Composite material frame coating method

Through high-voltage electric field electrostatic spraying technology and suspension methods, the problems of low coating utilization and low production efficiency in composite photovoltaic frame coating are solved, and the efficient and uniform coating film formation and the effect of reducing baking deformation is achieved.

CN118904671APending Publication Date: 2024-11-08JIANGSU ZHAOJUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411094544.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing composite photovoltaic frame coating technology, the coating utilization rate of the reciprocating machine spraying method is low, the efficiency is low, and the product is prone to deformation when baking.

Method used

High-voltage electric field electrostatic spraying technology is adopted, first spray antistatic agent and surface drying treatment, and then spray the paint under the high-voltage electric field, combined with suspension method to improve the utilization rate and production efficiency of the paint and reduce the deformation risk during baking.

Benefits of technology

Improve the utilization rate and production efficiency of the paint, reduce the deformation risk during baking, and the product quality after spraying is improved, the utilization rate of the paint is increased to more than 75%, the production beat is shortened to 2 seconds-2.5 seconds/root, baking The deformation is less than 1mm/m.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904671A_ABST
    Figure CN118904671A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material frame coating method. The composite material frame coating method comprises the following steps that an antistatic agent is sprayed on the surface of a composite material frame; the composite material frame sprayed with the antistatic agent is subjected to surface drying; and the composite material frame subjected to surface drying treatment is subjected to high-voltage electric field electrostatic spraying coating. The utilization rate of the coating is increased, and the production efficiency and the quality of a sprayed product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of photovoltaic technology, and in particular relates to a composite material frame coating method. Background Art

[0002] At present, the composite photovoltaic frame coating adopts the reciprocating spraying process, which includes the following steps: loading, dust removal, reciprocating spraying of surface A, leveling, reciprocating spraying of surface A, flipping, reciprocating spraying of surface B, leveling, baking and unloading. Problems and shortcomings of the existing technology: (1) The reciprocating spraying method has low coating utilization rate. The efficiency of low-pressure air gun spraying is only 30% to 40%, and the efficiency of medium-pressure mixed air gun spraying is 50% to 60%; (2) The reciprocating spraying method has low efficiency. Generally, based on the workpiece length of 2.4 meters, its efficiency is 8 seconds / piece to 15 seconds / piece; (3) The product is easy to deform during baking. After spraying, the product is easy to deform when it is laid flat and baked at 80°C. Summary of the invention

[0003] Purpose of the invention: In order to solve the problems of the prior art, the present application provides a composite material frame coating method, which improves the utilization rate of the coating and improves the production efficiency and the quality of the product after spraying.

[0004] Technical solution: The embodiment of the present application provides a composite material frame coating method, comprising the following steps:

[0005] The composite material frame surface is sprayed with antistatic agent; the composite material frame sprayed with the antistatic agent is surface dried; the composite material frame after surface drying is electrostatically sprayed with paint using a high-voltage electric field.

[0006] In some embodiments, the antistatic agent comprises a quaternary ammonium salt.

[0007] In some embodiments, the antistatic agent is sprayed with a thickness of 5 μm to 10 μm.

[0008] In some embodiments, the composite frame is painted by hanging.

[0009] In some embodiments, the composite material frame is sprayed using a spraying device.

[0010] In some embodiments, the composite frame is hung at a spacing of 10 cm to 25 cm.

[0011] In some embodiments, the surface drying temperature is 18° C. to 28° C., the surface drying humidity is 40% RH to 60% RH, and the surface drying time is 5 min to 10 min.

[0012] In some embodiments, the parameters of the high-voltage electric field electrostatic spraying are: voltage of 30 kV to 100 kV, and a coating discharge volume of 0 to 500 cc / min.

[0013] In some embodiments, the composite material frame surface is also preheated before antistatic spraying.

[0014] In some embodiments, the temperature of the preheating treatment is 60° C. to 80° C., and the time of the preheating treatment is 5 min to 15 min.

[0015] In some embodiments, after the composite material frame is preheated, it is also dusted.

[0016] In some embodiments, the dust removal process is to use an ion wind bar to remove dust on the surface of the composite material frame.

[0017] In some embodiments, the parameters of the dust removal process are: static electricity removal time 2 seconds to 5 seconds, ion balance -13V to +13V.

[0018] In some embodiments, the composite material frame is electrostatically sprayed with paint using a high voltage electric field and then subjected to a leveling treatment.

[0019] In some embodiments, the leveling parameters are: temperature of 18° C. to 28° C., humidity of 30% RH to 70% RH, and time of 10 min to 20 min.

[0020] Beneficial effect: The present application provides a composite material frame coating method, comprising the following steps: spraying an antistatic agent on the surface of the composite material frame; performing surface drying on the composite material frame sprayed with the antistatic agent; and applying coating to the composite material frame after surface drying using a high-voltage electric field electrostatic spraying. The present application improves the utilization rate of the coating, and improves the production efficiency and the quality of the product after spraying. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of the structure of a composite material frame spraying device in an embodiment of the present application;

[0022] Figure 2 This is a schematic diagram of the structure of the hanger and the composite material frame in the embodiment of the present application;

[0023] Figure 3 for Figure 2 A schematic diagram of the enlarged structure of the middle part A;

[0024] Figure 4 This is a schematic diagram of the structure of the first connecting member in the embodiment of the present application;

[0025] Figure 5This is a cross-sectional schematic diagram of a composite material frame structure in an embodiment of the present application;

[0026] Figure 6 This is a schematic diagram of the connection structure of adjacent composite material frames in an embodiment of the present application;

[0027] Figure 7 for Figure 6 The enlarged structural diagram of the middle B part;

[0028] Figure 8 This is a schematic diagram of the third hanger structure in the embodiment of the present application. DETAILED DESCRIPTION

[0029] The embodiment of the present application provides a composite material frame coating method, comprising the following steps: spraying an antistatic agent on the surface of the composite material frame; performing surface drying on the composite material frame sprayed with the antistatic agent; and applying a coating to the composite material frame after surface drying using a high-voltage electric field electrostatic spraying. The composite material frame of the present application is usually a polyurethane composite material, which is not conductive, and is prone to generating static charges during the grinding process that cannot be completely eliminated. When electrostatic spraying is performed using a high-voltage electric field, a coating repulsion phenomenon will occur. The present application sprays an antistatic agent on the surface of the composite material frame, which can rapidly dissipate the static charges without aggregation, and can generate electrical neutralization, thereby making it easier for negatively charged coating particles to adhere to the workpiece surface of the composite material frame. Furthermore, the high-voltage electrostatic field of the present application carries a high-voltage negative charge, which is evenly dispersed and directionally adsorbed under the action of the electric field, thereby forming a uniform and firm coating layer on the surface of the workpiece. In some embodiments, the spraying efficiency of the present application can reach 2 seconds / root to 2.5 seconds / root based on a workpiece length of 2.4 meters, and the method of the present application improves production efficiency.

[0030] In some embodiments, the antistatic agent comprises a quaternary ammonium salt.

[0031] In some embodiments, the quaternary ammonium salt includes 3,3'-(9-octadeceneimino)bis[2-hydroxy-N,N,Ntrimethyl]-1-propylammonium.

[0032] In some embodiments, the spray thickness of the antistatic agent is 5 μm to 10 μm. In some embodiments, the spray thickness of the antistatic agent is any value of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or a range consisting of any two values. The spray thickness of the antistatic agent of the present application is within this range, which can make the static charge dissipate quickly without accumulation.

[0033] In some embodiments, the mass percentage concentration of the antistatic agent is 0.1% to 10%. In some embodiments, the mass percentage concentration of the antistatic agent is 0.1% to 10%. For example, the mass percentage concentration of the antistatic agent is any value of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two values. The antistatic agent of the present application achieves a balance between production efficiency and product quality within this concentration range. Too high a concentration of the antistatic agent affects the adhesion of the coating film; too low a concentration of the antistatic agent affects the electrostatic spraying effect.

[0034] In some embodiments, the antistatic agent is 3,3′-(9-octadeceneimino)bis[2-hydroxy-N,N,Ntrimethyl]-1-propylammonium.

[0035] In some embodiments, the antistatic agent is present in the form of a stock solution, and the antistatic agent stock solution refers to an isopropanol solution of 3,3'-(9-octadecene imino)bis[2-hydroxy-N,N,N trimethyl]-1-propylammonium. In some embodiments, in the antistatic agent stock solution, the mass concentration of 3,3'-(9-octadecene imino)bis[2-hydroxy-N,N,N trimethyl]-1-propylammonium is 30% to 40%.

[0036] In some embodiments, the mass percentage concentration of the antistatic agent refers to the mass percentage concentration of 3,3'-(9-octadeceneimino)bis[2-hydroxy-N,N,Ntrimethyl]-1-propylammonium in the solution after the stock solution of the antistatic agent is diluted with deionized water.

[0037] In some embodiments, the composite frame of the present application is painted by hanging. In some embodiments, the spacing of the composite frame hanging is 10cm to 25cm. The hanging distance can be adjusted according to production needs. Figure 1 As shown, the present application sprays composite material frames by hanging, which can reduce the hanging spacing between workpieces, reduce production cycle, and improve production efficiency. The hanging method is compatible with composite material frames of different specifications. For example, during the production process, by adding connecting devices at both ends of the composite material frame material, long and short sides can be continuously produced without switching. In addition, the present application adopts a hanging method for material spraying, which can reduce the risk of deformation during baking in the subsequent processing process, avoid the stress baking at both ends of the composite material frame, and reduce the occurrence of deformation.

[0038] In some embodiments, the surface drying temperature is 18°C ​​to 28°C, the surface drying humidity is 40%RH to 60%RH, and the surface drying time is 5min to 10min. The present application can volatilize most of the water in the antistatic agent by controlling the surface drying parameters, and then carry out the subsequent spraying treatment. The present application can solve the problem of blisters or water stains on the coating film caused by untimely volatilization of the antistatic agent by adding a surface drying step between spraying the antistatic agent and electrostatic spraying. The present application controls the surface drying parameters to avoid volatilization too quickly, which may affect the spraying effect, such as the defect of low paint coverage rate.

[0039] In some embodiments, the parameters of high-voltage electric field electrostatic spraying are: voltage is 30kV~100kV, and the coating discharge amount is 0~500cc / min. In some embodiments, the voltage of high-voltage electric field electrostatic spraying is any value or any range of two values ​​in 30kV, 40kV, 50kV, 60kV, 70kV, 80kV, 90kV, 100kV. In some embodiments, the coating discharge amount is any value or any range of two values ​​in 100cc / min, 200cc / min, 300cc / min, 400cc / min, 500cc / min. In some specific embodiments, the high-voltage electric field electrostatic spraying of the present application is DISK electrostatic spraying, specifically using the effect of 30kV~100kV high-voltage electrostatic field, through the high-speed rotation of the rotating disc, the coating particles are dispersed by centrifugal force and carry high-voltage negative electricity, and are evenly dispersed and directional adsorbed under the action of the electric field, so as to form a uniform and firm coating layer on the surface of the workpiece. In some embodiments, before spraying the antistatic agent on the surface of the composite material frame, a preheat treatment is also performed. In some embodiments, the temperature of the preheat treatment is 60°C to 80°C, such as the temperature of the preheat treatment is any value among 60°C, 70°C, and 80°C, or a range consisting of any two values. In some embodiments, the time of the preheat treatment is 5min to 15min, such as the time of the preheat treatment is any value among 5min, 10min, and 15min, or a range consisting of any two values. The present application increases the surface temperature of the workpiece through preheat treatment, especially when the surface temperature of the workpiece is low, which can solve the problem of slow volatilization of the antistatic agent and affecting the spraying effect.

[0040] In some embodiments, after the composite material frame is preheated, a dust removal process is also performed. In some embodiments, the dust removal process is to use an ion wind bar to remove dust on the surface of the composite material frame. In some embodiments, the parameters of the dust removal process are: static electricity removal time 2s to 5s, ion balance degree -13V to +13V. The dust removal step of the present application can increase the spraying quality of the coating.

[0041] In some embodiments, the composite material frame is subjected to leveling treatment after being electrostatically sprayed with paint in a high voltage electric field. In some embodiments, the leveling parameters are: temperature of 18° C. to 28° C., humidity of 30% RH to 70% RH, and time of 10 min to 20 min.

[0042] In some specific embodiments, the composite material frame coating method of the present application includes the following steps:

[0043] (1) Loading: The product is transferred to the loading area through the auxiliary loading device and is suspended in the spray chamber after the elastic plug is installed;

[0044] (2) Preheating: The workpiece surface temperature is raised to 20°C ± 5°C by electric (or natural gas) heating (heating temperature 60°C ~ 80°C, time 5min ~ 15min);

[0045] (3) Dust removal: Use an ion wind bar to remove dust from the surface of the workpiece. The static electricity removal time is 2s to 5s, and the ion balance is + / -13V);

[0046] (4) Spraying conductive liquid (antistatic agent): dilute the antistatic agent stock solution with deionized water, and use the upper and lower reciprocating air spray guns to evenly spray the mixed conductive liquid (antistatic agent) onto the workpiece surface, with a spraying thickness of 5 μm to 10 μm;

[0047] (5) Surface drying: After spraying the conductive liquid (antistatic agent), the surface drying temperature of the product is 18°C ​​to 28°C, the surface drying humidity is 40% RH to 60% RH, and the surface drying time is 5min to 10min. The moisture on the surface of the product evaporates and leaves a conductive layer.

[0048] (6) DISK electrostatic spraying: The voltage is 30kV~100kV, and the paint discharge volume is 0~500cc / min for paint spraying. By utilizing the effect of high-voltage electrostatic field, the disc rotates at high speed to disperse the paint particles through centrifugal force and carry high-voltage negative charge. Under the action of the electric field, the paint particles are evenly dispersed and directionally adsorbed, thereby forming a uniform and firm coating layer on the surface of the workpiece;

[0049] (7) Re-spraying: Use the upper and lower reciprocating spray guns with tracking to re-spray some areas;

[0050] (8) Leveling: The sprayed product is leveled and surface dried under the conditions of temperature 18℃~28℃, humidity 30%RH~70%RH, and time 10min~20min;

[0051] (9) Baking: Baking is performed according to the TDS (technical parameter) requirements of the coating;

[0052] (10) Unloading: After the product is baked, the elastic insert is removed and after passing the inspection, it is transferred to the next process.

[0053] In other embodiments, when the ambient temperature is high, such as when the ambient temperature exceeds 20° C., preheating may not be used.

[0054] In other embodiments, the baking temperature in step (9) is 80° C. and the baking time is 60 min.

[0055] like Figure 1 and Figure 2 As shown, the spraying device of the present application is a DISK electrostatic spraying device. DISK electrostatic spraying utilizes the effect of a high-voltage (30kV-100kV) electrostatic field. The high-speed rotation of the rotating disc disperses the paint (paint discharge volume: 0-500cc / min) particles through centrifugal force and carries a high-voltage negative charge. Under the action of the electric field, the paint is evenly dispersed and directionally adsorbed (2 seconds-2.5 seconds / root, workpiece length 2.4 meters), thereby forming a uniform and firm coating layer on the surface of the workpiece. In order to realize the spraying of the composite material frame by the DISK electrostatic spraying device, the present application provides the following composite material frame spraying device, the spraying structure body of the spraying device is a DISK electrostatic spraying device, the spraying device has a spraying chamber 110, and the spraying device has a first direction X and a second direction Y. In some embodiments, the first direction X is vertically arranged or approximately vertically arranged with the second direction Y. The spraying device includes a track 101 extending along the first direction X, and the track 101 is driven by a motor and can move along the first direction X. The track 101 is connected to at least one first hanger 102. In some specific embodiments, the track 101 is connected to a plurality of first hangers 102, and the plurality of first hangers 102 are spaced apart along the first direction X. The lower end of the first hanger 102 is connected to the second hanger 103, and the second hanger 103 extends along the second direction Y. The second hanger 103 is detachably connected to the first hanger 102. The present application provides a suspension mechanism in the spraying chamber 110 of the spraying device for suspending the composite material frame, thereby achieving material spraying on the composite material frame through the DISK electrostatic spraying device, thereby improving production efficiency.

[0056] In some embodiments, the composite frame 200 is connected to the second hanger 103, the end of the second hanger 103 is provided with a first connector 104, the composite frame 200 has a cavity 210, and the first connector 104 is inserted into the cavity 210 of the composite frame 200, thereby achieving the connection between the second hanger 103 and the composite frame 200. In some specific applications, the second hanger 103 is made of iron wire with a diameter of 3 to 5 mm.

[0057] In some embodiments, the first connector 104 includes a guide end 1041 , and a width W1 of the guide end 1041 is smaller than a width W2 of the cavity 210 . The guide end 1041 facilitates the insertion of the first connector 104 into the cavity of the composite frame 200 , thereby improving production efficiency.

[0058] In some embodiments, the first connecting member 104 further includes a first connecting end 1042 and a second connecting end 1043, the first connecting end 1042 and the second connecting end 1043 are arranged opposite to each other, and the first connecting end 1042 and the second connecting end 1043 are respectively in contact with the inner surface of the cavity 210. The first connecting end 1042 is connected to the first hanger 102 through a first connecting rod 1044. The present application uses the first connecting end 1042 and the second connecting end 1043 arranged opposite to each other, and the two connecting ends are connected by an inclined connecting member in the middle, which can not only realize the connection of the composite material frame, but also reduce the connection area, reduce the friction of the insertion of the first connecting member 104, increase the difficulty of operation, and improve production efficiency.

[0059] like Figure 3 and Figure 4 As shown, in some specific embodiments, a first transition zone 1045 is provided between the first connection end 1042 and the first connection end 1042, the first transition zone 1045 connects the first connection rod 1044 and the first connection end 1042, and the first transition zone 1045 extends obliquely from the bottom end of the first connection rod 1044 to the top end of the first connection end 1042. A second transition zone 1046 is provided between the second connection end 1043 and the guide end 1041, the second transition zone 1046 connects the second connection end 1043 and the guide end 1041, and the second transition zone 1046 extends obliquely from the top end of the guide end 1041 to the bottom end of the second connection end 1043. The two transition zones realize the connection between the first connecting end face 1042 and the second connecting end face 1043 of the first connecting member 104 in the embodiment of the present application, which can reduce the contact area between it and the inner surface of the composite material frame. In addition, the guide end 1041 of the present application is an arc-shaped structure, which can reduce the stress concentration at the bottom end of the first connecting member 104 and improve the stability of the structure.

[0060] As described above, the composite frame spraying device of the present application sprays the composite frame by hanging, which can reduce the hanging distance between workpieces, reduce the production cycle, and improve production efficiency. The hanging method is compatible with composite frames of different specifications. For example, during the production process, by adding connecting devices at both ends of the composite frame material, the long and short sides can be continuously produced without switching. In some specific embodiments, the spraying device includes a third hanger 105, and the third hanger 105 is used to connect adjacent composite frames 200, such as Figure 6 , Figure 7 and Figure 8As shown, the third hanger 105 includes a second connecting rod 1051 and a second connecting piece 1052 and a third connecting piece 1053 arranged at both ends of the second connecting rod 1051. In some specific embodiments, the third hanger 105 is made of an iron wire with a diameter of 3 to 5 mm, the two ports of the third hanger 105 are open structures, the second connecting piece 1052 and the third connecting piece 1053 are both U-shaped structures, and the two structures are connected by the second connecting rod 1051. In the production process, by adding connecting devices at both ends of the composite frame material, continuous production of long and short sides can be achieved without switching.

[0061] Example 1: Composite material frame coating

[0062] Loading: The product is transferred to the loading area through the auxiliary loading device, and is hung on the hanging line after installing the elastic plug-in (secondary hanger). The horizontal distance between the composite material frames, that is, the hanging spacing, is 25cm.

[0063] Preheating: Raise the workpiece surface temperature to 20℃±5℃;

[0064] Dust removal: Use ion wind rod to remove dust on the surface of the workpiece (static removal time 3 seconds, ion balance + / -13V);

[0065] Spray conductive liquid (antistatic agent 3,3'-(9-octadecene imino)bis[2-hydroxy-N,N,N trimethyl]-1-propylammonium): dilute the antistatic agent stock solution with deionized water in a certain proportion (the final mass percentage concentration of the antistatic agent is 0.1%), and use the upper and lower reciprocating air spray gun to evenly spray the mixed conductive liquid (antistatic agent) onto the surface of the workpiece to apply a layer of about 10μm antistatic agent.

[0066] Surface drying: After spraying the conductive liquid (antistatic agent) on the product, the surface drying room temperature is 28°C, the humidity is 60% RH, and the surface drying time is 10 minutes. The moisture on the product surface evaporates and leaves an ion conductive layer.

[0067] DISK electrostatic spraying: The voltage of the high-voltage electrostatic field is 80kV. The high-speed rotation of the disc disperses the paint particles through centrifugal force and carries a high-voltage negative charge. The paint discharge volume is 500cc / min. Under the action of the electric field, the paint is evenly dispersed and directionally adsorbed, thus forming a uniform and firm coating layer on the surface of the workpiece.

[0068] Re-spraying: Use the upper and lower reciprocating spray guns with tracking to re-spray some areas.

[0069] Leveling: After spraying, the product is leveled and surface dried at a temperature of 20°C, a humidity of 50% RH, and a time of 15 minutes.

[0070] Baking: According to the TDS (technical parameter) requirements of the coating, the temperature is 80°C and the time is 60 minutes;

[0071] Next: After the product is baked, the elastic plug-in (secondary hanger) is removed and it is transferred to the next process after passing the inspection.

[0072] Example 2: The specific method is the same as that of Example 1, except that: the hanging interval is 10 cm; the deionized water is diluted with a certain proportion of the antistatic agent stock solution (the final mass percentage concentration of the antistatic agent is 2%).

[0073] Example 3: The specific method is the same as that of Example 1, except that: the hanging interval is 10 cm; the deionized water is diluted with a certain proportion of the antistatic agent stock solution (the final mass percentage concentration of the antistatic agent is 5%).

[0074] Comparative Example 1: The existing spraying technology is adopted, and the specific steps include: loading, dust removal, reciprocating machine spraying A side, leveling, reciprocating machine spraying A side, turning over, reciprocating machine spraying B side, leveling, baking, and loading.

[0075] Table 1 Coating quality of composite material frame after coating

[0076] Coating utilization rate (%) Production efficiency (seconds / root) Bake deformation Example 1 75%~78% 6 to 6.5 seconds Less than 1mm / m Example 2 80%~85% 2 seconds to 2.5 seconds Less than 1mm / m Example 3 85%~90% 2 seconds to 2.5 seconds Less than 1mm / m Comparative Example 1 30%~60% 8 to 15 seconds More than 1mm / m

[0077] Testing method for baking deformation: hang the product in an 80℃ oven for 1 hour, take it out, and test the curvature of the product after the product returns to room temperature.

[0078] The method of the present application has obtained the results shown in Table 1 through multiple production results statistics. It can be seen from the results in Table 1 that the method of the present application has the following effects: (1) the utilization rate of the coating is improved: it is increased from the original 30%-60% to more than 75%, and can basically be maintained in the range of 80%-90% (the utilization rate refers to the ratio of the weight of the unit volume of spraying to the weight of the coating used), saving the cost of coating use; (2) the production efficiency is improved: the production cycle is reduced from the original 8 seconds to 15 seconds per root to 6 seconds to 6.5 seconds. Since the present application adopts a hanging spraying method, after adjusting the spacing, the production cycle can even be reduced. Reduce to 2 seconds - 2.5 seconds per root without affecting the spraying quality; (3) Reduce the risk of deformation during baking (according to the composite frame industry standard of the "Guidelines for the First Batch Application Demonstration of Key New Materials (2024 Edition)": straightness ≤ 1mm / m); (4) Reduce production energy consumption: from the original 312kw / h to 147kw / h (the total power of electrical equipment can be measured by an electric energy meter); (5) Reduce VOC emissions: the VOC emissions generated by the original waste of 70%-40% of the paint are reduced to 20%-10% (VOC detection method GB / T23985-2009 national standard).

Claims

1. A composite material frame coating method, characterized in that: The following steps are involved: Antistatic agent is sprayed on the surface of the composite material frame; The composite material frame sprayed with the antistatic agent is surface dried; The composite material frame after surface drying treatment is coated with high voltage electric field electrostatic spray paint.

2. The composite material frame coating method according to claim 1, characterized in that: The antistatic agent includes a quaternary ammonium salt.

3. The composite material frame coating method according to claim 1, characterized in that: The spraying thickness of the antistatic agent is 5 μm to 10 μm; and / or, The mass percentage concentration of the antistatic agent is 0.1% to 10%.

4. The composite material frame coating method according to claim 1, characterized in that: The composite material frame is painted by hanging; and / or, The composite material frame is sprayed by a spraying device.

5. The composite material frame coating method according to claim 3, characterized in that: The composite material frame is suspended at a spacing of 10 cm to 25 cm.

6. The composite material frame coating method according to claim 1, characterized in that: The surface drying temperature is 18° C. to 28° C., the surface drying humidity is 40% RH to 60% RH, and the surface drying time is 5 min to 10 min.

7. The composite material frame coating method according to claim 1, characterized in that: The parameters of the high-voltage electric field electrostatic spraying are: voltage of 30 kV to 100 kV, and a coating discharge volume of 0 to 500 cc / min.

8. The composite material frame coating method according to claim 1, characterized in that: Before spraying the antistatic agent on the surface of the composite material frame, a preheating treatment is also performed; and / or, The temperature of the preheating treatment is 60° C. to 80° C., and the time of the preheating treatment is 5 min to 15 min.

9. The composite material frame coating method according to claim 8, characterized in that: After the composite material frame is preheated, dust removal is also performed; and / or, The dust removal process is to use an ion wind bar to remove dust on the surface of the composite material frame; and / or, The parameters of the dust removal process are: static electricity removal time 2 seconds to 5 seconds, ion balance -13V to +13V.

10. The composite material frame coating method according to claim 1, characterized in that: The composite material frame is subjected to leveling treatment after being electrostatically sprayed with paint using a high voltage electric field; and / or, The leveling parameters are: temperature of 18° C. to 28° C., humidity of 30% RH to 70% RH, and time of 10 min to 20 min.