Cobaltosic oxide super-hydrophilic / super-hydrophobic array fog collection film and preparation method thereof
By constructing a cobalt tetraoxide superhydrophilic/superhydrophobic array on the mist collecting film, the problem of low mist capture efficiency of the existing mist collecting film is solved, and efficient Fog capture and fog collection cycle.
Patent Information
- Application Number
- CN202410951271.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing mist-capturing films have low mist capture efficiency, mainly because the growth rate of surface condensation droplets is slow and easy to form a water film, which hinders the condensation of subsequent droplets.
The sol-gel method combined with DUV assisted low-temperature heat treatment technology was used to prepare a cobalt oxide film on a flexible plastic substrate. Nano clusters were deposited by hydrothermal method, low surface energy modification was used to use molecular self-assembly technology, and ultraviolet radiation was used to construct the ultras Hydrophilic/superhydrophobic arrays enable efficient mist capture and fog collection cycle.
By constructing an array of superhydrophilic/superhydrophobic regions, the nucleation and capture efficiency of fog droplets is significantly improved. The droplets can quickly gather and roll down from the array list, achieving efficient fog capture and fog collection cycles.
Smart Images

Figure CN118904688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mist collecting films, and in particular relates to a method for preparing a cobalt tetroxide super-hydrophilic / super-hydrophobic array mist collecting film, and also relates to a cobalt tetroxide super-hydrophilic / super-hydrophobic array mist collecting film. Background Art
[0002] Effectively collecting water from humid fog provides a new idea for solving problems in some water-scarce areas in my country. Through in-depth and systematic research on the basic principles, mechanisms and preparation methods of bionic fog collection, it is found that the development of high-performance fog collection films has become a hot topic. Most of the existing fog collection films are super-hydrophobic films regulated by factors such as surface wettability, chemical gradients, and micro-geometric structure gradients. Because the growth rate of condensed droplets on their surfaces is slow and it is easy to form a layer of water film covering the substrate surface, thereby hindering the condensation of subsequent droplets, their fog capture efficiency is not high. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film, which solves the problem of low fog capturing efficiency of the existing fog collecting film.
[0004] Another object of the present invention is to provide a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0005] The technical solution adopted by the present invention is a method for preparing a cobalt oxide super-hydrophilic / super-hydrophobic array fog collecting film, which is specifically implemented according to the following steps:
[0006] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0007] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0008] Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0009] Step 4: placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0010] The present invention is also characterized in that:
[0011] The specific process of step 1 is:
[0012] Step 1.1, adding cobalt acetate tetrahydrate into anhydrous methanol to dissolve, sealing the solution, stirring the solution magnetically at room temperature, and then adding acetylacetone to obtain a purple clear solution, sealing the purple clear solution, stirring the solution at room temperature, and allowing it to stand for aging to obtain a cobalt tetroxide sol;
[0013] Step 1.2, immersing the clean flexible plastic substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the flexible plastic substrate by a dipping-pulling method;
[0014] Step 1.3, placing the sol-gel film obtained in step 1.2 in an oven for drying, and then subjecting the dried sol-gel film to DUV-assisted low-temperature heat treatment to obtain a cobalt tetroxide film.
[0015] In step 1.1, the concentration of the cobalt oxide sol is 0.20 mol / L to 0.60 mol / L, and the molar ratio of cobalt acetate tetrahydrate to acetylacetone is 1:1;
[0016] In step 1.2, the flexible plastic substrate is a polyester plastic substrate (PET), a polyethylene naphthalate plastic substrate (PEN), or a polyimide (PI); the pulling speed of the dip-pull method is 1 mm / s to 3 mm / s;
[0017] In step 1.3, the process of DUV-assisted low-temperature heat treatment is as follows: temperature is 50°C to 200°C, irradiation time is 60min to 180min, and ultraviolet light wavelength is 180nm to 265nm.
[0018] The specific process of step 2 is:
[0019] Step 2.1, using cobalt chloride hexahydrate as a cobalt source and urea as an alkali source, fully dissolving them in deionized water to obtain a cobalt trioxide hydrothermal reaction solution;
[0020] Step 2.2, placing the cobalt oxide film obtained in step 1 in a polytetrafluoroethylene liner with the surface tilted downward at 45 degrees, and pouring the cobalt oxide reaction solution obtained in step 2.1 into the polytetrafluoroethylene liner, placing the polytetrafluoroethylene liner in a hydrothermal kettle for reaction, cooling to room temperature with the furnace, and taking out the sample after the reaction is completed;
[0021] Step 2.3, using deionized water and anhydrous ethanol to alternately wash the excess cobalt tetroxide nanopowder attached to the surface of the sample, drying and annealing the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface.
[0022] In step 2.1, the concentration of the cobalt tetraoxide hydrothermal reaction solution is 0.02 mol / L to 0.05 mol / L, and the molar ratio of cobalt chloride hexahydrate to urea is 1:5;
[0023] In step 2.2, the reaction temperature in the hydrothermal reactor is 95°C and the reaction time is 4h to 12h;
[0024] In step 2.3, the drying temperature is 60° C. to 80° C., and the drying time is 10 min to 30 min.
[0025] The specific process of step 3 is: placing the cobalt oxide film with a nanocluster structure on the surface obtained in step 2 in a low surface energy modifier solution for immersion modification, taking it out and washing it with anhydrous ethanol to remove the modifier remaining on the surface, and drying it to obtain a super hydrophobic cobalt oxide nanocluster film.
[0026] The concentration of the low surface energy modifier solution is 20g / L to 50g / L, the low surface energy modifier is one of octadecyltrimethyloxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, hexadecyltrimethyloxysilane, and tri-(1H,1H-pentadecafluorooctyloxy)-tert-butoxysilane, the solvent is anhydrous ethanol, the immersion modification time is 10min to 40min, the drying temperature is 25℃ to 80℃, and the time is 10min to 40min.
[0027] The specific process of step 4 is: covering the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3 with a mask having a specific pattern, and then irradiating the unmasked area with deep ultraviolet light at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0028] The wavelength of ultraviolet light is 180nm~265nm, and the irradiation time is 3h~4h.
[0029] Another technical solution adopted by the present invention is that the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film is obtained by adopting the above-mentioned preparation method.
[0030] The beneficial effects of the present invention are as follows: the preparation method of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collection film of the present invention first adopts a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology to prepare a cobalt tetroxide film on a flexible plastic substrate, and then uses a hydrothermal method to further deposit dense cobalt tetroxide nanoclusters on its surface, and then uses molecular self-assembly technology to perform low surface energy modification on it, and then uses deep ultraviolet radiation-assisted mask technology to construct an array with super-hydrophilic and super-hydrophobic regions regularly alternating, and then through the effective regulation of its curvature gradient, efficient fog capture and fog collection cycle can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM image of a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film prepared on a PET plastic substrate by the method of the present invention;
[0032] Figure 2 This is a characterization diagram of the movement of unbent droplets on the surface of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film prepared on a PET substrate by the method of the present invention;
[0033] Figure 3 This is a characterization diagram of the movement of fog droplets on the surface of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collection film bent 150 degrees on the PET substrate prepared by the method of the present invention;
[0034] Figure 4 This is a characterization diagram of the movement of fog droplets on the surface of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collection film bent 120 degrees on the PET substrate prepared by the method of the present invention;
[0035] Figure 5 This is a characterization diagram of the movement of fog droplets on the surface of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collection film bent 90 degrees on the PET substrate prepared by the method of the present invention;
[0036] Figure 6 This is a characterization diagram of the movement of fog droplets on the surface of the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collection film bent at 60° prepared on a PET substrate by the method of the present invention;
[0037] Figure 7 The figure is a relationship diagram between the surface contact angle and the number of frictions of the super-hydrophobic cobalt tetroxide nanocluster film prepared on a PEN plastic substrate by the method of the present invention. DETAILED DESCRIPTION
[0038] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0039] The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film of the present invention is specifically implemented according to the following steps:
[0040] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0041] The specific process of step 1 is:
[0042] Step 1.1, adding cobalt acetate tetrahydrate into anhydrous methanol to dissolve, sealing the solution, stirring the solution magnetically at room temperature, and then adding acetylacetone to obtain a purple clear solution, sealing the purple clear solution, stirring the solution at room temperature, and allowing it to stand for aging to obtain a cobalt tetroxide sol;
[0043] The concentration of the cobalt oxide sol is 0.20 mol / L to 0.60 mol / L, and the molar ratio of cobalt acetate tetrahydrate to acetylacetone is 1:1.
[0044] Step 1.2, immersing the clean flexible plastic substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the flexible plastic substrate by a dipping-pulling method;
[0045] Wherein, the flexible plastic substrate is one of a polyester plastic substrate (PET), a polyethylene naphthalate plastic substrate (PEN), or a polyimide (PI);
[0046] The pulling speed of the immersion-pulling method is 1 mm / s to 3 mm / s;
[0047] Step 1.3, drying the sol-gel film obtained in step 1.2 in an oven at 80° C. for 30 minutes, and then subjecting the dried sol-gel film to a DUV-assisted low-temperature heat treatment to obtain a cobalt oxide film;
[0048] Among them, the process of DUV (deep ultraviolet) assisted low-temperature heat treatment is: temperature is 50℃~200℃, irradiation time is 60min~180min, ultraviolet wavelength is 180nm~265nm;
[0049] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0050] The specific process is:
[0051] Step 2.1, using cobalt chloride hexahydrate as a cobalt source and urea as an alkali source, fully dissolving them in deionized water to obtain a cobalt trioxide hydrothermal reaction solution;
[0052] The concentration of the cobalt tetraoxide hydrothermal reaction solution is 0.02 mol / L to 0.05 mol / L, and the molar ratio of cobalt chloride hexahydrate to urea is 1:5;
[0053] Step 2.2, placing the cobalt oxide film obtained in step 1 in a polytetrafluoroethylene liner with the surface tilted downward at 45 degrees, and pouring the cobalt oxide reaction solution obtained in step 2.1 into the polytetrafluoroethylene liner, placing the polytetrafluoroethylene liner in a hydrothermal kettle for reaction, cooling to room temperature with the furnace, and taking out the sample after the reaction is completed;
[0054] The reaction temperature in the hydrothermal reactor is 95°C and the reaction time is 4h to 12h;
[0055] Step 2.3, washing the excess cobalt tetroxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface;
[0056] The drying temperature is 60°C to 80°C, and the drying time is 10min to 30min.
[0057] Step 3: using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface, to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0058] The specific process is:
[0059] The cobalt oxide thin film with a nanocluster structure on the surface obtained in step 2 is placed in a low surface energy modifier solution with a concentration of 20 g / L to 50 g / L for 10 to 40 minutes, and then washed with anhydrous ethanol to remove the modifier remaining on the surface, and dried at a temperature of 25° C. to 80° C. for 10 to 40 minutes to obtain a super hydrophobic cobalt oxide nanocluster thin film;
[0060] The low surface energy modifier is one of octadecyltrimethyloxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, hexadecyltrimethyloxysilane, and tris-(1H,1H-pentadecafluorooctyloxy)-tert-butoxysilane, and the solvent is anhydrous ethanol;
[0061] Step 4: placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film;
[0062] The specific process is:
[0063] A mask having a stripe size of 1 mm×4 cm is covered on the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3, and then deep ultraviolet light is used to irradiate the uncovered area at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film; the surface of the obtained cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film is bent under the action of an external force;
[0064] Among them, the wavelength of ultraviolet light is 180nm~265nm, and the irradiation time is 3h~4h.
[0065] The principle of the present invention is that the super-hydrophilic area in the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog-collecting film has great adhesion to the droplets, can quickly capture the droplets in the air, and make them condense each other to form larger droplets; the super-hydrophobic area has a lower surface free energy and a higher contact angle, and has extremely weak adhesion to the droplets, which can make the droplets quickly roll off the sample surface; the super-hydrophilic and super-hydrophobic areas are regularly arranged alternately, which can not only accelerate the convergence and growth of the droplets, but also significantly improve the nucleation and capture efficiency of the droplets, and when the droplets reach a critical size, they can quickly roll off the surface of the array fog-collecting film under the action of the low adhesion of the super-hydrophobic area, allowing the super-hydrophilic area to re-contact and capture the droplets. In addition, the surface of the material is bent by external force. As the degree of bending increases, the Laplace pressure difference generated on the surface increases accordingly, and the rate of directional movement of the droplets is accelerated. The droplets quickly nucleate in the superhydrophilic area, and after growing to a critical size, they move toward the middle under the combined action of the superhydrophobic area and the Laplace pressure difference. In this process, the droplets continue to converge and grow until they fall off, and this cycle repeats over and over again, thereby achieving efficient fog capture and fog collection cycle.
[0066] Example 1
[0067] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0068] The specific process of step 1 is:
[0069] Step 1.1, 5.98 g of cobalt acetate tetrahydrate was added to 40 mL of anhydrous methanol and dissolved, and the mixture was sealed and magnetically stirred at room temperature for 30 min, and then 2.40 g of acetylacetone was added to obtain a purple clear solution, and the purple clear solution was sealed and stirred at room temperature for 3 h, and allowed to stand for 12 h to obtain a purple cobalt tetroxide sol with a concentration of 0.20 mol / L;
[0070] Step 1.2, immersing the cleaned PET substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the PET substrate by an immersion-pulling method at a pulling speed of 1 mm / s;
[0071] Step 1.3, drying the sol-gel film obtained in step 1.2 in an oven at 80° C. for 30 minutes, and then subjecting the dried sol-gel film to a DUV-assisted low-temperature heat treatment to obtain a cobalt oxide film;
[0072] Among them, the process of DUV-assisted low-temperature heat treatment is: temperature is 50°C, irradiation time is 60min, and ultraviolet wavelength is 180nm~265nm;
[0073] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0074] The specific process is:
[0075] Step 2.1, 0.87 g of cobalt chloride hexahydrate as a cobalt source and 1.08 g of urea as an alkali source are fully dissolved in 60 mL of deionized water to obtain a hydrothermal reaction solution with a concentration of 0.02 mol / L cobalt tetraoxide;
[0076] Step 2.2, the cobalt oxide film obtained in step 1 is placed in a polytetrafluoroethylene liner with a capacity of 100 mL with the surface tilted downward at 45 degrees. During this process, it is noted that the volume of the reaction liquid must not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner, and the cobalt oxide reaction liquid obtained in step 2.1 is poured into the polytetrafluoroethylene liner, and the polytetrafluoroethylene liner is placed in a hydrothermal autoclave to react at 95°C for 4 hours, cooled to room temperature with the furnace, and the sample is taken out after the reaction is completed;
[0077] Step 2.3, washing the excess cobalt tetroxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface;
[0078] The drying temperature is 80°C and the drying time is 10 min.
[0079] Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0080] The specific process is:
[0081] The cobalt oxide film with a nanocluster structure on the surface obtained in step 2 is placed in an anhydrous ethanol solution of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane with a concentration of 20 g / L for immersion modification for 20 minutes, and then taken out and washed with anhydrous ethanol to remove the residual modifier on the surface, and dried at 80° C. for 10 minutes to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0082] Step 4, placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film, and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film;
[0083] The specific process is:
[0084] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 265 nm is irradiated on the unmasked area for 4 hours at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0085] Depend on Figure 1 It can be seen that the surface morphology of the cobalt tetroxide superhydrophilic / superhydrophobic array fog collection film is a nanocluster structure.
[0086] Example 2
[0087] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0088] The specific process of step 1 is:
[0089] Step 1.1, 11.95 g of cobalt acetate tetrahydrate was added to 40 mL of anhydrous methanol for dissolution, the mixture was sealed and magnetically stirred at room temperature for 30 min, and then 4.80 g of acetylacetone was added to obtain a purple clear solution, the purple clear solution was sealed and stirred at room temperature for 4 h, and allowed to stand for 12 h to obtain a purple cobalt tetroxide sol with a concentration of 0.40 mol / L;
[0090] Step 1.2, immersing the cleaned PET substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the PET substrate by an immersion-pulling method at a pulling speed of 2 mm / s;
[0091] Step 1.3, drying the sol-gel film obtained in step 1.2 in an oven at 80° C. for 30 minutes, and then subjecting the dried sol-gel film to a DUV-assisted low-temperature heat treatment to obtain a cobalt oxide film;
[0092] Among them, the process of DUV-assisted low-temperature heat treatment is: temperature is 150°C, irradiation time is 120min, and ultraviolet wavelength is 180nm~265nm;
[0093] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0094] The specific process is:
[0095] Step 2.1, using 1.30 g of cobalt chloride hexahydrate as a cobalt source and 1.62 g of urea as an alkali source, fully dissolving them in 60 mL of deionized water to obtain a hydrothermal reaction solution with a concentration of 0.03 mol / L cobalt tetraoxide;
[0096] Step 2.2, the cobalt oxide film obtained in step 1 is placed in a polytetrafluoroethylene liner with a capacity of 100 mL with the surface tilted downward at 45 degrees. During this process, it is noted that the volume of the reaction liquid must not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner, and the cobalt oxide reaction liquid obtained in step 2.1 is poured into the polytetrafluoroethylene liner, and the polytetrafluoroethylene liner is placed in a hydrothermal autoclave to react at 95°C for 6 hours, cooled to room temperature with the furnace, and the sample is taken out after the reaction is completed;
[0097] Step 2.3, washing the excess cobalt tetroxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface;
[0098] The drying temperature is 80°C and the drying time is 10 min.
[0099] Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0100] The specific process is:
[0101] The cobalt oxide film with a nanocluster structure on the surface obtained in step 2 is placed in an anhydrous ethanol solution of octadecyltrimethyloxysilane with a concentration of 50 g / L for 10 minutes for immersion modification, and then taken out and washed with anhydrous ethanol to remove the residual modifier on the surface, and dried at 80° C. for 10 minutes to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0102] Step 4, placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film, and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film;
[0103] The specific process is:
[0104] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 265 nm is irradiated on the unmasked area for 3 h at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0105] Depend on Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 It can be seen that when the surface is bent to 90°, the size of the droplets on the surface is the largest and the distribution is the most dense.
[0106] Example 3
[0107] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0108] The specific process of step 1 is:
[0109] Step 1.1, 8.96 g of cobalt acetate tetrahydrate was added to 40 mL of anhydrous methanol and dissolved, the mixture was sealed and magnetically stirred at room temperature for 30 min, and then 3.60 g of acetylacetone was added to obtain a purple clear solution, the purple clear solution was sealed and stirred at room temperature for 3 h, and allowed to stand for 12 h to obtain a purple cobalt tetroxide sol with a concentration of 0.30 mol / L;
[0110] Step 1.2, immersing the cleaned PET substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the PET substrate by an immersion-pulling method at a pulling speed of 1 mm / s;
[0111] Step 1.3, drying the sol-gel film obtained in step 1.2 in an oven at 80° C. for 30 minutes, and then subjecting the dried sol-gel film to a DUV-assisted low-temperature heat treatment to obtain a cobalt oxide film;
[0112] Among them, the process of DUV-assisted low-temperature heat treatment is: temperature is 100°C, irradiation time is 90 minutes, and ultraviolet light wavelength is 180nm~265nm;
[0113] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0114] The specific process is:
[0115] Step 2.1, 1.74 g of cobalt chloride hexahydrate as a cobalt source and 2.16 g of urea as an alkali source are fully dissolved in 60 mL of deionized water to obtain a hydrothermal reaction solution with a concentration of 0.04 mol / L cobalt tetraoxide;
[0116] Step 2.2, the cobalt oxide film obtained in step 1 is placed in a polytetrafluoroethylene liner with a capacity of 100 mL with the surface tilted downward at 45 degrees. During this process, it is noted that the volume of the reaction liquid must not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner, and the cobalt oxide reaction liquid obtained in step 2.1 is poured into the polytetrafluoroethylene liner, and the polytetrafluoroethylene liner is placed in a hydrothermal autoclave to react at 95°C for 8 hours, cooled to room temperature with the furnace, and the sample is taken out after the reaction is completed;
[0117] Step 2.3, washing the excess cobalt tetroxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface;
[0118] The drying temperature is 80°C and the drying time is 20 minutes.
[0119] Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0120] The specific process is:
[0121] The cobalt oxide film with a nanocluster structure on the surface obtained in step 2 is placed in an anhydrous ethanol solution of octadecyltrimethyloxysilane with a concentration of 30 g / L for immersion modification for 15 minutes, and then taken out and washed with anhydrous ethanol to remove the residual modifier on the surface, and dried at 80° C. for 20 minutes to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0122] Step 4, placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film, and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film;
[0123] The specific process is:
[0124] A mask with a grid size of 50 μm×50 μm is covered on the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3, and then ultraviolet light with a wavelength of 180 nm to 265 nm is irradiated on the unmasked area for 4 hours at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
[0125] Depend on Figure 7 It can be seen that with the increase in the number of frictions, the contact angle of the film surface slowly decreases. After 10 frictions, the contact angle still remains at 141.2°, which is hydrophobic.
[0126] Example 4
[0127] Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology;
[0128] The specific process of step 1 is:
[0129] Step 1.1, 17.93 g of cobalt acetate tetrahydrate was added to 40 mL of anhydrous methanol and dissolved, the mixture was sealed and magnetically stirred at room temperature for 30 min, and then 7.20 g of acetylacetone was added to obtain a purple clear solution, the purple clear solution was sealed and stirred at room temperature for 5 h, and allowed to stand for 12 h to obtain a purple cobalt tetroxide sol with a concentration of 0.60 mol / L;
[0130] Step 1.2, immersing the cleaned PEN substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the PET substrate by an immersion-pulling method at a pulling speed of 3 mm / s;
[0131] Step 1.3, drying the sol-gel film obtained in step 1.2 in an oven at 80° C. for 30 minutes, and then subjecting the dried sol-gel film to a DUV-assisted low-temperature heat treatment to obtain a cobalt oxide film;
[0132] Among them, the process of DUV-assisted low-temperature heat treatment is: temperature is 200°C, irradiation time is 180min, and ultraviolet light wavelength is 180nm~265nm;
[0133] Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface;
[0134] The specific process is:
[0135] Step 2.1, 2.17 g of cobalt chloride hexahydrate as a cobalt source and 2.70 g of urea as an alkali source are fully dissolved in 60 mL of deionized water to obtain a hydrothermal reaction solution with a concentration of 0.05 mol / L cobalt tetraoxide;
[0136] Step 2.2, the cobalt oxide film obtained in step 1 is placed in a polytetrafluoroethylene liner with a capacity of 100 mL with the surface tilted downward at 45 degrees. During this process, it is noted that the volume of the reaction liquid should not exceed 2 / 3 of the volume of the polytetrafluoroethylene liner, and the cobalt oxide reaction liquid obtained in step 2.1 is poured into the polytetrafluoroethylene liner, and the polytetrafluoroethylene liner is placed in a hydrothermal autoclave to react at 95°C for 12 hours, cooled to room temperature with the furnace, and the sample is taken out after the reaction is completed;
[0137] Step 2.3, washing the excess cobalt tetroxide nanopowder attached to the surface of the sample with deionized water and anhydrous ethanol alternately, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface;
[0138] Among them, the drying temperature is 60°C and the drying time is 30 minutes;
[0139] Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0140] The specific process is:
[0141] The cobalt oxide film with a nanocluster structure on the surface obtained in step 2 is placed in an anhydrous ethanol solution of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane with a concentration of 50 g / L for immersion modification for 40 minutes, and then washed with anhydrous ethanol to remove the residual modifier on the surface, and dried at 25° C. for 40 minutes to obtain a super-hydrophobic cobalt oxide nanocluster film;
[0142] Step 4, placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film, and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film;
[0143] The specific process is:
[0144] A mask with an aperture size of r = 5 mm is covered on the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3, and then ultraviolet light with a wavelength of 180nm to 265nm is irradiated on the unmasked area for 3 hours at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
Claims
1. A method for preparing a cobalt oxide super-hydrophilic / super-hydrophobic array fog collecting film, characterized in that: Follow the steps below to implement it: Step 1, preparing a cobalt tetroxide thin film on a flexible plastic substrate by using a sol-gel method combined with a DUV-assisted low-temperature heat treatment technology; Step 2, depositing cobalt tetroxide nanoclusters on the surface of the cobalt tetroxide film by a hydrothermal method to obtain a cobalt tetroxide film having a nanocluster structure on the surface; Step 3, using molecular self-assembly technology to perform low surface energy modification on the cobalt oxide film having a nanocluster structure on the surface to obtain a super-hydrophobic cobalt oxide nanocluster film; Step 4: placing a mask on the surface of the super-hydrophobic cobalt tetroxide nanocluster film and irradiating it with deep ultraviolet light to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
2. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, characterized in that: The specific process of step 1 is: Step 1.1, adding cobalt acetate tetrahydrate into anhydrous methanol to dissolve, sealing the solution, stirring the solution magnetically at room temperature, and then adding acetylacetone to obtain a purple clear solution, sealing the purple clear solution, stirring the solution at room temperature, and allowing it to stand for aging to obtain a cobalt tetroxide sol; Step 1.2, immersing the clean flexible plastic substrate into the cobalt tetroxide sol obtained in step 1.1, and preparing a smooth and flat sol-gel film on the surface of the flexible plastic substrate by a dipping-pulling method; Step 1.3, placing the sol-gel film obtained in step 1.2 in an oven for drying, and then subjecting the dried sol-gel film to DUV-assisted low-temperature heat treatment to obtain a cobalt tetroxide film.
3. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 2, characterized in that: In step 1.1, the concentration of the cobalt tetroxide sol is 0.20 mol / L to 0.60 mol / L, and the molar ratio of cobalt acetate tetrahydrate to acetylacetone is 1:1; In step 1.2, the flexible plastic substrate is one of a polyester plastic substrate (PET), a polyethylene naphthalate plastic substrate (PEN) or a polyimide (PI); the pulling speed of the dip-pull method is 1 mm / s to 3 mm / s; In step 1.3, the process of DUV-assisted low-temperature heat treatment is as follows: temperature is 50°C to 200°C, irradiation time is 60min to 180min, and ultraviolet light wavelength is 180nm to 265nm.
4. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, characterized in that: The specific process of step 2 is: Step 2.1, using cobalt chloride hexahydrate as a cobalt source and urea as an alkali source, fully dissolving them in deionized water to obtain a cobalt trioxide hydrothermal reaction solution; Step 2.2, placing the cobalt oxide film obtained in step 1 in a polytetrafluoroethylene liner with the surface tilted downward at 45 degrees, and pouring the cobalt oxide reaction solution obtained in step 2.1 into the polytetrafluoroethylene liner, placing the polytetrafluoroethylene liner in a hydrothermal kettle for reaction, cooling to room temperature with the furnace, and taking out the sample after the reaction is completed; Step 2.3, using deionized water and anhydrous ethanol to alternately wash the excess cobalt tetroxide nanopowder attached to the surface of the sample, and drying the washed sample to obtain a cobalt tetroxide film with a nanocluster structure on the surface.
5. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 4, characterized in that: In step 2.1, the concentration of the cobalt tetraoxide hydrothermal reaction solution is 0.02 mol / L to 0.05 mol / L, and the molar ratio of cobalt chloride hexahydrate to urea is 1:5; In step 2.2, the reaction temperature in the hydrothermal reactor is 95°C and the reaction time is 4h to 12h; In step 2.3, the drying temperature is 60° C. to 80° C., and the drying time is 10 min to 30 min.
6. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, characterized in that: The specific process of step 3 is: placing the cobalt oxide film with a nanocluster structure on the surface obtained in step 2 in a low surface energy modifier solution for immersion modification, taking it out and washing it with anhydrous ethanol to remove the modifier remaining on the surface, and drying it to obtain a super hydrophobic cobalt oxide nanocluster film.
7. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 6, characterized in that: The concentration of the low surface energy modifier solution is 20g / L to 50g / L, the low surface energy modifier is one of octadecyltrimethyloxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, hexadecyltrimethyloxysilane, and tri-(1H,1H-pentadecafluorooctyloxy)-tert-butoxysilane, the solvent is anhydrous ethanol, the immersion modification time is 10min to 40min, the drying temperature is 25℃ to 80℃, and the time is 10min to 40min.
8. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 1, characterized in that: The specific process of step 4 is: covering the surface of the super-hydrophobic cobalt tetroxide nanocluster film obtained in step 3 with a mask having a specific pattern, and then irradiating the unmasked area with deep ultraviolet light at room temperature to obtain a cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film.
9. The method for preparing the cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film according to claim 8, characterized in that: The wavelength of ultraviolet light is 180nm~265nm, and the irradiation time is 3h~4h.
10. Cobalt tetroxide super-hydrophilic / super-hydrophobic array fog collecting film, characterized in that: The method is adopted as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Construction method of titanium surface micrometre-grade pattern based on ultra-hydrophilic / ultra-hydrophobic characteristic
CN101016642A
Preparation method for super-hydrophobic Co3O4 thin film of micro-nano composite structure
CN105369248A
Co3O4 nanometer array super-hydrophobic material coating and preparation method thereof
CN109505115A
Preparation method of efficient condensation hydrophilic and hydrophobic thin-film coating with multi-scale structure
CN110372225A
Method of silica gel block material with hydrophilic and sliding surface and tapered copper needle with superhydrophobic-hydrophilic surface for collecting water mist
CN111411353A