Method for improving thermal fatigue resistance of die steel by using trace nano-particles

By introducing micro-nano particles into mold steel and combining them with specific processes, micro-nano particle-reinforced mold steel was prepared, solving the problem of insufficient thermal fatigue resistance of hot work mold steel and realizing the production of high-performance and low-cost mold steel.

CN118905209APending Publication Date: 2024-11-08JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410873185.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Domestically produced hot work die steel cannot meet high-performance requirements, making dies prone to failure during use. In particular, failures caused by thermal fatigue are quite common, which restricts the development of the die industry.

Method used

By introducing trace amounts of nanoparticles into mold steel and generating nanoparticles through an electro-explosion reaction, combined with processes such as vacuum induction melting, electroslag remelting, and vacuum heat treatment, micro- and nanoparticle-reinforced mold steel is prepared, thereby improving its resistance to thermal fatigue.

Benefits of technology

It significantly improves the thermal fatigue resistance of mold steel, extends the service life of molds, reduces production costs, and achieves independent control in the mold industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905209A_ABST
    Figure CN118905209A_ABST
Patent Text Reader

Abstract

The invention provides a method for improving thermal fatigue resistance of die steel through trace nano-particles, and belongs to the technical field of high-performance hot work die steel. The method comprises the following steps: placing a Ti-V-Zr wire in an electric explosion reaction device, vaporizing the wire, and reacting with nitrogen to generate a first kind of mixed nanoparticles; uniformly mixing with Fe powder to obtain second mixed powder, and rotationally coating the second mixed powder with iron foil to prepare a mixed particle wire; in a vacuum induction melting furnace, die steel is melted into molten steel, the molten steel is subjected to electric arc and argon blowing refining in an LF refining furnace, the molten steel is added into the molten steel, the molten steel enters a refining furnace outside a VD vacuum decarburization furnace to be subjected to degassing refining, and an electrode blank steel ingot is formed through casting; and carrying out electroslag remelting to remove inclusions in the steel, and carrying out multidirectional forging and vacuum heat treatment to prepare the micro-nano particle reinforced die steel. The method has important significance in improving the quality and performance level of domestic hot work die steel, reducing the production cost and realizing autonomous controllability of the die industry in China.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-performance hot working die steel, and in particular to a method for improving the thermal fatigue resistance of die steel with trace nanoparticles. Background Art

[0002] As the mold material required for hot processing and forming of metal products, hot working die steel plays an indispensable role in industrial production and metal forming. It is widely used in the mass production of die casting and extrusion products. However, the hot working die steel produced domestically often cannot meet the high performance requirements, which leads to the failure of the mold during use. According to statistics, about 70% of the failures are caused by thermal fatigue. Therefore, although my country is the world's largest steel producer, it needs to import hundreds of thousands of tons of high-end die steel every year, which not only increases the cost, but also limits the further development of my country's mold industry. At this stage, improving the quality and performance of domestic die steel has become an urgent need for the development of my country's mold industry. Traditional methods to improve the thermal fatigue resistance of die steel, such as alloy composition optimization, heat treatment process design and surface strengthening methods, have reached a research bottleneck. Using micro-nano particles to improve the thermal fatigue resistance of steel has become a new idea. This method provides an innovative method and approach for producing high thermal fatigue resistance and long life die steel. Summary of the invention

[0003] The purpose of the present invention is to propose a method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles. The thermal fatigue resistance of mold steel is improved by using trace nanoparticles, which is of great significance to improving the quality and performance level of domestic hot working die steel, reducing production costs, and realizing independent control of my country's mold industry.

[0004] The technical solution of the present invention is achieved in this way:

[0005] The present invention provides a method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles, comprising the following steps:

[0006] Step 1: placing Ti-V-Zr wire in an electric explosion reaction device, vaporizing the wire and reacting with nitrogen gas to generate first mixed nanoparticles;

[0007] Step 2: Evenly mix the first mixed nanoparticles with Fe powder to obtain a second mixed powder, and use iron foil to cover the second mixed powder to prepare a mixed particle wire;

[0008] Step 3: In a vacuum induction melting furnace, the mold steel is melted into molten steel, and then arc and argon blowing refining are carried out in a LF furnace refining furnace. During the refining process, the mixed particle wire is added to the molten steel, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining, and then cast into electrode billet steel ingots;

[0009] Step 4: Electroslag remelting the electrode billet steel ingot to remove inclusions in the steel, followed by multi-directional forging and vacuum heat treatment to finally obtain micro-nano particle reinforced die steel.

[0010] As a further improvement of the present invention, in the step 1, preparing the first hybrid nanoparticles comprises the following steps:

[0011] Step 1: using an electric explosion reaction device, placing the Ti-V-Zr wire alloy in a nitrogen atmosphere to react with the nitrogen atmosphere to generate micro-nano particles;

[0012] Step 2: In the mixed powder, the total mass fraction of the three ceramics of titanium nitride, vanadium nitride and zirconium nitride is 20wt.%-40wt.%, and the remainder is pure iron powder, which is the second mixed particle;

[0013] Step 3: first perform vacuum electroslag remelting, then perform high-temperature diffusion, and then directly forge after leaving the heat treatment furnace. The starting forging temperature is 1200°C, the final forging temperature is greater than 1100°C, and then spray water cooling treatment is performed to obtain the first mixed nanoparticles.

[0014] As a further improvement of the present invention, the composition of the Ti-V-Zr wire is: Ti: 0.75-0.85wt.%, V: 0.02-0.15wt.%, Zr: 0.05-0.20wt.%; the diameter is 2.0-4.0mm, and the particle size of the pure iron powder is 5-200 microns.

[0015] As a further improvement of the present invention, in the step 2, the first mixed nanoparticles and Fe-Cr powder are uniformly mixed in a mixer, the mixer speed is 10-60 r / min, and the mixing time is 4-10 h.

[0016] As a further improvement of the present invention, in the above step three, arc and argon blowing refining are carried out in the LF furnace refining furnace for 30-60 minutes. At the 10th minute of refining, the mixed particle wire is added to the molten steel liquid, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining for 40-60 minutes, and then cast into electrode billet ingots.

[0017] As a further improvement of the present invention, in the above step three, the total mass percentage of the three ceramics of micro-nano titanium nitride, vanadium nitride and zirconium nitride added to the mass percentage of the molten steel is 0.01wt.%-0.05wt.%.

[0018] As a further improvement of the present invention, in the above step 4, the arc power of the electroslag remelting furnace is set in the range of 120-180kW, and the current density is 6-9A / mm 2The melting time is 40-90 minutes, and argon is selected as the inert gas shielding gas.

[0019] As a further improvement of the present invention, in the above step four, the high-temperature diffusion temperature of the electroslag ingot is 1270-1290°C, and the high-temperature diffusion time is 15-25 hours. After being taken out of the furnace, the temperature of the electroslag ingot is reduced by 1200°C, and then forging is carried out with a forging ratio of 10-15, and water mist cooling is performed after forging.

[0020] As a further improvement of the present invention, in step four, the heating method of the vacuum heat treatment is staged heating, which is respectively increased to 550°C and 850°C and kept warm for 15 minutes, followed by an austenitizing temperature of 1030°C-1080°C, a holding time of 2h-3h, and an oil quenching method, a tempering temperature of 550-630°C, and a tempering time of 4-8h.

[0021] The present invention has the following beneficial effects: the present invention improves the thermal fatigue resistance of mold steel through trace nanoparticles. The mold steel preparation method is simple and efficient, the manufacturing cycle is short, the mold is durable, the module surface is smooth and crack-free, and the processing quality of plastic molds is greatly improved. It is of great significance to improve the quality and performance level of domestic hot working mold steel, reduce production costs, and realize independent control of my country's mold industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 This is the morphology of the surface oxide layer of the nanoparticle reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Example 1 of the present invention.

[0024] Figure 2 This is the side oxidation corrosion of the nanoparticle reinforced die steel in Example 1 of the present invention after 2000 times of thermal fatigue (20-650°C).

[0025] Figure 3 This is the thermal fatigue crack propagation of the nanoparticle reinforced die steel after 2000 thermal fatigue cycles (20-650°C) in Example 1 of the present invention.

[0026] Figure 4 This is the morphology of the surface oxide layer of the nanoparticle reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Example 2 of the present invention.

[0027] Figure 5This is the side oxidation corrosion condition of the nanoparticle reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Example 2 of the present invention.

[0028] Figure 6 This is the thermal fatigue crack propagation of the nanoparticle reinforced die steel after 2000 thermal fatigue cycles (20-650°C) in Example 2 of the present invention.

[0029] Figure 7 This is the morphology of the surface oxide layer of the nanoparticle reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Example 3 of the present invention.

[0030] Figure 8 This is the side oxidation corrosion condition of the nanoparticle reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Example 3 of the present invention.

[0031] Fig. 9 This is the thermal fatigue crack propagation of the nanoparticle reinforced die steel after 2000 thermal fatigue cycles (20-650°C) in Example 3 of the present invention.

[0032] Fig.10 This is the morphology of the surface oxide layer of the nanoparticle-reinforced die steel after 2000 times of thermal fatigue (20-650°C) in Comparative Example 1 of the present invention.

[0033] Fig.11 This is the side oxidation corrosion condition of the nanoparticle reinforced die steel in Comparative Example 1 of the present invention after 2000 times of thermal fatigue (20-650°C).

[0034] Fig.12 This is the thermal fatigue crack propagation of the nanoparticle reinforced die steel after 2000 thermal fatigue cycles (20-650°C) in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] In the preparation example of the present invention, the composition of the Ti-V-Zr wire is: Ti: 0.75-0.85wt.%, V: 0.02-0.15wt.%, Zr: 0.05-0.20wt.%; the diameter is 2.0-4.0mm, and the particle size of the pure iron powder is 5-200 microns.

[0037] In the present invention, the chemical composition range of the mold steel is: C: 0.21-0.55wt.%; Si: 0.05-0.15wt.%; Mn: 0.20-0.40wt.%; P: ≤0.005wt.%; S≤0.0015wt.%; Cr: 5.1-5.5wt.%; V: 0.7-0.85wt.%; Mo: 2.6-3.2wt.%; N: 0.04-0.06wt.%; H≤0.0003wt.%; O≤0.0010wt.%.

[0038] Preparation Example 1

[0039] Step 1: using an electric explosion reaction device, placing the Ti-V-Zr wire alloy in a nitrogen atmosphere to react with the nitrogen atmosphere to generate micro-nano particles;

[0040] Step 2, in the mixed powder, the total mass fraction of the three ceramics of titanium nitride, vanadium nitride and zirconium nitride is 30%, and the remainder is pure iron powder, which is the second mixed particle;

[0041] Step 3: vacuum electroslag remelting is performed on the mold steel, and then high-temperature diffusion is performed, and then forging is performed directly after leaving the heat treatment furnace. The starting forging temperature is 1200°C, the final forging temperature is 1150°C, and then spray water cooling treatment is performed to obtain the first mixed nanoparticles.

[0042] Example 1

[0043] This embodiment provides a method for improving the thermal fatigue resistance of mold steel by using trace amounts of nanoparticles, comprising the following steps:

[0044] Step 1: uniformly mix the first mixed nanoparticles prepared in Preparation Example 1 with Fe-Cr powder in a mixer at a mixer speed of 10 r / min for 4 h to obtain a second mixed powder, and use iron foil to cover the second mixed powder to prepare a mixed particle wire;

[0045] Step 2: In a vacuum induction melting furnace, the mold steel is melted into molten steel, and then arc and argon blowing are performed in a LF furnace refining furnace for 30 minutes. At the 10th minute of refining, the mixed particle wire is added to the molten steel, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining for 40 minutes, and then cast into an electrode billet steel ingot; the total mass percentage of the three ceramics of micro-nano titanium nitride, vanadium nitride and zirconium nitride added to the steel liquid is 0.01wt.%;

[0046] Step 3: Electroslag remelting is performed on the electrode billet steel ingot to remove inclusions in the steel, followed by multi-directional forging and vacuum heat treatment to finally obtain die steel reinforced with micro-nano particles. The arc power of the electroslag remelting furnace is set within 180kW and the current density is 9A / mm 2The smelting time is 90 minutes, argon is selected as the inert gas shielding gas, the high-temperature diffusion temperature of the electroslag ingot is 1290℃, and the high-temperature diffusion time is 25 hours. After being taken out of the furnace, the temperature of the electroslag ingot is reduced by 1200℃, and then forged with a forging ratio of 15. After forging, it is cooled by water mist. The heating method of vacuum heat treatment is staged heating, which is respectively increased to 550℃ and 850℃ and kept warm for 15min. Then the austenitizing temperature is 1080℃, and the holding time is 3h. The quenching method is oil quenching, the tempering temperature is 630℃, and the tempering time is 8h.

[0047] The 0.01wt.% micro-nano TiN+VN+ZrN particle reinforced die steel prepared in this embodiment has a surface oxide layer morphology after 2000 thermal fatigue cycles (20-650°C). Figure 1 As shown in the figure, the oxidized area on the surface is distributed in a dark brown crown area. Compared with the control example, the area of ​​the oxidized crown area is significantly reduced after the same number of thermal fatigue times. The side oxidation corrosion after 2000 thermal fatigue times (20-650℃) is shown in the figure. Figure 2 As shown in the figure, there is deep oxidation corrosion on the side, with a thickness of 31.3μm. Compared with the control example, the degree of oxidation corrosion inside the matrix is ​​reduced by 16.7%. After 2000 thermal fatigue cycles (20-650℃), the thermal fatigue crack propagation of 0.01wt.% micro-nano TiN+VN+ZrN particle reinforced die steel is shown in the figure. Figure 3 As shown. Obvious thermal fatigue cracks were produced on its surface, but the degree of cracking was significantly weaker than that of the comparative example. Its main thermal fatigue crack was 1.88 mm, and the length of the main thermal fatigue crack was shortened by 13.4% compared with that in the comparative example. Its thermal fatigue resistance was significantly stronger than that of the mold steel in the comparative example that was not reinforced by nanoparticles.

[0048] Example 2

[0049] This embodiment provides a method for improving the thermal fatigue resistance of mold steel by using trace amounts of nanoparticles, comprising the following steps:

[0050] Step 1: uniformly mix the first mixed nanoparticles prepared in Preparation Example 1 with Fe-Cr powder in a mixer at a mixer speed of 60 r / min for 10 h to obtain a second mixed powder, and use iron foil to cover the second mixed powder to prepare a mixed particle wire;

[0051] Step 2: In a vacuum induction melting furnace, the mold steel is melted into molten steel, and then arc and argon blowing are performed in a LF furnace refining furnace for 60 minutes. At the 10th minute of refining, the mixed particle wire is added to the molten steel, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining for 60 minutes, and then cast into an electrode billet steel ingot; the total mass percentage of the three ceramics of micro-nano titanium nitride, vanadium nitride and zirconium nitride added to the steel liquid is 0.05wt.%;

[0052] Step 3: Electroslag remelting is performed on the electrode billet steel ingot to remove inclusions in the steel, followed by multi-directional forging and vacuum heat treatment to finally obtain die steel reinforced with micro-nano particles. The arc power of the electroslag remelting furnace is set within 180kW and the current density is 9A / mm 2 The smelting time is 90 minutes, argon is selected as the inert gas shielding gas, the high-temperature diffusion temperature of the electroslag ingot is 1290℃, and the high-temperature diffusion time is 25 hours. After being taken out of the furnace, the temperature of the electroslag ingot is reduced by 1200℃, and then forged with a forging ratio of 15. After forging, it is cooled by water mist. The heating method of vacuum heat treatment is staged heating, which is respectively increased to 550℃ and 850℃ and kept warm for 15min. Then the austenitizing temperature is 1080℃, and the holding time is 3h. The quenching method is oil quenching, the tempering temperature is 630℃, and the tempering time is 8h.

[0053] The 0.05wt.% micro-nano TiN+VN+ZrN particle reinforced die steel prepared in this embodiment has been subjected to 2000 thermal fatigue tests (20-650°C). The surface oxide layer of the steel is as follows: Figure 4 Compared with the control example, the crown area around the prefabricated notch is evenly distributed and reduced. In addition, after the same number of thermal fatigue times, the side oxidation erosion is as shown in Figure 5 As shown in the figure, it shows obvious oxidation corrosion phenomenon, and the thickness of the oxidation corrosion zone is 22.7μm. Compared with the comparative example, it is reduced by 39.6%. After 2000 thermal fatigue (20-650℃), the thermal fatigue crack propagation of 0.05wt.% micro-nano TiN+VN+ZrN particle reinforced die steel is shown in the figure. Figure 6 As shown. Obvious thermal fatigue cracks appeared on the surface, but the degree of cracking was significantly reduced compared with the control group. The main thermal fatigue crack length was 1.64 mm, which was shortened by 24.4%. This shows that the thermal fatigue resistance of this nanoparticle-reinforced mold steel is significantly stronger than that of the unreinforced control group mold steel.

[0054] Example 3

[0055] This embodiment provides a method for improving the thermal fatigue resistance of mold steel by using trace amounts of nanoparticles, comprising the following steps:

[0056] Step 1: uniformly mix the first mixed nanoparticles prepared in Preparation Example 1 with Fe-Cr powder in a mixer at a mixer speed of 30 r / min for 7 h to obtain a second mixed powder, and use iron foil to cover the second mixed powder to prepare a mixed particle wire;

[0057] Step 2: In a vacuum induction melting furnace, the mold steel is melted into molten steel, and then arc and argon blowing are performed in a LF furnace refining furnace for 45 minutes. At the 10th minute of refining, the mixed particle wire is added to the molten steel, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining for 50 minutes, and then cast into an electrode billet steel ingot; the total mass percentage of the three ceramics of micro-nano titanium nitride, vanadium nitride and zirconium nitride added to the steel liquid is 0.03wt.%;

[0058] Step 3: Electroslag remelting is performed on the electrode billet steel ingot to remove inclusions in the steel, followed by multi-directional forging and vacuum heat treatment to finally obtain die steel reinforced with micro-nano particles. The arc power of the electroslag remelting furnace is set within 160kW and the current density is 7.5A / mm 2 The smelting time is 60 minutes, argon is selected as the inert gas shielding gas, the high-temperature diffusion temperature of the electroslag ingot is 1280℃, and the high-temperature diffusion time is 20 hours. After being taken out of the furnace, the temperature of the electroslag ingot is reduced by 1200℃, and then forged. The forging ratio is 12. After forging, it is cooled by water mist. The heating method of vacuum heat treatment is staged heating, which is respectively increased to 550℃ and 850℃ and kept warm for 15min. Then the austenitizing temperature is 1055℃, and the holding time is 2.5h. The quenching method is oil quenching, the tempering temperature is 600℃, and the tempering time is 6h.

[0059] The 0.03wt.% micro-nano TiN+VN+ZrN particle reinforced die steel prepared in this embodiment has a surface oxide layer morphology after 2000 thermal fatigue tests (20-650°C). Figure 7 Compared with the control group, the area of ​​the oxidized crown area is significantly reduced after the same number of thermal fatigue tests. In addition, after 2000 thermal fatigue tests (20-650℃), the oxidation corrosion on the side is as shown in Figure 8 As shown in the figure, the oxidation corrosion into the matrix is ​​significantly weakened, and the corrosion depth is 11.4μm, which is reduced by 69.6%. In addition, after 2000 thermal fatigue tests (20-650℃), the thermal fatigue crack propagation of 0.03wt.% micro-nano TiN+VN+ZrN particle reinforced die steel is as follows: Fig. 9 As shown in the figure, only one obvious thermal fatigue crack appeared on the surface, and the degree of cracking was significantly reduced compared with the control group. The length of the main thermal fatigue crack was 1.51 mm, which was shortened by 30.4%. This further shows that the thermal fatigue resistance of this mold steel reinforced with micro-nanoparticles is significantly better than that of the unreinforced control group mold steel.

[0060] Comparative Example 1

[0061] Compared with Example 3, the difference is that the first mixed nanoparticles prepared in Preparation Example 1 are not added in step 1. The specific steps are as follows:

[0062] Step 1: In a vacuum induction melting furnace, the mold steel is melted into molten steel. Subsequently, arc and argon blowing refining is carried out in the LF furnace refining furnace for 45 minutes. Then, it enters the VD vacuum decarburization furnace for degassing refining for 50 minutes.

[0063] Step 2: Electroslag remelting of the electrode billet steel ingot to remove inclusions in the steel. Then multi-directional forging and vacuum heat treatment are performed to finally obtain die steel reinforced with micro-nano particles. The arc power of the electroslag remelting furnace is set within 160kW and the current density is 7.5A / mm 2 , the smelting time is 60 minutes, and argon is used as an inert gas shielding gas. The high-temperature diffusion temperature of the electroslag ingot is 1280°C, and the high-temperature diffusion time is 20 hours. After leaving the furnace, the temperature of the electroslag ingot drops to 1200°C, and then forging is carried out. The forging ratio is 12, and water mist cooling is used after forging. The heating method of vacuum heat treatment is staged heating, which is respectively increased to 550°C and 850°C for 15 minutes, and then the austenitizing temperature is 1055°C, the holding time is 2.5 hours, and the quenching is oil quenching. Finally, tempering treatment is carried out, the tempering temperature is 600°C, and the tempering time is 6 hours.

[0064] The mold steel prepared in this comparative example has a surface oxide layer morphology after 2000 thermal fatigue cycles (20-650°C). Fig.10 As shown in the figure, there is an obvious oxidation crown area around the prefabricated notch, which is caused by the combined effect of oxygen exposure and internal thermal stress of the sample. The side oxidation corrosion after 2000 thermal fatigue (20-650℃) is shown in the figure. Fig.11 As shown in the figure, it can be observed that the thermal fatigue cracks extend from the surface to the inside of the matrix, and the erosion depth is 37.6μm. After 2000 thermal fatigue cycles (20-650℃), the thermal fatigue crack extension of the mold steel is as follows: Fig.12 As shown in the figure, very serious thermal fatigue cracks occurred on the surface, and the main crack length was 2.17mm.

[0065] The mold steels reinforced with micro-nano particles prepared in Examples 1-3 of the present invention and Comparative Example 1 were tested for thermal fatigue resistance. The results are shown in Table 1.

[0066] Table 1

[0067] Group Thickness of side oxidation corrosion layer (μm) Thermal fatigue main crack length (mm) Example 1 31.3 1.88 Example 2 22.7 1.64 Example 3 11.4 1.51 Comparative Example 1 37.6 2.17

[0068] According to the above experimental results, it can be concluded that adding 0.01-0.05wt.% micro-nano TiN+VN+ZrN particles can significantly improve the thermal fatigue resistance of mold steel. After multiple tests, it was determined that the optimal addition amount of micro-nano particles is 0.03wt.%. As can be seen from the above table, the mold steel reinforced with micro-nano particles prepared in Examples 1-3 of the present invention has good thermal fatigue resistance.

[0069] The present invention proposes a new method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles. Compared with traditional technologies, this method has unique advantages by introducing nano-ceramic particles into steel to regulate the microstructure, enhance high-temperature mechanical properties and improve oxidation resistance. This method effectively enhances the oxidation resistance and high-temperature strength plasticity of mold steel, and further improves the thermal fatigue resistance. The preparation process is simple and does not require additional equipment. It can be coordinated with the existing steel production procedures, and has the advantages of simple process, economical and efficient, and suitable for large-scale industrial production. In addition, this method can also effectively avoid the agglomeration of nanoparticles and reduce the stress concentration problem caused by the introduction of particles. It provides an effective way for the design and development of mold steel with high thermal fatigue resistance for industrial applications.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles, characterized in that: The steps include: Step 1: placing Ti-V-Zr wire in an electric explosion reaction device, vaporizing the wire and reacting with nitrogen gas to generate first mixed nanoparticles; Step 2: Evenly mix the first mixed nanoparticles with Fe powder to obtain a second mixed powder, and use iron foil to cover the second mixed powder to prepare a mixed particle wire; Step 3: In a vacuum induction melting furnace, the mold steel is melted into molten steel, and then arc and argon blowing refining are carried out in a LF furnace refining furnace. During the refining process, the mixed particle wire is added to the molten steel, and then enters the VD vacuum decarburization furnace external refining furnace for degassing and refining, and then cast into electrode billet steel ingots; Step 4: Electroslag remelting the electrode billet steel ingot to remove inclusions in the steel, followed by multi-directional forging and vacuum heat treatment to finally obtain micro-nano particle reinforced die steel.

2. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 1, characterized in that: In the step 1, preparing the first hybrid nanoparticles comprises the following steps: Step 1: using an electric explosion reaction device, placing the Ti-V-Zr wire alloy in a nitrogen atmosphere to react with the nitrogen atmosphere to generate micro-nano particles; Step 2, in the mixed powder, the total mass fraction of the three ceramics of titanium nitride, vanadium nitride and zirconium nitride is 20%-40%, and the remainder is pure iron powder, which is the second mixed particle; Step 3: first perform vacuum electroslag remelting, then perform high-temperature diffusion, and then directly forge after leaving the heat treatment furnace. The starting forging temperature is 1200°C, the final forging temperature is greater than 1100°C, and then spray water cooling treatment is performed to obtain the first mixed nanoparticles.

3. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 2, characterized in that: The Ti-V-Zr wire material comprises: Ti: 0.75-0.85wt.%, V: 0.02-0.15wt.%, Zr: 0.05-0.20wt.%, a diameter of 2.0-4.0mm, and a particle size of the pure iron powder of 5-200 microns.

4. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 2, characterized in that: In the step 2, the first mixed nanoparticles and Fe-Cr powder are uniformly mixed in a mixer, the mixer speed is 10-60 r / min, and the mixing time is 4-10 h.

5. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 4, characterized in that: In the above step three, arc and argon blowing refining are carried out in the LF furnace refining furnace for 30-60 minutes. At the 10th minute of refining, the mixed particle wire is added to the molten steel liquid, and then enters the VD vacuum decarburization furnace external refining furnace for degassing refining for 40-60 minutes, and then cast into electrode billet ingot.

6. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 5, characterized in that: In the above step three, the total mass percentage of the three ceramics of micro-nano titanium nitride, vanadium nitride and zirconium nitride added to the molten steel is 0.01wt.%-0.05wt.%.

7. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 6, characterized in that: In the above step 4, the arc power of the electroslag remelting furnace is set in the range of 120-180kW and the current density is 6-9A / mm 2 The melting time is 40-90 minutes, and argon is selected as the inert gas shielding gas.

8. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 7, characterized in that: In the above step 4, the high temperature diffusion temperature of the electroslag ingot is 1270-1290°C, and the high temperature diffusion time is 15-25 hours. After being taken out of the furnace, the temperature of the electroslag ingot is reduced by 1200°C, and then forging is carried out with a forging ratio of 10-15, and water mist cooling is performed after forging.

9. The method for improving the thermal fatigue resistance of mold steel by using trace nanoparticles according to claim 8, characterized in that: In step 4, the heating method of vacuum heat treatment is staged heating, which is respectively heated to 550°C and 850°C and kept for 15 minutes, followed by an austenitizing temperature of 1030°C-1080°C, a holding time of 2h-3h, and an oil quenching method, a tempering temperature of 550-630°C, and a tempering time of 4-8h.