Copper-doped iron-based MOF catalyst and preparation and application thereof

By introducing copper into iron-based MOF and adjusting its distribution by multi-stage solvent thermal method, the problems of short reactive oxygen life and poor environmental tolerance of iron-based MOF catalysts are solved, and the deep treatment and dyeing effect of complex printing and dyeing wastewater are achieved. promote.

CN118904398APending Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH TONGXIANG RES INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411057273.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When treating printing and dyeing wastewater, the existing iron-based MOF catalyst has a short life and poor environmental tolerance, making it difficult to adapt to complex water quality, which limits its application range.

Method used

By introducing copper into iron-based MOF, the oxidation properties of Cu(II) and Fe(III) and 3d orbital distribution differences are used to adjust the distribution of copper doping by multi-stage solvothermal method to improve the Lewis acid density on the catalyst surface. Selectively generate 1O2 as the primary reactive oxygen species, extending its lifespan and enhancing environmental tolerance.

Benefits of technology

The deep treatment of complex printing and dyeing wastewater and excellent dyeing effect are achieved, and the environmental tolerance and application range of the catalyst are improved, especially in the reuse dyeing of dark and blue dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904398A_ABST
    Figure CN118904398A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst synthesis, in particular to a copper-doped iron-based MOF catalyst and preparation and application thereof. The invention provides a preparation method of a copper-doped iron-based MOF (Metal Organic Framework) catalyst, and the copper-doped iron-based MOF catalyst is obtained by carrying out solvothermal reaction on N, N-dimethylformamide containing copper salt, iron salt and terephthalic acid and then drying, the solvothermal reaction is carried out at 50 DEG C for 20-30 minutes, then at 100 DEG C for 20-30 minutes, and then at 150 DEG C for 14-22 hours. According to the method for preparing the copper-doped Fe-MOFs through multi-stage solvothermal insulation, the Lewis acid site density on the surface of the catalyst is regulated and controlled, and < 1 > O2 is selectively generated in the ozone catalysis process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst synthesis, and in particular to a copper-doped iron-based MOF catalyst and a preparation and application thereof. Background Art

[0002] In response to the current problem of preventing and controlling polluted wastewater, heterogeneous catalytic ozonation (HCO) technology has the advantages of fast reaction speed, no secondary pollution, and clean and easy oxygen source. It shows strong competitiveness in advanced oxidation processes (AOPs) and is considered to be a very promising deep treatment technology for printing and dyeing wastewater.

[0003] The key to the application of HCO technology lies in the research and development of efficient ozone catalysts. Metal organic framework materials (MOFs) have the characteristics of rich pore structure, unsaturated metal coordination, and structurally modifiable design, which can provide a unique solution to the problem of active site exposure and mass transfer enrichment. Among them, iron-based MOF (Fe-MOFs) materials, when combined with HCO technology, show excellent performance in the deep treatment of printing and dyeing wastewater. Fe-MOFs are easily activated by ozone (Ozone, O3) to generate ·OH, but although ·OH has relatively high activity, it has a short life and poor environmental tolerance, and is suitable for the treatment of printing and dyeing wastewater with relatively simple water quality components.

[0004] Therefore, improving the main reactive oxygen species (ROS) groups of iron-based MOF catalysts can broaden their application scope in printing and dyeing wastewater. Summary of the invention

[0005] The present invention provides a copper-doped iron-based MOF catalyst and its preparation and application. The present invention utilizes the differences in oxidizability and 3d orbital distribution between Cu(II) and Fe(III) to adjust the electron density of the active center of the iron metal by copper doping through a multi-stage solvent thermal method, thereby improving the Lewis acid site density on the surface of the iron-based MOF catalyst and regulating the 1 O2 is the main active oxygen group. 1 The long life cycle of O2 enables the treatment of printing and dyeing wastewater with complex components; at the same time, the treated printing and dyeing wastewater still shows excellent dyeing effect in reuse dyeing.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a copper-doped iron-based MOF catalyst. The copper-doped iron-based MOF catalyst is obtained by subjecting N,N-dimethylformamide containing copper salt, iron salt and terephthalic acid to a solvent thermal reaction and then drying; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.

[0008] The present invention provides a method for preparing copper-doped Fe-MOFs by multi-stage solvent thermal insulation. The copper atoms and iron atoms are fully combined through oxygen bridge bonds to form more stable crystal nuclei by multi-stage heating. The growth rate of the crystal nuclei can be controlled during the gradient heating process to achieve uniform doping of copper atoms, thereby achieving regulation of the Lewis acid site density on the surface of Fe-MOFs, so that the selective generation of Fe-MOFs in the ozone catalysis process is achieved. 1 O2.

[0009] Specifically, at the low temperature stage of 50°C, the metal precursor and the ligand begin to interact slowly, but the reaction rate is slow, forming a metastable structure. At 100°C, the binding force between the Cu ions and the ligands in the metastable structure is enhanced. At this time, the Cu ions begin to be more effectively incorporated into the framework of the Fe-MOF to form oxygen bridge bonds (-O- bonds), which helps to stabilize the formation of the crystal nucleus. At this stage, the growth of the crystal nucleus begins to accelerate, but the growth rate can be adjusted by controlling the temperature to prevent the grains from being too large or too small and ensure the uniform distribution of Cu. Finally, the temperature is raised to 150°C and enters the strong binding stage. At this time, the Fe-O-Cu bond binding force between the copper atoms and the iron atoms is rapidly enhanced under high temperature and high pressure, allowing the Cu uniformly distributed in the framework of the Fe-MOF to be tightly bound to the entire Fe-MOF framework. In this process, the Lewis acid site density on the surface of Fe-MOFs is changed.

[0010] The applicant prepared copper-doped Fe-MOFs by multi-stage solvent thermal insulation, and finally obtained a catalyst with regulated Lewis acid site density, which showed extremely strong advantages in directional catalysis.

[0011] Preferably, the solvent thermal reaction is: 50°C for 30 min, then 100°C for 30 min, then 150°C for 16 to 20 h.

[0012] Further preferably, the solvent thermal reaction is: 30 min at 50°C, then 30 min at 100°C, then 18 h at 150°C.

[0013] Preferably, the molar ratio of copper to iron in the copper salt and the iron salt is 1:(1-4).

[0014] The molar ratio of copper to iron affects the doping amount of copper in the iron-based MOF. The applicant found that Fe-MOFs with different doping amounts exhibited different Lewis acid site densities in the ozone catalytic oxidation system. Furthermore, the copper-doped iron-based MOF catalyst was applied to the ozone catalytic oxidation system and found that: ozone decomposes to produce ·OH to produce 1 The degree of O2 modulation has a certain dependence on the copper doping ratio. As the copper doping ratio increases, ·OH 1 When the molar ratio of copper to iron is 1:(1-4), 1 O2 concentration is controlled at 1.38*10 -5 ~2.60*10 -5 μM.

[0015] Further preferably, the molar ratio of copper to iron in the copper salt and the iron salt is 1:(3-4).

[0016] Preferably, the iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.

[0017] Preferably, the copper salt is selected from any one of copper nitrate, copper sulfate and copper chloride.

[0018] Preferably, the ratio between the total molar amount of copper and iron in the copper salt and the iron salt and the molar amount of terephthalic acid is 1:1.

[0019] Preferably, the drying temperature is 80-120° C., and the drying time is 12-36 hours.

[0020] More preferably, the drying temperature is 100° C. and the drying time is 24 hours.

[0021] The present invention also provides a copper-doped iron-based MOF catalyst prepared by the above method.

[0022] The present invention also provides the use of a copper-doped iron-based MOF catalyst in the ozone-catalyzed oxidation degradation of electron-rich organic pollutants.

[0023] 1 The O2-dominated MIL-53(FeCu)-18H / ozone system showed a more efficient and thorough degradation effect in the degradation of electron-rich organic pollutants than other degradants. The reason is that 1 O2 has strong electrophilicity and can easily attack the electron-rich groups in electron-rich organic pollutants during the catalytic degradation process, causing the electron-rich organic pollutants to quickly decolorize and degrade.

[0024] The present invention also provides application of copper-doped iron-based MOF catalyst in the treatment of printing and dyeing wastewater.

[0025] Preferably, the treated printing and dyeing wastewater can be used for dyeing.

[0026] At the same time, the printing and dyeing wastewater deeply treated by MIL-53 (FeCu2) -18H catalytic ozone oxidation technology is reused in the process of dyeing knitted cotton fabrics with reactive dyes, which is more suitable for blue and dark colors.

[0027] Therefore, the present invention has the following beneficial effects:

[0028] (1) The present invention provides a method for preparing copper-doped Fe-MOFs by multi-stage solvent thermal insulation. The copper atoms and iron atoms are fully combined through oxygen bridge bonds to form more stable crystal nuclei by multi-stage heating. The growth rate of the crystal nuclei can be controlled during the gradient heating process to achieve uniform doping of copper atoms, thereby achieving regulation of the Lewis acid site density on the catalyst surface, so that the selective generation of Fe-MOFs in the ozone catalysis process is achieved. 1 O2.

[0029] (2) The series of catalysts prepared by copper-doping Fe-MOFs in the present invention can effectively reduce the density of Lewis acid sites on the surface of Fe-MOFs and enhance the selective production of catalytic ozone. 1 The efficiency of O2 provides new ideas for the development of catalytic materials for efficient and directional catalytic ozone conversion.

[0030] (3) The copper-doped Fe-MOFs ozone catalyst developed in the present invention is used to deeply treat the effluent from the secondary sedimentation tank of a printing and dyeing enterprise and is applied to the reactive dyeing process for knitted cotton, showing good recycling performance, among which dark and blue dyes have better recycling dyeing performance; it can realize the reuse of printing and dyeing wastewater, save energy, and achieve efficient circulation and green development.

[0031] (4) The present invention develops 1 The O2-dominated copper-doped Fe-MOFs / ozone system has strong environmental tolerance and strong anti-interference to water matrices such as high concentrations of inorganic salts. It is suitable for deep treatment of printing and dyeing wastewater with high salt content, complex water quality components and variable matrix composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 PXRD spectra of MIL-53(Fe)-18H before and after copper doping;

[0033] Figure 2 are SEM images, where Figure a corresponds to MIL-53(Fe)-18H, Figure b corresponds to MIL-53(FeCu1)-18H, Figure c corresponds to MIL-53(FeCu2)-18H, and Figure d corresponds to MIL-53(FeCu3)-18H;

[0034] Figure 3FT-IR spectra of undoped and copper-doped MIL-53(Fe)-18H, where Figure b is an enlarged view of Figure a;

[0035] Figure 4 The pore size distribution diagrams of undoped and copper-doped MIL-53(Fe)-18H, where Figure a is the nitrogen adsorption / desorption curve diagram and Figure b is the pore size distribution diagram;

[0036] Figure 5 XPS spectra of undoped and copper-doped MIL-53(Fe)-18H, where a is the full spectrum, b is Cu2p, and c is O1s;

[0037] Figure 6 are Py-FTIR spectra, where Figure a corresponds to MIL-53(Fe)-18H, Figure b corresponds to MIL-53(FeCu1)-18H, Figure c corresponds to MIL-53(FeCu2)-18H, Figure d corresponds to MIL-53(FeCu3)-18H, and Figure e corresponds to the surface Lewis acid site density map;

[0038] Figure 7 Solid-state EPR spectra of undoped and copper-doped MIL-53(Fe)-18H;

[0039] Figure 8 EPR spectra of undoped and copper-doped MIL-53(Fe)-18H catalytic ozone system, where a is DMPO / ·OH and b is DMPO / O2 ·- , c is TEMP / 1 O2;

[0040] Fig. 9 ·OH and 1 O2 concentration measurement diagram, where a is the fluorescence spectrum of catalytic ozone oxidation of coumarin, b is the curve of the cumulative concentration of ·OH produced over time, c is the bar graph of the cumulative concentration of ·OH, d is the degradation curve of oxidized MDE, e is the corresponding pseudo-first-order kinetic fitting curve, and f is 1 O2 steady-state concentration bar graph;

[0041] Fig.10 The effect of different quenchers on phenol degradation;

[0042] Fig.11 The comparison diagram of the contribution of quencher to phenol degradation, where Figure a shows the effect of k value, and Figure b shows the contribution rate of ROS to phenol degradation;

[0043] Fig.12The ozone degradation diagram of undoped and copper-doped MIL-53(Fe)-18H, where a is AO-7, b is SMX, and c is ATZ;

[0044] Fig.13 is the ozone decomposition diagram, where a is the ozone decomposition curve and b is the pseudo-first-order kinetic fitting curve (b);

[0045] Fig.14 is the linear relationship between the copper doping amount and the Lewis total acid density, where a is the Cu doping ratio, b is the EPR intensity of OH, c is the cumulative concentration, and d is 1 EPR intensity of O2, e is the steady-state concentration;

[0046] Fig.15 This is the dyeing process flow chart;

[0047] Fig.16 This is the EEM image of MIL-53 (FeCu2) -18H catalytic ozone deep treatment of printing and dyeing wastewater, where a is the printing and dyeing wastewater before treatment, b is the treatment after 30 minutes, and c is the corresponding water sample picture;

[0048] Fig.17 is the UV-visible absorption spectrum of the reactive dye, where a corresponds to 0.1% concentration of red, b corresponds to 0.1% concentration of yellow, and c corresponds to 0.1% concentration of blue;

[0049] Fig.18 is the reflectance curve of knitted cotton fabric dyed with reactive dyes, where a corresponds to red, b corresponds to yellow, and c corresponds to blue;

[0050] Fig.19 The effect of water matrix on the catalytic effect of catalyst, where a corresponds to SO4 2- , b corresponds to Cl - , c corresponds to HCO3 - , d corresponds to CO3 2- , e corresponds to HA, f is the k value corresponding to a~e;

[0051] Fig. 20 Figure 2 is the catalyst stability result diagram, a is the FT-IR spectrum before and after repeated use, and b is the PXRD spectrum before and after repeated use. DETAILED DESCRIPTION

[0052] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0053] [Example]

[0054] Example 1

[0055] In this embodiment, copper accounts for 0.2 of the total metal molar amount.

[0056] Copper-doped MIL-53(Fe)-18H was prepared by a solvothermal method. The specific preparation method is as follows: at room temperature, a metal salt mixed with 16mmol FeCl3·6H2O and 4mmol Cu(NO3)·3H2O and 20mmol terephthalic acid (H2BDC) was dissolved in 120mL N,N-dimethylformamide (DMF) to obtain a clear and transparent precursor solution, which was then transferred to a polytetrafluoroethylene reactor and kept at 50℃ for 30min, then heated to 100℃ for another 30min, and finally heated to 150℃ for 18h. After the reaction timer was terminated, the crude catalyst was obtained by centrifugation at 10000rpm for 5min after natural cooling, and then washed at least three times with 50mL DMF and 50mL ethanol respectively to completely remove residual raw materials and impurities. Finally, the washed solid was placed in a vacuum oven at 100℃ and dried for 24h to obtain a yellow powder catalyst, which was marked as MIL-53(FeCu1)-18H.

[0057] Example 2

[0058] In this embodiment, copper accounts for 0.3 of the total metal molar amount.

[0059] This embodiment is basically the same as embodiment 1, except that the amount of Cu(NO3)·3H2O used is 6 mmol, and the amount of FeCl3·6H2O used is 14 mmol; it is marked as MIL-53(FeCu2)-18H.

[0060] Example 3

[0061] In this embodiment, copper accounts for 0.5 of the total metal molar amount.

[0062] This embodiment is basically the same as embodiment 1, except that the amount of Cu(NO3)·3H2O used is 10 mmol, the amount of FeCl3·6H2O used is 10 mmol and is marked as MIL-53(FeCu3)-18H.

[0063] Comparative Example 1

[0064] This comparative example is basically the same as Example 1, except that the metal salts of 16 mmol FeCl3·6H2O and 4 mmol Cu(NO3)·3H2O are replaced by 20 mmol FeCl3·6H2O, and are labeled as MIL-53(Fe)-18H.

[0065]

Performance test

[0066] 1. Structural characterization

[0067] ①Crystal structure

[0068] In order to explore the structural evolution caused by the copper doping amount, the copper-doped MIL-53(Fe)-18H obtained in Examples 1 to 3 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were subjected to PXRD tests. The results are as follows: Figure 1 shown.

[0069] observe Figure 1 It can be seen that the characteristic peaks at 9.4° and 18.9° 2θ are respectively attributed to the (220) and (11-1) crystal planes of the MIL-53(Fe) material. Figure 1 It can be observed that with the increase of copper doping ratio, the ratio of the two peak intensities changes significantly, indicating that copper doping can significantly affect the crystal structure of MIL-53(Fe)-18H. Specifically, the intensity ratio of the characteristic peaks at 9.4° and 18.9° is calculated, and the values ​​of MIL-53(Fe)-18H, MIL-53(FeCu1)-18H, MIL-53(FeCu2)-18H and MIL-53(FeCu3)-18H are 1.52, 2.02, 3.07 and 3.25, respectively, showing an increasing pattern, indicating that MIL-53(Fe)-18H is oriented toward the (220) crystal plane with the increase of copper doping ratio, that is, from the morphology, it is inferred that the proportion of the bipyramidal parts at both ends decreases, the middle columnar part increases, and gradually shows a rod-like morphology.

[0070] ② Appearance

[0071] In order to further verify the results of PXRD, the copper-doped MIL-53(Fe)-18H obtained in Examples 1 to 3 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were subjected to SEM tests, and the results are as follows: Figure 2 shown.

[0072] observe Figure 2It can be seen that copper doping significantly changes the crystal micromorphology of MIL-53(Fe)-18H, and different copper doping ratios also have an effect on its crystal micromorphology. Undoped MIL-53(Fe)-18H presents a bipyramidal diamond-like shape, accompanied by many surface cracks, and the longitudinal size of the crystal is about 3-4μm; MIL-53(FeCu1)-18H crystals have a spindle structure due to the elongation of the middle columnar part, and the surface cracks also disappear; as the middle columnar part continues to elongate, MIL-53(FeCu2)-18H crystals present a rod-like structure, and large cracks appear on the surface, and the longitudinal size of the crystal is about 5μm; although the longitudinal size of MIL-53(FeCu3)-18H crystals decreases, the proportion of the length of the middle columnar part still increases, and it can be observed that some cracks have intensified, and even fragments have peeled off from the main body. From the perspective of the proportion of the middle columnar length of the MIL-53(Fe)-18H crystal, the evolution of its morphology with the increase of the copper doping ratio is consistent with the PXRD results, which further confirms that copper doping causes the MIL-53(Fe)-18H crystal to be oriented toward the (220) crystal plane, gradually transforming from a diamond-like shape to a rod-like structure. In addition, the crystallization nucleation rate of MOFs determines its morphology and particle size. Generally, a fast nucleation rate is likely to produce a large number of crystal nuclei, shortening the crystal growth process and causing the particles to become smaller; conversely, a slow nucleation rate is likely to produce large-sized particles. It can be seen that copper doping slows down the crystallization nucleation rate of MIL-53(Fe)-18H, but as the copper doping ratio increases to 0.50, the crystallization nucleation rate is accelerated.

[0073] ③Molecular structure

[0074] Furthermore, the organic linker and iron oxide cluster structure of the copper-doped MIL-53(Fe)-18H obtained in Examples 1 to 3 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were comprehensively studied by FT-IR spectroscopy. Figure 3 shown.

[0075] observe Figure 3 It can be seen that: Figure 3 In a, the FT-IR spectra of all catalysts are at 3400 cm -1 A broad peak appears near the wave number. This characteristic absorption peak is attributed to the characteristic vibration absorption peak of the -OH group, which is mainly caused by water molecules adsorbed or bound to the catalyst surface. In the spectrum, C=O also appears at 1300cm -1 -1700cm -1 The characteristic absorption band in the wavenumber range; at the same time, at 750cm -1 The bending vibration peaks attributable to CH on the benzene ring were monitored at the wavenumber. Figure 3 It can be observed in b that the relative concentration of undoped MIL-53(Fe)-18H at 552 cm-1 The characteristic absorption peak at 555 cm-1, which is attributed to the stretching vibration of the Fe-O bond, appears at 555 cm-1. -1 This is attributed to the partial substitution of Cu atoms for Fe atoms in the Fe-O-Fe structure to form a new Fe-O-Cu structure, which further proves the successful preparation of copper-doped MIL-53(Fe)-18H catalyst.

[0076] ④Aperture

[0077] The porous structures of the copper-doped MIL-53(Fe)-18H obtained in Examples 1 to 3 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were evaluated using the BET technique. The test conditions were: degassing temperature 100°C. The results are shown in Figure 2. Figure 4 And as shown in Table 1.

[0078] like Figure 4 As shown in a, the hysteresis loops in the nitrogen adsorption / desorption isotherms of the prepared catalysts are all type IV, indicating that they are all mesoporous structures. As shown in Table 1, the introduction of Cu atoms greatly increases the specific surface area of ​​MIL-53(Fe)-18H, among which the maximum value (242.75 m 2 g -1 ), when the copper doping ratio continues to increase, the specific surface area decreases and drops to a minimum of 56.51m 2 g -1 The pore volume of the catalyst material is closely related to the specific surface area. Therefore, the pore volume of MIL-53(Fe)-18H changes with the copper doping ratio in a manner consistent with its specific surface area, reaching a maximum value of 0.275 cm when the copper doping ratio is 0.20. 3 g -1 At the same time, from Figure 4 b It can be seen that the pore size of copper-doped MIL-53(Fe)-18H is mainly concentrated in the range of 2.0-4.0nm. Compared with the undoped MIL-53(Fe)-18H, the number of small pores has increased significantly, so the average pore size has decreased, and the minimum has dropped to 3.47nm. It can be seen that copper doping optimizes the pore structure of MIL-53(Fe)-18H, which is specifically manifested in reducing the pore size, increasing the specific surface area and pore volume, which is beneficial to the mass transfer of ozone and organic pollutants on the catalyst surface.

[0079] Table 1 Pore structure information of undoped and copper-doped MIL-53(Fe)-18H

[0080]

[0081] ⑤Element composition and chemical state

[0082] In order to analyze the effect of copper doping on the elemental composition and chemical state of the surface structure of MIL-53(Fe)-18H catalyst, the present application uses XPS technology to characterize the copper-doped MIL-53(Fe)-18H obtained in Examples 1 to 3 and the MIL-53(Fe)-18H obtained in Comparative Example 1. The results are shown in Figure 2. Figure 5 shown.

[0083] observe Figure 5 It can be seen that: Figure 5 a is the full XPS spectrum, where a new peak regarding the Cu element can be observed in copper-doped MIL-53(Fe)-18H, confirming the successful preparation of the copper-doped MIL-53(Fe)-18H catalyst. Figure 5 In b, the two characteristic peaks located near the binding energy of 933 eV and 953 eV correspond to the Cu 2p 3 / 2 and Cu 2p 1 / 2 region. Meanwhile, the other two signal peaks located near 941eV and 960eV belong to the characteristic satellite peaks of Cu(II), indicating that in the copper-doped MIL-53(Fe)-18H catalyst, the Cu element mainly exists in the +2 valence state. In addition, it was found from the high-resolution O1sXPS spectrum that as the copper doping ratio increased from 0 to 0.50, the characteristic absorption peak area ratio of Oads and Olatt gradually decreased, and their ratios were 5.56, 4.17, 1.30, and 1.20, respectively, indicating that copper doping leads to a decrease in the oxygen vacancy content in the MIL-53(Fe)-18H catalyst structure, and as the copper doping ratio increases, the degree of oxygen vacancy content attenuation becomes more obvious.

[0084] ⑥Lewis acid site density

[0085] The Py-FTIR technique was used to measure the MIL-53(Fe)-18H before and after doping. The results are as follows: Figure 6 And as shown in Table 2.

[0086] observe Figure 6 It can be seen that: located at 1040cm -1 and 1070cm -1 The two characteristic signal peaks near the wave number are respectively attributed to the ν12 and ν18a vibration forms formed by the coordination of the unsaturated coordination center of Fe or Cu with the pyridine molecule, indicating that the copper-doped MIL-53(Fe)-18H material has Lewis acid sites. According to the principle of Py-FTIR technology, low degassing temperature (50°C) corresponds to total acid (weak acid + medium acid + strong acid), medium degassing temperature (150°C) corresponds to medium acid + strong acid, and high degassing temperature (250°C) corresponds to strong acid. Figure 6It can be seen from ad that with the increase of degassing temperature, the intensity of all signal peaks gradually decays or even disappears, indicating that the strong acid type accounts for a small proportion on the catalyst surface. The Lewis acid site composition and density of the surface of MIL-53(Fe)-18H materials with different copper doping ratios were calculated based on the characteristic band area representing the ν18a vibration form in the Py-FTIR spectra at three degassing temperatures. The results are shown in Figure 6 e and Table 2. It can be found that when the copper doping ratio increases from 0 to 0.50, the total acid, medium acid and strong acid densities of MIL-53(Fe)-18H decrease accordingly, among which the total acid density increases from 2.08 mmol g -1 Reduced to 0.60 mmol g -1 , a decrease of 71.2%.

[0087] Table 2 Surface Lewis acid site density of undoped and copper-doped MIL-53(Fe)-18H

[0088]

[0089] ⑦ Oxygen vacancies

[0090] This application uses solid EPR technology to characterize MIL-53(Fe)-18H before and after copper doping. The test conditions are: microwave frequency 9.85GHz, power 12.72mW. The results are as follows Figure 7 shown.

[0091] observe Figure 7 It can be seen that: except for the MIL-53(FeCu3)-18H signal peak which is not obvious, the other catalysts all have signal peaks symmetrical with g=2.02 in the EPR spectrum, which are attributed to the oxygen vacancies of the metal oxygen cluster nodes, indicating that there are unsaturated coordinated metal centers in the structure of the undoped and copper-doped MIL-53(Fe)-18H catalysts. From the signal peak intensity, it can be seen that with the increase of the copper doping ratio, the signal peak intensity decays, indicating that both oxygen vacancies and unsaturated coordination centers decrease, which is consistent with the O1sXPS and Py-FTIR test results, thus confirming the positive correlation between oxygen vacancies in Fe-MOFs materials and the total acid density of Lewis acid sites on the surface.

[0092] 2. Catalytic ozone oxidation degradation experiment

[0093] The experimental conditions and procedures of this part are as follows:

[0094] Phenol, AQ-7, SMX, ATZ, and MDE were selected as the organic pollutant simulation objects to explore the ozone activation efficiency of the MIL-53 (FeCu)-18H series catalysts. The specific experimental process is as follows: 30 mg of powdered catalyst is evenly dispersed in 300 mL of 20 mg L -1phenol / AQ-7 / SMX / ATZ solution, and then a concentration of 100 mg L -1 , flow rate 60 mL min -1 The HCO process was started with ozone gas. 1 mL of sample was taken with a syringe at given time intervals and filtered with a 0.22 μm aqueous PES filter. 30 μL of 0.1 mol L -1 Na2S2O3 solution was added to quench the residual ozone molecules and ROS. All oxidative degradation experiments were carried out in a water bath at 25°C and 30 rpm.

[0095] The parameters in this section are determined as follows:

[0096] (1) Analysis of organic pollutant concentration

[0097] The absorbance of AO-7 solution sample was measured at λ = 485 nm using Lambda35 UV-visible spectrophotometer from PerkinElmer, USA. t The calculation of the reaction rate constant k is as follows:

[0098]

[0099] Where A0 is the absorbance of the initial sample solution, A t is the absorbance of the sample solution at time t.

[0100] The peak intensities of phenol, SMX, ATZ and MDE solution samples were detected by 1260 high performance liquid chromatograph from Agilent Technologies, USA. The stationary phase of the high performance liquid chromatography test was a ZORBAX Eclipse XDB-C18 column (3.5 mm, 4.6 × 150 mm), and other test conditions are shown in Table 3.

[0101] Table 3 HPLC test conditions

[0102]

[0103] Degradation rate of organic pollutants (1-C t / C0) is calculated as follows:

[0104]

[0105] Where B0 is the peak intensity corresponding to the initial sample solution, B t is the peak intensity corresponding to the sample solution at time t.

[0106] (2) ROS determination

[0107] In the free radical quenching experiment, DMPO (20 mM) was used as ·OH and O2 ·- Signal capture agent, in which water is used as solvent for the capture of OH, O2 ·- Methanol was used as the capture solvent; TEMP (20 mM) was used as 1 O2 signal capture agent, the solvent is water; FFA (5mM) as 1 O2 quencher, comparative quencher (2 g L -1 ) to the catalytic degradation system to identify the contribution of ROS to the degradation of organic pollutants; p-BQ (5 mM) as O2 ·- The EPR spectrum of ROS generated by ozone decomposition and transformation was tested using an A300 electron spin resonance spectrometer from Bruker, USA.

[0108] In the free radical probe method, coumarin (10 mM) was used as the ·OH probe to measure the cumulative concentration of ·OH in the system. 1 O2 probe, measuring system 1 O2 steady-state concentration, MDE and ozone, ·OH, 1 O2, O2 ·- The second-order reaction rate constants are k 1 O2,MDE=1.5×10 8 M -1 s -1 , k·OH,MDE=6×10 9 M -1 s -1 , kO3, MDE < 1M -1 s -1 , kO2 ·- ,MDE=0M - 1 s -1 It can be seen that in the catalytic ozone system, MDE is mainly 1 O2 and ·OH oxidative degradation, so 20mgL -1 The solvent composition was replaced by 50% water and 50% methanol to eliminate the reaction between OH and MDE, so that the concentration of MDE changed from 1 O2 dominated, and other reaction conditions were consistent with the catalytic ozone oxidation degradation experiment. 1 The steady-state concentration of O2 is determined by MDE and the relationship between ozone, OH, 1 O2, O2 ·- The second-order reaction rate constant is calculated by the following formula: 1 Take O2 as an example:

[0109] MDE+1 O1→Substrate (3)

[0110]

[0111] (3) Ozone concentration measurement

[0112] The indigo method was used to determine the ozone concentration in the solution. First, the concentration was set to 278.65 mg / L -1 Prepare a phosphate buffer solution with a pH of 2 using the standard stock solution of sodium indigo disulfonate: weigh 7.1 g of anhydrous disodium hydrogen phosphate and 6.8 g of potassium dihydrogen phosphate, dissolve in water, and dilute to 1 L. Then, add 2.00 mL of sodium indigo disulfonate solution, 5.00 mL of phosphate buffer, and 5.00 mL of solution sample to a 50 mL colorimetric tube, and then dilute to 50 mL with water. Finally, use a Lambda35 UV-visible spectrophotometer from PerkinElmer, USA, to measure the sample absorbance at λ=610 nm. The thickness of the cuvette is 1 cm. The mass concentration of ozone in the solution sample is calculated according to formula (7):

[0113]

[0114] Where: ρ is the mass concentration of ozone, g L -1 ; ε is the molar absorptivity of sodium indigo disulfonate, which is 0.193×10 4 Lmol -1 cm -1 ; b is the thickness of the cuvette, which is 1 cm; V 水样 is the volume of the water sample, mL; A0 is the absorbance of the blank sample; A1 is the absorbance of the sample; 48 is the molar mass of ozone, g mol -1 .

[0115] In order to analyze the consumption of ozone in the presence of catalyst, 50 mL of saturated ozone solution (the power of the ozone generator was controlled at 60% and the gas flow rate was 60 mL min -1 , water bath temperature is 25℃, keep continuous ventilation for more than 1h) add 5mg catalyst sample, place it in an intelligent constant temperature oscillator, control the temperature to 25℃, the speed is 50rpm, and take 5.00mL with a pipette at regular intervals, quickly add it to a 50mL colorimetric tube for absorbance determination. The ozone consumption rate in the solution is calculated according to formula (8):

[0116]

[0117] Where A is the ozone consumption rate; ρ0 is the initial sample ozone mass concentration, that is, the mass concentration of the ozone saturated solution, which is calculated to be 0.008 g L -1 ρt is the ozone mass concentration of the sampled solution at time t, g L -1 .

[0118] ① Exploration of degradation pathways

[0119] (1) Identify ROS types

[0120] Ozone catalytic tests were conducted on MIL-53(Fe)-18H before and after copper doping. The ozone system without adding catalyst was used as the control group, and the degradation liquid was collected for EPR test. No pollutants were added in this part, and water was used as the solvent for testing. The rest of the experimental conditions were referred to the above part of "2. Catalytic ozone oxidation degradation experiment".

[0121] The results are as follows Figure 8 As shown in the figure, it can be observed that in the EPR spectra of undoped and copper-doped MIL-53(Fe)-18H catalytic ozone, obvious ions belonging to DMPO / ·OH and DMPO / O2 ·- and TEMP / 1 The characteristic signal peak of O2 indicates that ·OH and O2 exist in the catalytic ozone system. ·- and 1 A careful comparison of the changes in the peak intensity of the ROS characteristic signal from 0 to 0.50 copper doping ratio revealed an interesting pattern: as the copper doping ratio increased, the peak intensity of the characteristic signal representing ·OH gradually weakened, accompanied by the peak intensity representing 1 The characteristic signal peak intensity of O2 gradually increased, which confirmed that copper doping induced MIL-53(Fe)-18H to selectively produce ROS from ozone, and the copper doping ratio was an important influencing factor. ·- The characteristic signal peak intensity reaches the highest when the copper doping ratio is 0.30, but suddenly weakens when the copper doping ratio continues to increase to 0.50. ·- Yes OH and 1 O2 is an intermediate product of the chain reaction, so its concentration is similar to OH and 1 The overall concentration of O2 is closely related to the reference OH and 1 The variation of O2 with the increase of copper doping ratio, O2 ·- The sudden decrease in the value of ·OH may be due to the fact that the attenuation of ·OH is stronger than that of 1 The increase in O2 leads to OH and 1 The overall concentration of O2 decreases.

[0122] (2) Quantification of ROS production concentration

[0123] Based on the discovery that the copper doping ratio can be controlled to adjust the efficiency of MIL-53(Fe)-18H in selectively producing ROS from ozone, in order to further refine the effect of copper doping ratio on the catalytic ozone decomposition to produce ·OH1 The modulation degree of O2, this application quantifies the ·OH and 1 O2 concentration.

[0124] Coumarin was used as a probe to quantify the cumulative concentration of ·OH in the system, and MDE was used as a probe to quantify the cumulative concentration of ·OH in the system. 1 The steady-state concentration of O2 is as follows: Fig. 9 shown.

[0125] observe Fig. 9 It can be seen that the characteristic fluorescence absorption peak at 450nm represents the heptahydroxycoumarin generated by the reaction of ·OH and coumarin, and its intensity can reflect the cumulative concentration of ·OH. It can be found that as the copper doping ratio increases, the intensity of the characteristic fluorescence peak at 30min of reaction becomes lower, indicating that the ability to catalyze ozone to selectively generate ·OH becomes weaker, which is consistent with the EPR test results. Fig. 9 b It can be seen that the cumulative concentration of ·OH produced by ozone decomposition of the four copper-doped catalysts increases steadily with the extension of catalytic time, and the cumulative concentration of ·OH produced by ozone decomposition of MIL-53(Fe)-18H with a copper doping ratio of 0 is always much higher than that of the other three. Fig. 9 c It can be seen that when the reaction time is 30 min, MIL-53(FeCu1)-18H, MIL-53(FeCu2)-18H, and MIL-53(FeCu3)-18H catalysts can activate ozone to accumulate and produce 23.12, 18.85, and 17.2 μmol L -1 The concentration of ·OH was higher than that of undoped MIL-53(Fe)-18H (47.42 μmol L -1 ) weakened by 51.2%, 60.2% and 63.7% respectively.

[0126] Fig. 9 d~ Fig. 9 e is the result of the degradation of MDE by ozone oxidation catalyzed by undoped and copper-doped MIL-53(Fe)-18H. As the copper doping ratio increases, the removal efficiency of MDE increases significantly, and the degradation rate at 5 min increases from about 30% to about 70%, and the k value increases from 0.070 min -1 Increased to 0.234min -1 , indicating that ozone activation produces 1 O2 increases with the increase of copper doping ratio, which is consistent with the EPR test results. According to the k value of HCO technology for degradation of MDE and the secondary reaction rate constant of MDE, ozone and ROS, the 1 The results of O2 steady-state concentration are as follows Fig. 9As shown in f, it can be found that MIL-53(FeCu1)-18H, MIL-53(FeCu2)-18H, and MIL-53(FeCu3)-18H catalysts can activate ozone to stably produce 1.38*10 -5 μM, 2.01*10 -5 μM, 2.60*10 -5 μM concentration 1 O2, compared with undoped MIL-53(Fe)-18H (7.78*10 -6 μM) were increased by 77.4%, 158.4% and 234.2% respectively.

[0127] In summary, copper doping can induce the selective conversion of ozone, and with the increase of copper doping ratio, the catalytic decomposition of ozone by MIL-53(Fe)-18H produces ·OH 1 The modulation degree of O2 increases, so the concentration of ROS components in the catalytic ozone system can be controlled by adjusting the copper doping ratio.

[0128] (3) Determine the dominant component of ROS

[0129] In order to explore the contribution of ROS to the degradation and removal of phenol in the process of ozone catalysis by copper-doped MIL-53(Fe)-18H, the contribution rate of different ROS was calculated using ROS quenching experiment.

[0130] like Fig.10 As shown in Table 4, TEMP is 1 FFA is an efficient O2 capture agent that can inhibit the degradation and removal efficiency of phenol in all four catalyst systems. 1 O2 quencher, but FFA and OH 1 O2 can react quickly, and the secondary reaction rate constants are 1.5×10 10 M -1 s -1 and 1.2×10 8 M -1 s -1 , both exceeding OH and 1 The secondary reaction rate of O2 and phenol is low, so FFA was selected as a quencher to compete with phenol for ·OH and 1 O2, to explore OH and 1 The contribution of O2 to the degradation and removal of phenol. When excessive FFA was added to the catalytic degradation system, the removal of phenol was significantly inhibited and the degradation rate was reduced to about 30%. ·- and 1O2 can react quickly, but compared with phenol, the secondary reaction rate constant of p-BQ with ·OH is lower, so it cannot effectively inhibit the reaction of phenol with ·OH. ·- It is a highly nucleophilic free radical that is difficult to attack and destroy the electron-rich structure of phenol (the secondary reaction rate constant is 5.8×10 2 M -1 s -1 ), so p-BQ mainly competes with phenol as a quencher 1 O2 (second-order reaction rate constant is 6.6×10 7 M -1 s -1 ).Depend on Fig.10 a- Fig.10 d It can be found that the addition of p-BQ can also inhibit the degradation rate of phenol to a great extent, and its inhibition degree is slightly higher than that of TEMP, which may be due to the fact that O2 ·- As OH and 1 O2 generates intermediate products of the chain reaction, and its quenching inhibits the OH and 1 Oxidation of phenol by O2.

[0131] Table 4 Secondary reaction rate constants of quenchers with ozone and ROS

[0132]

[0133] Fig.11 a shows the pseudo-first-order reaction rate constant k value of phenol degradation and removal before and after the addition of TEMP, FFA and p-BQ, and the contribution rate of ROS is calculated based on the k value. Fig.11 As shown in b, as the copper doping ratio increases from 0 to 0.30, 1 The contribution of O2 to phenol degradation increased from 58.0% to 79.6%, while the contribution of OH decreased from 29.0% to 13.4%. 1 The contribution rate of O2 did not continue to increase, but slightly decreased by 3%. The contribution rate of ·OH did not continue to decrease, and remained at the same level as when the doping ratio was 0.30. This is also the reason why the catalytic ozone degradation efficiency of MIL-53(FeCu3)-18H is lower than that of MIL-53(FeCu2)-18H.

[0134] The above results show that the contribution of ROS in the catalytic ozone oxidation degradation process is highly dependent on the copper doping ratio. The introduction of Cu atoms strengthens the 1 The non-radical process dominated by O2 indirectly indicates that copper doping induces the selective transformation of ozone, and the composition change of ROS generated by ozone decomposition is closely related to the copper doping ratio.

[0135] ②1 Selective degradation in O2-dominated systems

[0136] In “① Degradation Path Exploration”, it has been found that copper doping strengthens the catalytic ozone oxidation degradation process of MIL-53(Fe)-18H. 1 The leading role of O2, combined with 1 Based on the behavioral characteristics and mechanism of action of O2 on the degradation of organic pollutants, it is speculated that the copper-doped MIL-53(Fe)-18H / ozone system has selectivity for the oxidative degradation of organic pollutants. Therefore, this section takes MIL-53(Fe)-18H and MIL-53(FeCu1)-18H catalysts as examples to explore and compare the efficiency of the two in catalyzing ozone degradation of different types of organic pollutants.

[0137] This section adopts the easy-to-be-OH and 1 AO-7, SMX oxidized by O2, and OH-attacked ...AO-7 oxidized by O2 1 O2-destroyed ATZ was used as a substrate, and the results were as follows Fig.12 shown.

[0138] observe Fig.12 It can be seen that in the AO-7 and SMX degradation experiments, MIL-53(FeCu1)-18H showed better catalytic ozone degradation efficiency than MIL-53(Fe)-18H. The k values ​​of the former for the two organic pollutants were 1.164min and 2.377min, respectively. -1 and 0.489min -1 , which is more accurate than the latter (1.023min -1 and 0.334min -1 ) increased by 13.8% and 46.4% respectively. Taking AO-7 as an example, the N=N in its structure is easily absorbed by the electrophilic 1 O2 attack, resulting in rapid decolorization, therefore, with the MIL-53 (FeCu1) -18H / ozone system 1 As the amount of O2 increases, the degradation efficiency of AO-7 also increases. However, in the ATZ degradation experiment, it was found that undoped MIL-53(Fe)-18H had a higher degradation rate, and its k value was 19.1% higher than that of copper-doped MIL-53(Fe)-18H. This is because ATZ is relatively electron-deficient and its structure is difficult to be 1 Therefore, with the decrease of ·OH in the MIL-53(FeCu1)-18H / ozone system, the degradation efficiency of ATZ also decreases.

[0139] The above results show that the MIL-53(FeCu1)-18H ozone catalyst has selective oxidation degradation of organic pollutants, which further verifies that copper doping induces the selective conversion of ozone and enhances the decomposition of ozone to produce ·OH.1 The performance of O2 modulation is improved 1 The contribution rate of O2 in the oxidative degradation of electron-rich organic matter.

[0140] ③ Kinetics of catalytic ozone decomposition

[0141] Fig.13 Figure 2 shows the decomposition curves and pseudo-first-order kinetic fitting curves of ozone in different systems. It can be seen that under normal temperature and pressure conditions, the decomposition and consumption rate of ozone in water is slow, and only about 10% of ozone is decomposed within 4 minutes. In the presence of Fe-MOFs catalyst, the ozone decomposition rate is greatly increased, and most of the ozone in the aqueous solution is decomposed and consumed within 4 minutes.

[0142] As the copper doping ratio in the MIL-53(Fe)-18H catalyst increases, the decomposition rate of ozone decreases gradually, and the k value increases from 0.011s -1 Reduced to 0.006s when the doping ratio is 0.50 -1 This may be because copper doping enhances the selective generation of ozone. 1 The efficiency of O2, and as the copper doping ratio increases, ozone → 1 O2 selectivity also increases, and the system contains a large amount of 1 Due to its relatively long lifetime, O2 participates in the decolorization of the indicator reagent sodium indigo disulfonate, thus creating the illusion that ozone consumption slows down with the increase of copper doping ratio.

[0143] ④Lewis acid site and 1 Relevance of O2 generation

[0144] In order to further study the intrinsic relationship between copper doping ratio and ozone selective conversion and explore the role of Lewis acid sites on the surface of MIL-53(Fe)-18H catalyst, this section analyzes the relationship between surface Lewis acid site density and copper doping ratio as well as ·OH, 1 Correlation of O2 concentration.

[0145] Fig.14 In a, a scatter plot was made with the copper doping ratio as the horizontal axis and the total acid density of the Lewis acid sites on the surface as the vertical axis, and a linear fit was performed. The results showed that the copper doping ratio and the total acid density of the Lewis acid sites on the surface had a good linear relationship. Adj.R 2 is 0.87, indicating that Fe-MOFs with different surface Lewis acid densities can be constructed by adjusting the copper doping ratio.

[0146] In order to confirm the key role of surface Lewis acid sites in the selective conversion of ozone and further reveal the structure-activity relationship between catalysts and the selective conversion of ozone, the total acid density of surface Lewis acid sites was used as the horizontal coordinate, and the ·OH and 1The EPR intensity and production concentration of O2 are plotted as ordinates and linear fitting is performed. The results are as follows: Fig.14 be shown. Fig.14 It can be seen from bc that the total acid density of Lewis acid sites on the surface of MIL-53(Fe)-18H catalyst shows an excellent positive linear correlation with the EPR intensity and cumulative concentration of OH. 2 are 0.97 and 0.94, respectively. Combined with the correlation between the copper doping ratio and the total acid density of Lewis acid sites on the surface, it is shown that the total acid density of Lewis acid sites on the surface can be increased by reducing the copper doping ratio, mediating the selective conversion of ozone and enhancing the efficiency of ozone decomposition to produce ·OH. Fig.14 d- Fig.14 e shows that the total acid density of Lewis acid sites on the surface is 1 The EPR intensity and steady-state concentration of O2 showed a good negative linear relationship. 2 The surface Lewis acid sites are 0.77 and 0.86, respectively, which further verifies the regulatory role of the surface Lewis acid sites as the key structure in the selective conversion of ozone and reveals the rule that the copper doping ratio precisely regulates the surface Lewis acid sites to mediate the selective conversion of ozone, that is, high surface Lewis acid site total acid density mediates the selective conversion of ozone into ·OH, and low surface Lewis acid site total acid density mediates the selective conversion of ozone into 1 O2.

[0147] The precise regulation of the total acid density of Lewis acid sites on the surface by the copper doping ratio is mainly achieved by increasing the electron density of metal active centers, strengthening the binding force of metal-oxygen coordination bonds, reducing empty metal coordination orbitals (i.e., reducing oxygen vacancies), and weakening the ability to accept lone pairs of electrons. That is, the copper doping ratio determines the electron density of metal active centers, thereby regulating the total acid density of Lewis acid sites on the surface, and ultimately mediating the selective conversion of ozone.

[0148] 3. Performance of MIL-53(FeCu2)-18H catalytic ozone deep treatment of printing and dyeing wastewater for reuse

[0149] The experimental conditions and procedures of this part are as follows:

[0150] (1) The target degradation object is the printing and dyeing wastewater of Zhejiang Daneng Printing and Dyeing Co., Ltd., and the ozone activation efficiency of the MIL-53 (FeCu)-18H series catalyst is explored. The specific experimental process is: 30 mg of powdered catalyst is evenly dispersed in 300 mL of printing and dyeing wastewater, and then a concentration of 100 mg L -1 , flow rate 60 mL min -1The HCO process was started by ozone gas. After 30 min of reaction, 10 mL of the sample was taken and filtered with a 0.22 μm aqueous PES filter. 30 μL of 0.1 mol L -1 Na2S2O3 solution was added to quench the residual ozone molecules and ROS. All oxidative degradation experiments were carried out in a water bath at 25°C and 30 rpm.

[0151] (2) The purified water from the printing and dyeing wastewater of Zhejiang Daneng Printing and Dyeing Co., Ltd. after deep treatment with HCO technology for 60 minutes was used for dyeing and compared with the fabric samples dyed with tap water. The knitted cotton fabrics and reactive dyes used were provided by Zhejiang Daneng Printing and Dyeing Co., Ltd. according to the company's main processing categories.

[0152] The Shanghai Qianli adjustable proofing machine is used for dyeing. The knitted cotton fabric is cut into 5cm×20cm size and weighs 2.25g. The reactive dyes are selected in three basic colors: red, yellow and blue. The specific dyeing process is as follows: Fig.15 As shown:

[0153] The dyeing prescription is shown in Table 5:

[0154] Table 5 Reactive dyes for cotton dyeing

[0155]

[0156] Soaping prescription: soap flakes 2g L -1 , bath ratio 1:20, temperature 98℃, time 10min.

[0157] The parameters in this section are determined as follows:

[0158] The absorbance of the reactive dye red K-3BE, yellow K-3RE, and blue K-BF dye solution samples was measured at λ=542nm, λ=422nm, and λ=612nm using a Lambda35 UV-visible spectrophotometer from PerkinElmer, USA. The dye uptake (1-C1 / C0) was calculated according to the following formula:

[0159]

[0160] Where C0 is the initial dye solution concentration; C1 is the dye solution concentration after dyeing; A0 is the absorbance of the initial dye solution; A1 is the absorbance of the dye solution after dyeing.

[0161] ①Efficiency of deep treatment of printing and dyeing wastewater

[0162] The EEM spectral technique was used to analyze the composition and composition of organic matter in printing and dyeing wastewater, as well as the residual pollutants after treatment. The efficiency of MIL-53 (FeCu2) -18H catalytic ozone treatment of printing and dyeing wastewater was preliminarily evaluated. The results are as follows: Fig.16 shown.

[0163] observe Fig.16 It can be seen that according to the characteristic regions of aromatic proteins, fumaric acid-like compounds, soluble microbial byproducts and humic acid-like organic matter in the EEM spectrum: Region I (λ ex / λ em =(200-250nm) / (280-380nm)) represents aromatic proteins; II region (λ ex / λ em =(200-250nm) / (380-550nm)) represents fumaric acid-like compounds; Region III (λ ex / λ em =(>250nm) / (<380nm)) represents soluble microbial byproducts; Zone IV (λ ex / λ em =(>280nm) / (>380nm)) represents humic acid-like organic matter. It was found that the printing and dyeing wastewater of Zhejiang Daneng Printing and Dyeing Co., Ltd. contained high concentrations of soluble microbial byproducts, medium concentrations of aromatic proteins and humic acid-like organic matter, and a small amount of fumaric acid-like compounds. After 30 minutes of deep treatment, the corresponding EEM spectrum ( Fig.16 b) It can be observed that the fluorescence intensity of the four characteristic areas is not monitored because the organic pollutant molecules are oxidized and degraded into smaller molecules, indicating that the MIL-53 (FeCu2) -18H catalytic ozone oxidation technology has excellent treatment efficiency for printing and dyeing wastewater. Comparison of the color of printing and dyeing wastewater before and after treatment ( Fig.16 c), changed from purple-black before treatment to clear and transparent, further confirming that the HCO technology based on MIL-53(FeCu2)-18H catalyst has great application potential in printing and dyeing wastewater.

[0164] ② Dyeing performance of printing and dyeing wastewater after deep treatment

[0165] In order to evaluate the dyeing performance of the recycled water after deep treatment of printing and dyeing wastewater from Zhejiang Daneng Printing and Dyeing Co., Ltd. using MIL-53 (FeCu2) -18H catalytic ozone oxidation technology.

[0166] (1) Dye absorbance curve

[0167] The full spectrum test mode of UV-visible spectrophotometer was used to obtain the absorbance curves of three active dyes, Jingren Red K-3BE, Jingren Yellow K-3RE, and Jingren Blue K-BF, at a concentration of 0.1%, and the effect of the recycled water after deep treatment on the dye absorption properties was analyzed. The results are as follows Fig.17 shown.

[0168] observe Fig.17 It can be seen that the red, yellow and blue dyes have maximum absorption peaks at 423nm, 542nm and 613nm respectively, and the maximum absorption peak of the dye solution prepared with recycled water after deep treatment as solvent is consistent with that prepared with tap water, and the peak shape is almost the same, indicating that recycled water has no obvious effect on the absorption properties of the prepared dye solution.

[0169] (2) Dye uptake rate

[0170] The dye uptake of three dyes on knitted cotton fabrics was calculated respectively, and the dyeing difference between tap water and recycled water was compared. From Table 6, it can be found that the dye uptake of recycled water dyeing is slightly lower than that of tap water dyeing. Among them, the dye uptake of 0.1% and 2.0% red and yellow dyes with recycled water is significantly different from that with tap water, while the difference of dark color (5.0% concentration) is very small; at the same time, the difference of blue dye uptake of light, medium and dark colors with recycled water and tap water is also small, which is controlled within 5.0%. This shows that considering the dye uptake alone, recycled water dyeing may be more suitable for dyeing dark colors and blue.

[0171] Table 6 Dyeing rate and rubbing color fastness of tap water and recycled water

[0172]

[0173]

[0174] (3) Dyeing fabric shade

[0175] The color characteristic values ​​of dyed fabrics were tested by a colorimeter, including L, a, b, c, DE and K / S values ​​of the CIE mode, which respectively represent lightness, red-green value, yellow-blue value, chroma value, color difference and color depth. The test conditions were reflectance mode, aperture: 11 mm, and the average value was taken after 3 tests. The results are listed in Table 7. At the same time, the reflectance curve was drawn according to the reflectance R value measured for each dyed fabric. The results are shown in Table 7. Fig.18 As shown in Table 7, it can be found that similar to the dye uptake, the color difference between the light and medium colors of red and yellow dyes in recycled water and tap water dyeing is large, especially red. However, the color difference between the dark colors of red and yellow and the light, medium and dark colors of blue and tap water dyeing is small, and the CIE color difference value is basically controlled below 1. From the dyeing K / S value, a similar pattern is observed. Fig.18It can be found that the reflectance curves of fabrics dyed with 5.0% concentration of red and yellow dyes and light, medium and dark concentrations of blue dyes using recycled water and tap water are very close and almost overlap, indicating that the color tones of the corresponding dyed fabrics are similar.

[0176] The above results show that the printing and dyeing wastewater deeply treated by MIL-53 (FeCu2) -18H catalytic ozone oxidation technology is more suitable for blue and dark colors when reused in the process of dyeing knitted cotton fabrics with reactive dyes.

[0177] Table 7 Color characteristic values ​​of tap water and recycled water

[0178]

[0179] (4) Color fastness to rubbing

[0180] The Y571 dyeing friction color fastness tester produced by Laizhou Yuanmao Instrument Co., Ltd. was used to measure the dry friction color fastness of dyed knitted cotton fabrics in accordance with the national standard GB / T3920-2008 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing".

[0181] The results of the dry rubbing color fastness of the dyed fabrics are shown in Table 6. Observing the dry rubbing color fastness in Table 6, it can be seen that the dry rubbing color fastness of the recycled water-dyed fabric and the tap water-dyed fabric is not much different, both of which are 4-5 or above, indicating that the reuse of printing and dyeing wastewater after deep treatment by MIL-53 (FeCu2) -18H catalytic ozone oxidation technology in the process of reactive dyeing knitted cotton has little effect on the dry rubbing color fastness of the fabric.

[0182] The above research results on the dyeing performance of recycled water and tap water show that water quality has a certain influence on dyeing performance. The HCO technology based on MIL-53 (FeCu2) -18H catalyst is applied to the deep treatment of printing and dyeing wastewater. The treated water is reused in the process of dyeing knitted cotton with reactive dyes, and the dyeing performance of different dye colors and depths is different. Among them, the treated printing and dyeing wastewater reused in the process of dyeing knitted cotton with reactive dyes is more suitable for blue and dark colors.

[0183] ③ Stability and adaptability of catalyst

[0184] Fig.19 The degradation of MIL-53(FeCu2)-18H catalyst in different inorganic salt / HA systems. Fig.15 It can be seen that the degradation efficiency of MIL-53(FeCu2)-18H / ozone system on phenol under the coexistence of different concentrations of inorganic salt anions or HA. Considering the high salt content of printing and dyeing wastewater, the maximum addition of 50mM (about 3-7g L -1) concentration of inorganic salts to simulate the salt content of printing and dyeing wastewater in real conditions (taking the printing and dyeing wastewater from Zhejiang Daneng Printing and Dyeing Co., Ltd. as an example: the conductivity is 7.79mS cm -1 , converted into a total dissolved solid content of about 3-7g L -1 The above results show that the MIL-53 (FeCu2) -18H ozone catalyst has excellent resistance to inorganic salt anions and HA and other common water matrices in printing and dyeing wastewater, which means that the removal of target organic pollutants by MIL-53 (FeCu2) -18H catalytic ozone oxidation technology in actual printing and dyeing wastewater deep treatment will hardly be affected by the competition of complex water matrices.

[0185] Fig. 20 This is a characterization diagram before and after use. Fig. 20 a is the FT-TR spectrum, Fig. 20 b is the PXRD pattern. Fig. 20 It can be seen that the FT-TR spectrum and PXRD spectrum before and after use have obvious changes, indicating that the MIL-53 (FeCu2) -18H ozone catalyst has good structural stability, indicating that the MIL-53 (FeCu2) -18H catalytic ozone oxidation technology has good application potential in practical applications.

Claims

1. A method for preparing a copper-doped iron-based MOF catalyst, characterized in that: The copper-doped iron-based MOF catalyst is obtained by solvent thermal reaction of N,N-dimethylformamide containing copper salt, iron salt and terephthalic acid and then drying; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.

2. The preparation method according to claim 1, characterized in that The molar ratio of copper to iron in the copper salt and the iron salt is 1:(1-4).

3. The preparation method according to claim 1 or 2, characterized in that: The iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.

4. The preparation method according to claim 1 or 2, characterized in that: The copper salt is selected from any one of copper nitrate, copper sulfate and copper chloride.

5. The preparation method according to claim 1 or 2, characterized in that: The ratio between the total molar amount of copper and iron in the copper salt and the iron salt and the molar amount of terephthalic acid is 1:

1.

6. The preparation method according to claim 1, characterized in that: The drying temperature is 80 to 120° C., and the drying time is 12 to 36 hours.

7. The copper-doped iron-based MOF catalyst prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the copper-doped iron-based MOF catalyst as claimed in claim 7 in the ozone catalytic oxidation degradation of electron-rich organic pollutants.

9. Use of the copper-doped iron-based MOF catalyst as claimed in claim 7 in the treatment of printing and dyeing wastewater.

10. The use according to claim 9, characterized in that The treated printing and dyeing wastewater can be used for dyeing.

Citation Information

Patent Citations

  • Ce-doped Fe-MOF ozone catalyst, and preparation and application thereof

    CN111715294A

  • Palladium-copper catalyst as well as preparation method and application thereof

    CN113231076A

  • Preparation method of iron-based metal organic framework material photocatalyst

    CN116212953A

  • Preparation method and application of atom encapsulated MOFs (Metal-Organic Frameworks) derived nano polyhedral catalyst

    CN118320849A