Fluorine-doped carbon nanotube, preparation method thereof and application of fluorine-doped carbon nanotube in efficiently removing phenolic pollutants at low temperature

Through the joint action of fluorine-doped carbon nanotubes and persulfate, the problem that the prior art is difficult to efficiently remove phenolic pollutants at low temperatures is solved, and the effect of efficiently removing phenolic pollutants at low temperatures is achieved, and the effect of efficiently removing phenolic pollutants at low temperatures is reduced. Chemical residues, suitable for stricter emission standards.

CN118904364AActive Publication Date: 2024-11-08NANJING TECH UNIV

Patent Information

Application Number
CN202410995927.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing advanced persulfate oxidation technology is difficult to efficiently remove phenolic pollutants at low temperatures, resulting in a decrease in pollutant removal efficiency.

Method used

By modifying commercial carbon nanotubes with ammonium fluoride, fluorine-doped carbon nanotubes are prepared, which work together with persulfate to improve the activation rate and reaction rate of the catalyst, and achieve efficient removal of phenolic pollutants at low temperatures.

Benefits of technology

The complete and efficient degradation of phenolic pollutants is achieved at extremely low concentrations of persulfate, with a wide range of application, reducing the chemical residues of water after treatment, and meeting stricter emission standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904364A_ABST
    Figure CN118904364A_ABST
Patent Text Reader

Abstract

The invention discloses a fluorine-doped carbon nanotube, a preparation method thereof and an application of the fluorine-doped carbon nanotube in efficiently removing phenolic pollutants at low temperature, the preparation method of the fluorine-doped carbon nanotube comprises the following steps: carrying out first calcination on a carbon nanotube to obtain a calcined carbon nanotube, and carrying out second calcination on the obtained calcined carbon nanotube and NH4F to obtain the fluorine-doped carbon nanotube. The commercial carbon nanotubes and ammonium fluoride are used as raw materials, the materials are simple and easy to synthesize, and the problems that peroxymonosulfate is low in activation efficiency and difficult to carry out at low temperature are solved through a simple carbon-based catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental chemistry, and in particular to a fluorine-doped carbon nanotube and a preparation method thereof, and an application thereof in efficiently removing phenol pollutants at low temperature. Background Art

[0002] This section merely provides background information related to the present disclosure and is not necessarily prior art.

[0003] Water safety is related to human health and life span. It is an important guarantee for the sustainable development of human beings and social economy, and it is also an important issue that people have always been concerned about. Phenol pollutants in water mainly come from industrial activities, such as wastewater discharge from petrochemical, printing and dyeing, and pesticide manufacturing industries, as well as urban fecal sewage and the use of pesticides. Phenol pollutants are not easily degraded naturally in the environment. They can accumulate in water bodies and soil, and may enter the food chain and affect organisms, such as causing slow growth or death of fish, and even changing their taste. For humans, phenol pollutants may cause acute poisoning symptoms such as diarrhea and stomatitis, and long-term exposure may cause chronic health problems such as skin reactions and nervous system effects. Therefore, controlling and treating phenol pollution is crucial to protecting water resources and the ecological environment.

[0004] Persulfate advanced oxidation technology is an advanced wastewater treatment method. This technology has the advantages of fast reaction speed, high treatment efficiency, simple operation and environmental friendliness. It can convert pollutants into low-toxic or non-toxic small molecules in a short time, or even directly mineralize them into carbon dioxide and water. In addition, persulfate as an oxidant has the characteristics of high stability, low volatility and a wide pH adaptability range, but it is indeed greatly affected by temperature. In order to overcome this challenge under low temperature conditions, researchers may use auxiliary means to accelerate the reaction, such as increasing the intensity of the light source, using more effective catalysts or optimizing the reaction conditions. With the advancement of technology, some studies have shown that by selecting suitable activators and optimizing reaction conditions, persulfate advanced oxidation technology can improve its performance at low temperatures to a certain extent, ensuring that it can effectively treat pollutants, including phenolic compounds, at lower temperatures. Summary of the invention

[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a fluorine-doped carbon nanotube and a preparation method thereof and an application thereof for efficiently removing phenol pollutants at low temperature in view of the deficiencies in the prior art.

[0006] In order to solve the above technical problems, the present invention discloses the following technical solutions:

[0007] In a first aspect, the present invention discloses a fluorine-doped carbon nanotube and a method for preparing the same.

[0008] The method comprises the steps of subjecting carbon nanotubes to a first calcination to obtain calcined carbon nanotubes, and subjecting the obtained calcined carbon nanotubes to a second calcination with NH4F to obtain fluorine-doped carbon nanotubes.

[0009] Wherein, the carbon nanotubes are commercial carbon nanotubes.

[0010] The mass of NH4F is 0.9-1.8 times, preferably 1.1-1.6 times, and preferably 1.3-1.4 times that of carbon nanotubes.

[0011] Wherein, the temperatures of the first calcination and the second calcination are independently selected from 450-550°C, preferably 490-510°C, preferably 500°C.

[0012] Wherein, the heating rates of the first calcination and the second calcination are independently selected from 3-9°C / min, preferably 4-7°C / min, preferably 5°C / min.

[0013] Wherein, the time of the first calcination and the second calcination are independently selected from 1-4h, preferably 1.5-3h, preferably 2h.

[0014] Wherein, the first calcination and the second calcination are both carried out in an inert gas atmosphere, preferably an argon atmosphere.

[0015] In a second aspect, the present invention discloses the use of the fluorine-doped carbon nanotubes described in the first aspect in removing phenol pollutants.

[0016] Wherein, the phenolic compounds include phenol, bisphenol A, tetrachlorophenol (4-CP) and the like.

[0017] The fluorine-doped carbon nanotubes and peroxymonosulfate (PMS) work together to remove phenolic pollutants, specifically, the fluorine-doped carbon nanotubes are added to a solution containing phenolic pollutants, and peroxymonosulfate is added to remove the pollutants.

[0018] The mass molar ratio of the fluorine-doped carbon nanotubes to the peroxymonosulfate is 0.01 g:0.5-0.62 μmol, preferably 0.01 g:0.56 μmol.

[0019] Wherein, in the system for removing phenolic pollutants, the dosage of persulfate is 0.07-0.15 mM / 10 ppm of phenolic pollutants, preferably 0.09-0.13 mM / 10 ppm of phenolic pollutants, and preferably 0.11 mM / 10 ppm of phenolic pollutants.

[0020] Among them, in the removal of phenolic pollutants by the fluorine-doped carbon nanotubes, the temperature of the water containing phenolic pollutants is -5 to 30°C, preferably 0-25°C, such as low temperature (0-2°C), 5°C, 10°C, 15°C, 20°C, etc., and the pH of the water containing phenolic pollutants is 3 to 11, such as pH 4, 6, 8, 10.

[0021] Wherein, the removal of phenolic pollutants by the fluorine-doped carbon nanotubes is carried out in an air atmosphere.

[0022] In the present invention, the peroxymonosulfate includes potassium peroxymonosulfate and the like.

[0023] In the prior art, the high-grade oxidation technology based on persulfate will slow down the activation of PMS and the reaction rate of pollutants due to the low temperature environment, resulting in a decrease in the rate of the entire oxidation process, thereby affecting the removal efficiency of pollutants such as phenolic compounds. The fluorine-doped carbon nanotubes provided by the present invention are modified by using ammonium fluoride to modify commercial carbon nanotubes, and a trace amount of fluorine is loaded on the surface of the carbon nanotubes through a high-temperature pyrolysis method, thereby increasing the activation rate of PMS and the reaction rate of pollutants, and can achieve efficient degradation of pollutants at low temperatures, solving the problem that the high-grade oxidation technology of persulfate is difficult to efficiently remove pollutants at low temperatures.

[0024] The present invention uses commercial carbon nanotubes and ammonium fluoride as raw materials, which are simple and easy to synthesize. The present invention uses a relatively simple carbon-based catalyst to simultaneously solve the problems of low activation efficiency of peroxymonosulfate and difficulty in low temperature. The present invention degrades pollutants when the concentration of peroxymonosulfate is only 0.11mM, achieves complete and efficient degradation of pollutants at extremely low concentrations of PMS, reduces chemical residues in the treated water, and is conducive to achieving more stringent emission standards.

[0025] Beneficial effects:

[0026] (1) Compared with CNT0 and CNT, the fluorine-doped carbon nanotubes provided by the present invention can be used not only at room temperature but also in extreme environments (low temperature), and have a wide range of applications.

[0027] (2) The fluorine-doped carbon nanotube catalyst provided by the present invention uses commercial carbon nanotubes and ammonium fluoride as raw materials, which are simple and easy to synthesize. The problem of low persulfate activation efficiency and difficulty in low temperature is solved with a relatively simple carbon-based catalyst.

[0028] (3) The fluorine-doped carbon nanotubes provided by the present invention can enable peroxymonosulfate to degrade pollutants at a concentration of only 0.11 mM, achieving complete and efficient degradation of pollutants at extremely low PMS concentrations, reducing chemical residues in treated water, and facilitating the achievement of more stringent emission standards. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0030] Figure 1 XRD patterns of CNT0, CNT and F-CNT prepared in Example 1.

[0031] Figure 2 This is the Raman image of CNT0, CNT and F-CNT prepared in Example 1.

[0032] Figure 3 This is the X-ray photoelectron spectrum of the CNT and F-CNT prepared in Example 1.

[0033] Figure 4 This is the transmission electron microscopy image and mapping image of the F-CNT prepared in Example 1.

[0034] Figure 5 This is a diagram showing the removal effect of tetrachlorophenol on the CNT0, CNT, F-CNT1, F-CNT2 and F-CNT3 catalysts prepared in Example 1 and Comparative Example 1 at room temperature.

[0035] Figure 6 This is a comparison chart of the removal effects of the F-CNT catalyst prepared in Example 1 on tetrachlorophenol at room temperature and low temperature.

[0036] Figure 7 This is a diagram showing the removal effect of BPA by F-CNT at low temperature. DETAILED DESCRIPTION

[0037] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.

[0038] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0039] The concentration of 4-CP in the reaction solution was determined by high performance liquid chromatography (HPLC, Agilent), with a detection wavelength of 280 nm and a 3.5 μm C18 column (4.6×150 mm). The mobile phase contained ultrapure water and methanol in a ratio of 20:80 (v / v), the flow rate was fixed at 1.0 mL / min, the injection volume was 5 μL, and the column and box temperature were set to 35°C. Under the above conditions, the retention time of 4-CP was about 5 minutes.

[0040] The ppm described in the present invention, unless otherwise specified, means mg / L.

[0041] Example 1

[0042] (1) Preparation methods of CNT0, CNT and F-CNT catalysts

[0043] Commercial carbon nanotubes (length 10-30 μm, diameter 10-20 nm) from Xianfeng Nano were used as a comparative sample for the experiment and named CNT0.

[0044] Commercial carbon nanotubes were placed in a tubular furnace under an argon atmosphere, heated to 500°C at 5°C / min, and calcined for 2 hours. The obtained catalyst was used as a comparative sample of the experiment and was named CNT.

[0045] 0.3g CNT and 0.4155g NH4F were added to a certain amount (about 4mL) of anhydrous ethanol and ground thoroughly until the anhydrous ethanol was completely volatilized. Then, it was placed in a tube furnace under an argon atmosphere, heated to 500℃ at 5℃ / min, and calcined for 2h. Then, it was washed with ultrapure water in an ultrasonic crusher for 10min, filtered, and repeated 3 times. After washing, it was placed in a vacuum drying oven at 70℃ for 6h and ground, named F-CNT.

[0046] Figure 1 The a-region X-ray diffraction pattern (XRD) confirms the crystal composition and defect structure of CNT0, CNT, and F-CNT prepared in Example 1. Figure 1 All three materials show characteristic peaks corresponding to carbon materials near 25° and 44°, which are attributed to the (002) and (100) crystal planes of carbon. Therefore, graphitic carbon and amorphous carbon exist in the three carbon materials.

[0047] Figure 2 The Raman spectra of CNT0, CNT, and F-CNT prepared in Example 1 are given. All Raman spectra show two characteristic peaks: one at 1346 cm -1 The D peak of the sp2 hybridized carbon network and the peak at 1571 cm -1 The G peak of CC stretching sp2. D peak intensity (I D ) and G peak intensity (I G ) ratio (I D / I G ) represents the defect size related to the electron transfer ability of the carbon material. D / I G The values ​​are 0.66, 0.51, and 0.58, respectively. This indicates that high-temperature calcination increases the defects of carbon nanotubes, and fluorine doping reduces the structural defects of carbon nanotubes.

[0048] Figure 3 It is the X-ray photoelectron spectrum of F-CNT prepared in Example 1; by comparing the carbon peaks of CNT and F-CNT, it is found that the carbon peak of F-CNT may be slightly shifted to the left due to fluorine doping, and the scanning of the fluorine peak confirms the doping of fluorine element.

[0049] Figure 4 The morphology and mapping of F-CNT prepared in Example 1. TEM shows that it has a typical CNT tubular structure, and high temperature calcination does not affect the structure and morphology of the CNT sample. EDX element mapping of C, O and halogen elements confirms that fluorine is successfully doped.

[0050] (2) Solution preparation

[0051] Weigh 0.5 g of tetrachlorophenol and dissolve it in 1000 mL of ultrapure water to prepare a 500 ppm 4-CP solution.

[0052] 0.5 g of bisphenol A (BPA) was weighed and dissolved in 1000 mL of ultrapure water to prepare a 500 ppm BPA solution.

[0053] Weigh 0.123 g of potassium permonosulfate and dissolve it in 2 mL of ultrapure water to prepare a 200 mM PMS solution.

[0054] Example 2

[0055] The removal effects of the three catalysts in Example 1 on 4-CP at room temperature were compared.

[0056] 1 mL of 4-CP in Example 1 was added to 49 mL of ultrapure water to prepare a 10 ppm 4-CP solution, and then 0.01 g of catalyst was added to the prepared 4-CP solution. After adding 28 μL of the PMS solution in Example 1, the pH of the solution was 3-4. It was placed in a 25°C water bath, and 0.5 mL of the reaction solution was taken out at a specific time point, filtered using a 0.45 μm polytetrafluoroethylene membrane, and then mixed evenly with 0.5 mL of methanol and tested using a liquid chromatograph.

[0057] The results are as follows Figure 5 As shown in the figure, it was found through experiments that 4-CP was basically not removed in the CNT0 / PMS system; the 4-CP removal rate of the CNT / PMS system was greatly improved compared with the CNT0 / PMS system, but it still could not be completely removed. Calcination can improve the catalytic properties of carbon nanotubes, but the effect is not very ideal; the F-CNT / PMS system showed the best degradation efficiency and could degrade 100% of pollutants within 6 minutes, which shows that the fluorine doping strategy significantly improved the catalytic performance of carbon nanotubes.

[0058] Example 3

[0059] The removal effect of the F-CNT catalyst on 4-CP at room temperature and low temperature in comparative example 1.

[0060] 1 mL of the solution in Example 1 was added to 49 mL of ultrapure water to prepare a 10 ppm 4-CP solution, and then 0.01 g of the catalyst was added to the prepared 4-CP solution. After adding 28 μL of the PMS solution in Example 1, the pH of the solution was 3-4. It was placed in a 25°C water bath and a 0°C water bath filled with an ice-water mixture. 0.5 mL of the reaction solution was taken out at a specific time point, filtered using a 0.45 μm polytetrafluoroethylene membrane, and then evenly mixed with 0.5 mL of methanol and tested using a liquid chromatograph.

[0061] The results are as follows Figure 6 As shown, experiments have shown that F-CNT can still completely remove 4-CP efficiently and quickly at low temperatures.

[0062] Comparative Example 1

[0063] 0.3g CNT and 0.24g polyvinylidene fluoride (PVDF) were added to a certain amount (about 4mL) of anhydrous ethanol and fully ground until the anhydrous ethanol was completely volatilized. Then, it was placed in a tubular furnace under an argon atmosphere, heated to 500°C at 5°C / min, and calcined for 2h. Then, it was washed with ultrapure water in an ultrasonic crusher for 10min, filtered, and repeated 3 times. After washing, it was placed in a vacuum drying oven at 70°C for 6h and ground to prepare comparative sample 1, named F-CNT1.

[0064] Comparative sample 2 was prepared using the same method using 0.207 g of perfluorooctanoic acid as a fluorine source and was named F-CNT2.

[0065] In order to compare the catalytic performance of the control sample, the 4-CP degradation experiment in Example 2 was carried out using F-CNT1 and F-CNT2 as catalysts.

[0066] from Figure 5 It can be seen that the catalytic performance of F-CNT1 and F-CNT2 is much lower than that of F-CNT, so ammonium fluoride is the most suitable fluorine source.

[0067] Example 4

[0068] 1 mL of BPA in Example 1 was added to 49 mL of ultrapure water to prepare a 10 ppm 4-CP solution, and then 0.01 g of catalyst was added to the prepared BPA solution, and 28 μL of the PMS solution in Example 1 was added, and the pH of the solution was 3-4. It was placed in a 0°C water bath, and 0.5 mL of the reaction solution was taken out at a specific time point, filtered with a 0.45 μm polytetrafluoroethylene membrane, and then evenly mixed with 0.5 mL of methanol and tested using a liquid chromatograph.

[0069] The results are as follows Figure 7 As shown, experiments have shown that F-CNT can still completely remove BPA efficiently and quickly at low temperatures.

[0070] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing fluorine-doped carbon nanotubes, characterized in that: The carbon nanotubes are subjected to a first calcination to obtain calcined carbon nanotubes, and the calcined carbon nanotubes are subjected to a second calcination with NH4F to obtain fluorine-doped carbon nanotubes.

2. The preparation method according to claim 1, characterized in that: The mass of the NH4F is 0.9-1.8 times that of the carbon nanotubes, preferably 1.1-1.6 times, and preferably 1.3-1.4 times.

3. The preparation method according to claim 1, characterized in that: The temperatures of the first calcination and the second calcination are independently selected from 450-550°C, preferably 490-510°C, preferably 500°C.

4. The preparation method according to claim 1, characterized in that: The heating rates of the first calcination and the second calcination are independently selected from 3-9°C / min, preferably 4-7°C / min, preferably 5°C / min.

5. The preparation method according to claim 1, characterized in that: The time of the first calcination and the second calcination are independently selected from 1-4 hours, preferably 1.5-3 hours, preferably 2 hours; preferably, the first calcination and the second calcination are both carried out under an inert gas atmosphere, preferably an argon atmosphere.

6. Fluorine-doped carbon nanotubes prepared by the method according to any one of claims 1 to 5.

7. Use of the fluorine-doped carbon nanotubes according to claim 6 in removing phenol pollutants; preferably, the phenolic compounds include phenol, bisphenol A, and tetrachlorophenol.

8. The use according to claim 7, characterized in that: The fluorine-doped carbon nanotubes and peroxymonosulfate remove phenolic pollutants.

9. The use according to claim 8, characterized in that: The mass molar ratio of the fluorine-doped carbon nanotubes to the peroxymonosulfate is 0.01 g:0.5-0.62 μmol, preferably 0.01 g:0.56 μmol.

10. The use according to any one of claims 7 to 9, characterized in that: The temperature for removing phenolic pollutants by the fluorine-doped carbon nanotubes is -5 to 30°C, preferably 0 to 25°C.

Citation Information

Patent Citations

  • Carbon nano-tube with fluorine-containing surface and preparation method thereof

    CN102730664A

  • Preparation method and application of defective carbon nanotubes

    CN109174074A

  • Fluorinated bamboo-like carbon nanotubes as well as preparation method and application thereof

    CN112645309A

  • Fluorine-modified double-walled carbon nanotube

    JP2006240938A

Cited By

  • Fluorine-doped Fe-N-C composite material as well as preparation method, application and regeneration thereof

    CN119707074A

  • A fluorine-doped fe-n-c composite material, a preparation method and application and regeneration thereof

    CN119707074B

  • Fluorine-doped carbon material and application thereof in removal of antibiotics

    CN119735290A

  • Fluorine-doped carbon material and its use in removing antibiotics

    CN119735290B