Welding self-adaptive process method

通过获取工件坡口特征和尺寸参数,匹配焊接工艺并计算焊道位置和宽度,解决了自动化焊接中因工件不平整导致的焊接效果不佳问题,实现了焊接参数的自动调整和焊接质量的提升 .

CN118905389AActive Publication Date: 2024-11-08NANJING YANGOU TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411200289.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

During the automated welding process, the uneven surface of the workpiece, deformation of the bevel plane, fluctuations in the gap distance and differences in angles lead to poor welding effect. It is necessary to adjust the swing speed, width, step length, wire feeding speed and current in real time to control the welding filling amount. Meet the requirements of floor height and molding effect.

Method used

By obtaining the visual scanning point cloud diagram of the workpiece bevel, segmenting and extracting the bevel features and dimension parameters, matching the corresponding process, calculating the bead position and width, and adjusting the welding speed and step length to ensure welding quality.

Benefits of technology

It realizes the ideal state of automatically adjusting welding parameters according to the workpiece bevel characteristics, improving welding quality, adapting to the needs of automated mass production, and ensuring the ideal state of welding filling and forming effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905389A_ABST
    Figure CN118905389A_ABST
Patent Text Reader

Abstract

The invention discloses a welding self-adaptive process method, which can select a matched process according to the groove characteristics of a workpiece to adjust the swing speed, the swing width, the swing welding step length, the wire feeding speed, the current, the voltage and the like so as to control the increase or decrease of the welding filling amount, ensure the layer height and the welding forming effect and achieve an ideal state. And the automatic batch production requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding technology, and in particular to a welding adaptive process method. Background Art

[0002] In the actual automated welding process, there are reasons such as uneven workpiece surface, slight deformation of the groove plane, fluctuation of the gap distance at the groove, slight difference in the groove angle, etc., which affect the welding effect. It is necessary to immediately select a matching process according to the welding position to adjust the swing speed, swing width, swing welding step length, wire feeding speed, current, voltage, etc., to control the increase or decrease of the welding filling amount, ensure the layer height and welding forming effect, achieve the ideal state, and adapt to the requirements of automated mass production. Summary of the invention

[0003] The present invention provides a welding adaptive process method, which can solve the problems pointed out in the background technology.

[0004] A welding adaptive process method comprises the following steps:

[0005] S1. Obtain a visual scanning point cloud image of the groove of the workpiece to be welded, divide it into multiple sub-grooves, and extract groove features and groove size parameters respectively;

[0006] S2. Perform process matching on each section of the groove, select processes that meet the characteristic range, and combine multiple processes into a welding process for the groove of the workpiece;

[0007] S3. Calculate the weld bead position and the weaving welding width in the multi-segment sub-groove section according to the groove size parameters and groove characteristics;

[0008] S4. Calculate the cross-sectional area of ​​the weld and the welding speed according to the groove size parameters, groove characteristics and process parameters;

[0009] S5. The calculated welding speed, welding width and welding step length are used as the welding speed, welding width and welding step length of the welding process of the groove of the workpiece, and the welding work of the groove is performed.

[0010] The groove size parameters at least include: groove type, groove gap, groove angle;

[0011] The groove features at least include: groove reference point, groove depth, groove gap, groove angle, groove growth direction, groove multi-plane line;

[0012] The process parameters include at least: wire feeding speed, wire material, wire diameter, weaving step length and weaving frequency.

[0013] The process selection method in S2 is as follows:

[0014] The groove features are matched with the corresponding groove feature ranges of various processes in the process library. Based on the weights assigned to the features, the sum of the weight values ​​of various processes is calculated, and the process with the highest weight value is selected as the welding process for this section of the groove.

[0015] The calculation process of the weld bead position and the weaving weld width in the segmented section of S3 is as follows:

[0016] Calculate the relative position z within the groove section i :

[0017] z i =lp i *gh

[0018] Among them, lp i is the layer height percentage, gh is the groove depth;

[0019] The translation vector tp based on the groove reference point bp (x0, y0, z0) and the position of the weld relative to the reference point i (0, 0, z i ), calculate the plane coordinate system of the layer where the weld bead is located, and obtain the point position p on the layer where the weld bead is located i (x0,y0,z0+z i );

[0020] Given the groove growth direction vector n and weld point position p i , the vector perpendicular to the groove growth direction is expressed as p ni ;

[0021] Weld pass point p i Draw a straight line L perpendicular to the groove growth direction i (p i , p ni );

[0022] Based on the straight line L i Fitted curve C of the left side of the intersecting groove feature li And the fitting curve C on the right side ri , get two intersection points, calculate the distance between the two intersection points, the two intersection points are p li (x li ,y li , z li ) and p ri (x ri ,y ri , z ri ), the distance between the two points is the width hw of the layer i ;

[0023]

[0024] Based on the size parameters, get the weld width percentage p j , calculate the weld width w i :

[0025] w i =hw i *p j

[0026] Based on the weld width w i And the point p on the layer where the weld is located i (x0,y0,z0+z i ) to obtain the weld bead position p h (x0,y0+w i , z0+z i ).

[0027] Calculate the welding width ARCw based on the width adjustment factor cw i :

[0028] ARC i =w i ±cw.

[0029] The calculation method of weld cross-sectional area in S4 is as follows:

[0030] If the weld has curvature on both sides of the layer in the groove, then based on the weld position obtained by S3, take the layer where the weld is located as the center, and set the normal straight line of the lowest point as L li , let the top point normal straight line be L hi , let the left side curve be C li , let the right side curve be C ri , the lowest point French straight line L li With the left side curve C li and right side curve C ri The intersection points are p1 and p2, and the top point is the French straight line L hi With the left side curve C li and right side curve C ri The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, the width of the upper base can be obtained respectively. and bottom width

[0031] Connect p1, p2, p4 and p3 in sequence to form a quadrilateral with a known height of z. i , calculate the area s of the quadrilateral ic :

[0032]

[0033] Among them, pj is the weld width percentage, the weld width percentage of the first layer at the bottom is 100%;

[0034] Curve C li Expressed as y = f(x); construct straight line L through p1 and p3 ai , straight line L ai Expressed as y=bx+c, calculate curve C li and the straight line L ai The area of ​​the enclosed area s il :

[0035]

[0036] Construct the line L through p2 and p4 bi , and calculate curve C based on the same method ri and the straight line L bi The area of ​​the enclosed area s ir ;

[0037] Calculate the cross-sectional area s of the weld bead i :

[0038] s i =s il +s ic +s ir .

[0039] The calculation method of weld cross-sectional area in S4 is as follows:

[0040] If the weld bead is a straight line on both sides of the layer in the groove, then based on the weld bead position obtained by S3, the layer where the weld bead is located is taken as the center, and the bottom layer point normal straight line is set as L li , let the top point normal straight line be L hi , let the left point be the French straight line L ai , let the right point be the French straight line L bi , the lowest point French straight line L li The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p1 and p2, and the top point is the French straight line L hi The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, the width of the upper base can be obtained respectively. and bottom width

[0041] The height is known as z i , calculate the area s of the region enclosed by the four straight lines i

[0042]

[0043] s i It is the cross-sectional area of ​​the weld in the current section.

[0044] The calculation method of welding speed is as follows:

[0045] The segment spacing is known to be h i , calculate the relative gentle filling volume v i :

[0046] v i =s i *h i

[0047] Calculate the filling volume v per second in this segment based on the wire diameter and wire feeding speed used in the selected process s :

[0048]

[0049] Where D is the wire diameter and V is the wire feeding speed;

[0050] Based on the filling volume per second v s and the filling volume v i The welding speed d i for:

[0051] d i =v i / v s .

[0052] The welding step length wl of the process selected in S2 i The calculation formula is as follows:

[0053] w i =d i / f

[0054] Among them, d i is the welding speed and f is the welding frequency.

[0055] The welding step length of the process selected in S2 adopts a fixed step length wl.

[0056] Preferably, the method for adjusting the welding wire speed calculated by S4 is as follows:

[0057] Based on the welding speed adjustment factor df, calculate the actual welding speed ARCd i :

[0058] ARCd i =d i ±df.

[0059] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention can select a matching process according to the groove characteristics of the workpiece to adjust the swing speed, swing width, swing welding step length, wire feeding speed, current, voltage, etc., so as to control the welding filling amount to increase or decrease accordingly, ensure the layer height and welding forming effect, achieve an ideal state, and adapt to the requirements of automated mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 It is a schematic diagram of the cross-sectional characteristics and weld bead of the V-shaped groove of the present invention;

[0061] Figure 2 It is a schematic diagram of the U-shaped groove cross-section characteristics and weld bead of the present invention;

[0062] Figure 3 This is a segmented image of the workpiece scan of the present invention. DETAILED DESCRIPTION

[0063] A specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation.

[0064] like Figure 1 and Figure 3 As shown, an embodiment of the present invention provides a welding adaptive process method, comprising the following steps:

[0065] S1. Obtain a visual scanning point cloud image of the groove of the workpiece to be welded, divide it into multiple sub-grooves, and extract groove features and groove size parameters respectively;

[0066] Figure 1 1-15 in the middle are multiple sub-slopes;

[0067] The groove dimension parameters include at least: groove type, groove gap, groove angle;

[0068] The groove features at least include: groove reference point bp (x0, y0, z0), groove depth gh, groove gap, groove angle, groove growth direction vector n, groove multi-plane line;

[0069] The process parameters include at least: wire feeding speed, wire material, wire diameter, weaving step length and weaving frequency;

[0070] For workpieces with complex conditions, small-spacing segments can be used to adapt to different processes and weld out suitable forming effects; for relatively standard workpieces, the segment spacing can be increased to increase efficiency;

[0071] S2. Perform process matching on each section of the groove, select processes that meet the characteristic range, and combine multiple processes into a welding process for the groove of the workpiece;

[0072] That is, the following process matching is performed for each section of the groove: according to the groove characteristics, the features are compared one by one in the bound process library, and the appropriate process is selected; there are multiple processes in the process library, and each process is equipped with a corresponding feature value, and it has a range; if the features extracted from the workpiece meet the feature range of the process, then the process is hit; then according to the weights assigned to the features, the sum of the weight values ​​of the process is calculated, and the process with the highest weight value is selected as the process used for the groove welding (the specific matching conditions and features can be set according to the groove type; the weight value of each matching condition is set according to the process requirements).

[0073] For example, if the groove angle in the process is [43, 47] and the groove angle of the workpiece is 45, it is a hit;

[0074] According to the weight setting, if the hit is 3, the weight is 1 if it is exactly the boundary value (43 / 47, which can be rounded or set to a fluctuation range), and the weight is 0 if it exceeds the range;

[0075] If the groove angle and groove depth are used as the matching conditions, the sum of the weight values ​​of each process is calculated and the process with the highest weight value is selected.

[0076] S3. According to the groove size parameters and groove characteristics, the weld bead position and the swing welding width in the multi-segment groove section are calculated respectively. Different welds need to process the upper and lower bottom widths according to the weld bead width percentage to obtain a more accurate weld bead cross-sectional area;

[0077] The specific calculation process is as follows:

[0078] Calculate the relative position z within the groove section i :

[0079] z i =lp i *gh

[0080] Among them, lp i is the layer height percentage, gh is the groove depth;

[0081] Based on the groove reference point bp (x0, y0, z0) and translation vector tp i (0, 0, z i )(like Figure 1 , in the cross section, the position of each weld bead relative to the reference point can be regarded as a translation vector), calculate the weld bead in the plane coordinate system where the layer is located, and obtain the point position p on the layer i (x0,y0,z0+z i );

[0082] Given the groove growth direction vector n and weld point position pi , the vector perpendicular to the growth direction is expressed as pn i ; Perpendicular to the growth direction; Use this to calculate the layer width and weld bead width;

[0083] Pass this point i Draw a straight line L perpendicular to the groove growth direction i (p i , p ni );

[0084] like Figure 1 As shown, the groove of this embodiment is a V-shaped groove, based on the straight line L i Fitting straight line L of surface A of the intersecting groove feature ai And the fitting straight line L of surface B bi , get two intersection points, calculate the distance between the two intersection points, the two intersection points are p ai (x ai ,y ai , z ai ) and p bi (x bi ,y bi , z bi ), the distance between the two points is the width hw of the layer i ;

[0085]

[0086] Based on the size parameters, get the weld width percentage p j , calculate the weld width w i :

[0087] w i =hw i *p j

[0088] Based on the weld width w i And the point p on the layer where the weld is located i (x0,y0,z0+z i ) to obtain the weld bead position p h (x0,y0+w i , z0+z i ).

[0089] Calculate the welding width ARCw based on the width adjustment factor cw i :

[0090] ARC i =w i ±cw.

[0091] S4. Calculate the cross-sectional area of ​​the weld and the welding speed according to the groove size parameters, groove characteristics and the selected process parameters;

[0092] The specific calculation method is as follows:

[0093] Knowing the layer where the weld is located and the arrangement order in the layer, the weld position p can be obtained i (x0,y0+w i , z0+z i );

[0094] Given the height percentage of each layer, taking the current layer as the center, we can know the percentage of the upper and lower layers lp i-1 , lp i+1 , calculate the upper and lower layer positions, then the upper and lower limits of the layer can be known; and the direction of the layer is perpendicular to the growth direction of the groove, so the normal straight line of the lowest layer point is expressed as L li , the top point French straight line is represented by L hi ,

[0095] Known weld bead position p i , weld width w i , the left point French straight line is represented by L li , the French straight line of the right point is represented by L ri , the above four straight lines form a quadrilateral;

[0096] The lowest point French straight line L li The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p1 and p2, and the top point is the French straight line L hi The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, the width of the upper base can be obtained respectively. and bottom width

[0097] The height is known as z i , calculate the area s of the region enclosed by the four straight lines i :

[0098]

[0099] s i That is, the cross-sectional area of ​​the weld in the current section;

[0100] Here is the cross-sectional area of ​​the weld bead of the first layer groove 1 at the bottom. The weld bead width percentage is 100%. The weld bead width percentages of the other sub-grooves are not 100%. The upper and lower bottom widths need to be processed according to the weld bead width calculation method, that is, and

[0101] The segment spacing is known to be h i , calculate the relative gentle filling volume v i :

[0102] v i =s i *h i

[0103] Calculate the filling volume v per second in this segment based on the wire diameter and wire feeding speed used in the selected process s :

[0104] v s =π(D / 2) 2 *V

[0105] Where D is the wire diameter and V is the wire feeding speed; (the calculation here is a theoretical value. The actual wire feeding speed is related to the robot posture and welding equipment, and there will be some loss. The welding speed adjustment coefficient df below can be adjusted to be closer to the actual production environment);

[0106] Based on the filling volume per second v s and the filling volume v i The welding speed d i for:

[0107] d i =v i / v s

[0108] S5, using the calculated welding speed, welding width, and welding step length as the welding speed, welding width, and welding step length of the welding process of the groove of the workpiece, and performing the welding work of the groove;

[0109] The welding wire speed of each sub-groove is not the same, and each is used as the welding speed of the process matched therewith. According to the sequence of the sub-groove, multiple processes are combined to obtain a complete welding process of the workpiece groove;

[0110] In addition, the welding speed adjustment parameter df is added to adapt to the spattering, flowing, etc. of the molten pool in different processes during welding. The actual welding speed after adjustment is ARCd i :

[0111] ARCd i =d i ±df.

[0112] In addition, the welding step length of the process selected in S2 can adopt a fixed step length wl or use a fixed welding frequency to calculate the welding step length of each section, that is, set the step length wl i The calculation formula is as follows:

[0113] w i =d i / f

[0114] Among them, d i is the welding speed and f is the welding frequency.

[0115] Embodiment 2

[0116] like Figure 2 As shown, the U-shaped groove is different from the V-shaped groove. The weld has an arc on both sides of the layer in the groove. Using the same calculation method will result in a large error. This embodiment proposes a welding adaptive process method applicable to the U-shaped groove on the basis of the first embodiment. The difference from the first embodiment is steps S3-S5. Only the two steps are described in detail below:

[0117] S3. Calculate the weld bead position and the weaving welding width in the multi-segment sub-groove section according to the groove size parameters and groove characteristics;

[0118] The specific calculation process is as follows:

[0119] Calculate the relative position z within the groove section i :

[0120] z i =lp i *gh

[0121] Among them, lp i is the layer height percentage, gh is the groove depth;

[0122] Based on the groove reference point bp (x0, y0, z0) and translation vector tp i (0, 0, z i )(like Figure 1 , in the cross section, the position of each weld bead relative to the reference point can be regarded as a translation vector), calculate the weld bead in the plane coordinate system where the layer is located, and obtain the point position p on the layer i (x0,y0,z0+z i );

[0123] Given the groove growth direction vector n and weld point position p i , the vector perpendicular to the growth direction is expressed as pn i ; Perpendicular to the growth direction; Use this to calculate the layer width and weld bead width;

[0124] Pass this point i Draw a straight line L perpendicular to the groove growth direction i (p i , p ni );

[0125] like Figure 2 The groove of this embodiment is a U-shaped groove, which is different from the V-shaped groove. i Fitted curve C of the left side of the intersecting groove feature l i and the fitting curve C on the right side ri , get two intersection points, calculate the distance between the two intersection points, the two intersection points are p li (x li ,y li , z li ) and p ri (x ri ,y ri , z ri ), the distance between the two points is the width hw of the layer i ;

[0126]

[0127] Based on the size parameters, obtain the weld width percentage pj and calculate the weld width w i :

[0128] w i =hw i *p j

[0129] Based on the weld width w i And the point p on the layer where the weld is located i (x0,y0,z0+z i ) to obtain the weld bead position p h (x0,y0+w i , z0+z i ).

[0130] Calculate the welding width ARCw based on the width adjustment factor cw i :

[0131] ARC i =w i ±cw.

[0132] S4. Calculate the cross-sectional area of ​​the weld and the welding speed according to the groove size parameters, groove characteristics and the selected process parameters;

[0133] The specific calculation method is as follows:

[0134] Knowing the layer where the weld is located and the arrangement order in the layer, the weld position p can be obtained i (x0,y0+w i , z0+z i );

[0135] Given the height percentage of each layer, taking the current layer as the center, we can know the percentage of the upper and lower layers lp i-1 , lp i+1 , calculate the upper and lower layer positions, then the upper and lower limits of the layer can be known; and the direction of the layer is perpendicular to the growth direction of the groove, so the normal straight line of the lowest layer point is expressed as L li , the top point French straight line is represented by L hi ,

[0136] Known weld bead position p i , weld width w i , the left side curve is C li , the right side curve is C ri The above four straight lines form a quadrilateral;

[0137] The lowest point French straight line L li The left side curve is C li and the right side curve is C ri The intersection points are p1 and p2, and the top point is the French straight line L hi The left side curve is C li and the right side curve is C ri The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, the width of the upper base can be obtained respectively. and bottom width

[0138] Note: The layer where the weld bead is located in the groove has arcs on both sides, so the above method is applicable; if the side of the layer is close to a straight line, the calculation method of the V-groove can be used, directly using the plane fitting straight line to intersect with the upper / lower layer line, which is simpler;

[0139] The area enclosed by the two straight lines and the two curves can be divided into three regions, namely:

[0140] The area s of the quadrilateral formed by connecting p1, p2, p4 and p3 in sequence ic ;

[0141] Curve C li and the straight line L ai The area of ​​the enclosed area s il ;as well as

[0142] Curve C ri and the straight line L bi The area of ​​the enclosed area s ir ;

[0143] The height is known as z i , calculate the area s ic :

[0144]

[0145] Here is the cross-sectional area of ​​the weld bead of the first layer groove 1 at the bottom. The weld bead width percentage is 100%. The weld bead width percentages of the other sub-grooves are not 100%. The upper and lower bottom widths need to be processed according to the weld bead width calculation method, that is, and

[0146] Then the cross-sectional area of ​​the remaining grooves can be expressed as:

[0147]

[0148] Curve C li It is expressed as y=f(x);

[0149] Construct the straight line L through p1 and p3 ai , straight line L ai It is expressed as y=bx+c, the intersection points are p1 and p3, and the curve C is calculated. li and the straight line L ai The area of ​​the enclosed area s il :

[0150]

[0151] Construct the line L through p2 and p4 bi , based on the same method to calculate curve C ri and the straight line L bi The area of ​​the enclosed area s ir ;

[0152] Finally, the cross-sectional area s of the weld is calculated i :

[0153] s i =s il +s ic +s ir

[0154] The segment spacing is known to be h i , calculate the relative gentle filling volume v i :

[0155] v i =s i *h i

[0156] Calculate the filling volume v per second in this segment based on the wire diameter and wire feeding speed used in the selected process s :

[0157] v s =π(D / 2) 2 *V

[0158] Where D is the wire diameter and V is the wire feeding speed; (the calculation here is a theoretical value. The actual wire feeding speed is related to the robot posture and welding equipment, and there will be some loss. The welding speed adjustment coefficient df below can be adjusted to be closer to the actual production environment);

[0159] Based on the filling volume per second v s and the filling volume v i The welding speed d i for:

[0160] d i =v i / v s

[0161] S5, using the calculated welding speed, welding width, and welding step length as the welding speed, welding width, and welding step length of the welding process of the groove of the workpiece, and performing the welding work of the groove;

[0162] The welding wire speed of each sub-groove is not the same, and each is used as the welding speed of the process matched therewith. According to the sequence of the sub-groove, multiple processes are combined to obtain a complete welding process of the workpiece groove;

[0163] In addition, the welding speed adjustment parameter df is added to adapt to the spattering, flowing, etc. of the molten pool in different processes during welding. The actual welding speed after adjustment is ARCd i :

[0164] ARCd i =d i ±df.

[0165] In addition, the welding step length of the process selected in S2 can adopt a fixed step length wl or use a fixed welding frequency to calculate the welding step length of each section, that is, set the step length wl i The calculation formula is as follows:

[0166] w i =d i / f

[0167] Among them, d i is the welding speed and f is the welding frequency.

[0168] In addition, although the above two embodiments take V-shaped groove and U-shaped groove as examples respectively, it does not mean that the welding adaptive process method of the present application can only be used for welding work on these two types of grooves. The technical solution of this embodiment can also be used for welding work on other types of grooves.

[0169] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A welding adaptive process method, characterized in that: The steps include: S1. Obtain a visual scanning point cloud image of the groove of the workpiece to be welded, divide it into multiple sub-grooves, and extract groove features and groove size parameters respectively; S2. Perform process matching on each section of the groove, select processes that meet the characteristic range, and combine multiple processes into a welding process for the groove of the workpiece; S3. Calculate the weld bead position and the weaving welding width in the multi-segment sub-groove section according to the groove size parameters and groove characteristics; S4. Calculate the cross-sectional area of ​​the weld and the welding speed according to the groove size parameters, groove characteristics and process parameters; S5. The calculated welding speed, welding width and welding step length are used as the welding speed, welding width and welding step length of the welding process of the groove of the workpiece, and the welding work of the groove is performed.

2. The welding adaptive process method according to claim 1, characterized in that: The groove size parameters at least include: groove type, groove gap, groove angle; The groove features at least include: groove reference point, groove depth, groove gap, groove angle, groove growth direction, groove multi-plane line; The process parameters include at least: wire feeding speed, wire material, wire diameter, weaving step length and weaving frequency.

3. The welding adaptive process method according to claim 1, characterized in that: The process selection method in S2 is as follows: The groove features are matched with the corresponding groove feature ranges of various processes in the process library. Based on the weights assigned to the features, the sum of the weight values ​​of various processes is calculated, and the process with the highest weight value is selected as the welding process for this section of the groove.

4. The welding adaptive process method according to claim 1, characterized in that: The calculation process of the weld bead position and the weaving welding width in the segmented section in S3 is as follows: Calculate the relative position z within the groove section i : z i =p i *gh Among them, lp i is the layer height percentage, gh is the groove depth; The translation vector tp based on the groove reference point bp (0, y0, z0) and the position of the weld relative to the reference point i (0, 0, z i ), calculate the plane coordinate system of the layer where the weld bead is located, and obtain the point position p on the layer where the weld bead is located i (0,y0,z0+ i ); Given the groove growth direction vector n and weld point position p i , the vector perpendicular to the groove growth direction is expressed as p ni ; Weld pass point p i Draw a straight line L perpendicular to the groove growth direction i ( i , p ni ); Based on the straight line L i Fitted curve C of the left side of the intersecting groove feature li And the fitting curve C on the right side ri , get two intersection points, calculate the distance between the two intersection points, the two intersection points are p li ( li ,y li , z li ) and p ri ( ri ,y ri , z ri ), the distance between the two points is the width of the layer h i ; Based on the size parameters, get the weld width percentage p j , calculate the weld width w i : w i =hw i * j Based on the weld width w i And the point p on the layer where the weld is located i (0,y0,z0+ i ) to obtain the weld bead position p h (0,y0+ i , z0+ i ). Calculate the welding width ARCw based on the width adjustment factor cw i : ARCw i = i ±cw。 5. The welding adaptive process method according to claim 4, characterized in that: The method for calculating the cross-sectional area of ​​the weld in S4 is as follows: If the weld has curvature on both sides of the layer in the groove, then based on the weld position obtained by S3, take the layer where the weld is located as the center, and set the normal straight line of the lowest point as L li , let the top point normal straight line be L hi , let the left side curve be C li , let the right side curve be C ri , the lowest point French straight line L li With the left side curve C li and the right side curve C ri The intersection points are p1 and p2, and the top point is the French straight line L hi With the left side curve C li and the right side curve V ri The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, we can get the upper base width respectively. and bottom width Connect p1, p2, p4 and p3 in sequence to form a quadrilateral with a known height of z. i , calculate the area s of the quadrilateral ic : Among them, p j is the weld width percentage, the weld width percentage of the first layer at the bottom is 100%; Curve C li Expressed as y = f(x); construct straight line L through p1 and p3 ai , straight line L ai Expressed as y=bx+c, calculate curve C li and the straight line L ai The area of ​​the enclosed area s il : Construct the line L through p2 and p4 bi , and calculate curve C based on the same method ri and the straight line L bi The area of ​​the enclosed area s ir ; Calculate the cross-sectional area s of the weld bead i : s i = il + ic + ir 。 6. The welding adaptive process method according to claim 4, characterized in that: The method for calculating the cross-sectional area of ​​the weld in S4 is as follows: If the weld bead is a straight line on both sides of the layer in the groove, then based on the weld bead position obtained by S3, the layer where the weld bead is located is taken as the center, and the bottom layer point normal straight line is set as L li , let the top point normal straight line be L hi , let the left point be the French straight line L ai , let the right point be the French straight line L bi , the lowest point French straight line L li The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p1 and p2, and the top point is the French straight line L hi The French straight line L with the left point ai and the French straight line L at the right point bi The intersection points are p3 and p4 respectively. By calculating the distance between p1 and p2 and the distance between p3 and p4, we can get the upper base width respectively. and bottom width The height is known as z i , calculate the area s of the region enclosed by the four straight lines i s i It is the cross-sectional area of ​​the weld in the current section.

7. The welding adaptive process method according to claim 4 or 5, characterized in that: The calculation method of the welding speed is as follows: The segment spacing is known to be h i , calculate the relative gentle filling volume v i : v i = i *h i Calculate the filling volume v per second in this segment based on the wire diameter and wire feeding speed used in the selected process s : Where D is the wire diameter and V is the wire feeding speed; Based on the filling volume per second v s and the filling volume v i The welding speed d i for: d i = i / s 。 8. The welding adaptive process method according to claim 7, characterized in that: The welding step length wl of the process selected in S2 i The calculation formula is as follows: wl i = i / Among them, d i is the welding speed and f is the welding frequency.

9. The welding adaptive process method according to claim 1, characterized in that: The welding step length of the process selected in S2 adopts a fixed step length wl.

10. The welding adaptive process method according to claim 7, characterized in that: The adjustment method of the welding wire speed calculated by S4 is as follows: Based on the welding speed adjustment factor df, calculate the actual welding speed ARCd i : ARCd i = i ±df。

Citation Information

Patent Citations

  • Thick plate large groove multi-layer multi-pass welding track planning method

    CN112276390A

  • Additive manufacturing evaluation method and system based on multi-information fusion quantification

    CN113034014A

  • Welding control method

    CN116689973A

  • Ship structure welding process intelligent design method based on examples and rules

    CN117763705A

  • Tig welding method for stainless steel tube

    JP1999077300A