in the aluminum silicate wool composite purification material is 5.3% to 5.5%; and the mass percentage of aluminum oxide in the aluminum silicate wool composite purification material is 3.8% to 4.1%.