Polishing method for optical part with convex spherical surface
By setting protective parts on the optical parts and using multiple polishing abrasives to partition the convex spherical surface, the problem that the convex spherical surface in the existing technology cannot be fully covered for polishing, the polishing efficiency and accuracy are improved, and high-precision Convex spherical processing.
Patent Information
- Application Number
- CN202411209470.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The prior art cannot fully cover the small diameter convex spherical surface on the planar substrate, resulting in low processing efficiency and insufficient accuracy.
The optical parts are supported by protective parts, and the local arc surface and annular surface of the convex spherical surface are roughly polished and finely polished by multiple polishing abrasives. The combination of different polishing auxiliary materials and abrasives is used to realize the full surface of the convex spherical surface. Highly efficient polishing.
It improves polishing efficiency and accuracy, ensures that the roughness, surface shape and polishing grade of the convex spherical surface meet high accuracy requirements, and is suitable for spherical surfaces with diameters less than 5mm.
Smart Images

Figure CN118905809A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of optical component processing, and more specifically, to a polishing method for an optical component with a convex spherical surface. Background Art
[0002] For mechanical polishing of optical parts, the traditional polishing process usually uses optical grinding tools (polishing pads) on a polishing machine to perform grinding and polishing. Traditional polishing pads can usually perform full coverage polishing on relatively flat optical parts, but cannot achieve full coverage polishing on small-diameter spherical surfaces on flat glass plates.
[0003] See also Figure 3 For example, in an optical component 10, there is at least one convex spherical surface 12 on a plane substrate 11 (specifically, two convex spherical surfaces 12 need to be polished, and the diameters of the two convex spherical surfaces 12 are different, both less than 5 mm. The thickness of the plane substrate 11 is 0.3 mm (and the two convex spherical surfaces 12 of the optical component 10 are both located in the groove 13, and the bottom surface of the groove 13 is the surface of the plane substrate 11), the surface roughness of the polished convex spherical surface 12 is Rq<80nm, the polishing surface shape requires PV<3.5λ@633nm, the polishing grade is P2, and the annular structure is the coating area 14 that needs to be protected from damage during the polishing process. Due to the insufficient processing range of the equipment and the ability to make mold sizes, optical components of this structure and size cannot be processed.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] The purpose of the present application is to provide a polishing method for an optical component with a convex spherical surface, which solves the problem that the existing polishing process cannot perform full coverage polishing on the small convex spherical surface on the planar substrate.
[0006] To achieve the above purpose, the technical solution adopted in this application is:
[0007] The present application provides a polishing method for an optical component with a convex spherical surface, comprising the steps of:
[0008] providing a protective member, and arranging the protective member on the back side of the optical member;
[0009] Roughly polishing the convex spherical surface on the front surface of the optical component by using a first polishing tool and a second polishing tool respectively, wherein the convex spherical surface includes a local arc-shaped surface located in the middle and a local annular surface located on the outside, the first polishing tool is used for rough polishing the local arc-shaped surface, and the second polishing tool is used for rough polishing the local annular surface;
[0010] The convex spherical surface of the front surface of the optical component after rough polishing is finely polished by a third polishing tool and a fourth polishing tool, wherein the third polishing tool is used for fine polishing a local arc surface, and the fourth polishing tool is used for fine polishing a local annular surface;
[0011] Separate the finished optical component from the protective component.
[0012] In an optional embodiment, the step of providing a protective member and disposing the protective member on the back side of the optical member specifically includes:
[0013] The protective member includes a protective glass with a cavity-avoiding groove, and the protective glass is heated;
[0014] Apply a hot melt adhesive layer on the side of the protective glass provided with the air avoidance groove;
[0015] The side of the protective glass provided with the air avoidance groove is bonded to the back side of the optical component through a hot-melt adhesive layer, wherein the air avoidance groove is used to avoid the coating area on the back side of the optical component.
[0016] In an optional embodiment, the step of roughly polishing the convex spherical surface of the front surface of the optical component by using the first polishing tool and the second polishing tool respectively specifically includes:
[0017] Dropping a first concentration of polishing auxiliary material mixed liquid into the groove on the front side of the optical component, so that the liquid level of the polishing auxiliary material mixed liquid is above the top of the convex spherical surface;
[0018] Roughly polishing a local arc surface of the convex spherical surface by using a first polishing tool, wherein the surface area of the local arc surface accounts for three quarters of the surface area of the convex spherical surface at most;
[0019] The partial annular surface of the convex spherical surface is roughly polished by a second polishing abrasive tool, wherein the diameter of the top end of the second polishing abrasive tool is smaller than the diameter of the top end of the first polishing abrasive tool.
[0020] In an optional embodiment, in the step of roughly polishing the local arc surface of the convex spherical surface by using the first polishing abrasive tool:
[0021] The first polishing tool is tilted and contacts the local arc surface of the convex spherical surface;
[0022] Gradually increase the polishing speed of the first polishing tool to reach the first rough polishing speed;
[0023] During the polishing process using the first rough polishing rotation speed, the inclination angle of the first polishing tool is adjusted within a predetermined range, and the optical component is rotated around the center point of the convex spherical surface at an arbitrary angle from time to time.
[0024] In an optional embodiment, in the step of roughly polishing the local arc surface of the convex spherical surface by using the first polishing abrasive tool:
[0025] Stopping the machine at a first predetermined interval to observe the polishing auxiliary material mixture, and adding the polishing auxiliary material mixture when the liquid level of the polishing auxiliary material mixture is lower than the top of the convex spherical surface;
[0026] The roughly polished partial arc-shaped surface is subjected to lighting inspection at intervals of a second predetermined time to ensure that the roughly polished partial arc-shaped surface reaches the rough polishing quality standard.
[0027] In an optional embodiment, in the step of fine-polishing the convex spherical surface of the front surface of the optical component after rough polishing by the third polishing tool and the fourth polishing tool respectively:
[0028] Dropping a polishing auxiliary material mixed liquid of a second concentration into the groove on the front side of the optical component so that the liquid level of the polishing auxiliary material mixed liquid is above the top of the convex spherical surface, wherein the second concentration is higher than the first concentration;
[0029] Fine polishing is performed on the local arc-shaped surface after rough polishing by a third polishing abrasive tool, wherein the roughness of the third polishing abrasive tool is less than the roughness of the first polishing abrasive tool, and the polishing speed of the third polishing abrasive tool is gradually increased to reach a second fine polishing speed, and the second fine polishing speed is less than the first rough polishing speed;
[0030] The partial annular surface of the convex spherical surface is finely polished by a fourth polishing tool, wherein the top diameter of the fourth polishing tool is smaller than the top diameter of the third polishing tool.
[0031] In an optional embodiment, the step of separating the finely processed optical component from the protective component specifically includes:
[0032] A cleaning tray is provided, and the polished optical component with the protective component is placed in the cleaning tray containing the cleaning liquid;
[0033] The cleaning liquid in the cleaning tray is heated to melt the hot-melt adhesive layer between the polished optical component and the protective component;
[0034] Remove the polished optic from the protector and clean it.
[0035] In an optional embodiment, in the step of heating the cleaning liquid in the cleaning tray to hot-melt the hot-melt adhesive layer between the polished optical component and the protective component:
[0036] A heating pan is provided, in which hot water is contained, wherein the temperature of the hot water is higher than a preset temperature;
[0037] A cleaning tray containing cleaning liquid and the polished optical component with a protective component is placed in a heating tray and left to stand for a predetermined time.
[0038] In an optional embodiment, before the step of applying the hot melt adhesive layer on the heating surface of the protective glass, the step further includes:
[0039] The polished optical parts with protective parts are ultrasonically cleaned in different cleaning tanks in sequence, wherein the different cleaning tanks include: a strong alkali tank, a weak alkali tank, a first water washing tank, and a second water washing tank.
[0040] In an optional embodiment, after the step of separating the finely processed optical component from the protective component, the method further comprises:
[0041] After the separated optical components are left to stand at room temperature for a predetermined period of time, the optical components are finally inspected.
[0042] The polishing method for an optical component with a convex spherical surface provided by the present application has at least the following beneficial effects: by setting a protective member on the back of the optical component, the optical component is supported and the back of the optical component is protected, and the convex spherical surface on the front of the optical component is roughly polished by the first polishing abrasive tool and the second polishing abrasive tool respectively, the first polishing abrasive tool quickly polishes the local arc surface that is easy to process on the surface, and the second polishing abrasive tool quickly polishes the local annular surface that is not easy to process, thereby achieving rough polishing of the entire surface of the convex spherical surface, a large amount of polishing, and improving the polishing efficiency. The convex spherical surface on the front of the optical component after rough polishing is finely polished by the third polishing abrasive tool and the fourth polishing abrasive tool respectively, the third polishing abrasive tool finely polishes the local arc surface that is easy to process on the surface, and the fourth polishing abrasive tool finely polishes the local annular surface that is not easy to process, thereby achieving fine polishing of the entire surface of the convex spherical surface, a small amount of polishing, and ensuring that the entire surface of the convex spherical surface meets the high-precision requirements of roughness, surface shape, and polishing grade. After the finely processed optical component is separated from the protective member, the processed optical component is obtained. When the processing scheme is used to polish a spherical surface with a diameter less than 5 mm on a flat substrate, the local annular surface that is difficult to process can be polished by the second polishing abrasive and the fourth polishing abrasive, and the roughness, surface shape and polishing grade of the optical component can be stably controlled during the polishing process, so that this type of optical component product can meet the technical index requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0044] Figure 1 A flowchart of the main steps of a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application;
[0045] Figure 2A flowchart of detailed steps of a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application;
[0046] Figure 3 A partial cross-sectional view of a protective member used in a polishing method for an optical member with a convex spherical surface provided in an embodiment of the present application after being fixed to the optical member;
[0047] Figure 4 A schematic structural diagram of a polishing abrasive tool used in a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application;
[0048] Figure 5 A schematic diagram of a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application when polishing a local curved surface;
[0049] Figure 6 A schematic diagram of a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application when polishing a partial annular surface;
[0050] Figure 7 The anti-touch angle α in a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application is x Schematic diagram of Figure 7 (1) is the anti-touch angle α at different positions when a convex spherical surface is polished x Schematic diagram of Figure 7 (2) is the anti-touch angle α at different positions when another convex spherical surface is polished x Schematic diagram of
[0051] Figure 8 A schematic structural diagram of a polishing method for an optical component with a convex spherical surface provided in an embodiment of the present application when the optical component is separated.
[0052] Among them, the reference numerals in the figure are:
[0053] 10. Optical part; 11. Planar substrate; 12. Convex spherical surface; 13. Groove; 14. Coating area; 20. Protective part; 21. Protective glass; 22. Air avoidance groove; 23. Hot-melt adhesive layer; 30. First polishing tool; 31. Cylindrical polishing end; 32. Connecting rod; 40. Second polishing tool; 41. Conical polishing end; 50. Third polishing tool; 60. Fourth polishing tool; 70. Heating plate; 71. Cleaning plate. DETAILED DESCRIPTION
[0054] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0055] It should be noted that when a component is referred to as being "fixed on" or "disposed on" another component, it may be directly or indirectly located on the other component. When a component is referred to as being "connected to" another component, it may be directly or indirectly connected to the other component. The directions or positions indicated by the terms "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the directions or positions shown in the accompanying drawings and are only for the convenience of description and cannot be understood as limitations on the present technical solution. The terms "first" and "second" are only used for the convenience of description and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0056] The explanations of some professional terms involved in this embodiment are as follows:
[0057] Surface roughness: refers to the unevenness of the machined surface with small spacing and tiny peaks and valleys. The distance (wave distance) between two peaks or two valleys is very small (less than 1mm), which belongs to the microscopic geometric shape error. The smaller the surface roughness, the smoother the surface.
[0058] Surface shape: PV (Peak to valley), also known as peak to valley value, is a common indicator of optical surface shape quality. It refers to the height difference between the highest point and the lowest point within the sampling range (based on 2D contour lines or 3D data maps) after removing the reference surface.
[0059] Polishing grade: corresponds to the number N of tiny defects allowed within the 10mm sampling range.
[0060] Micro defects: small and irregular defects (generally less than 1μm in size) on the mirror surface.
[0061] This embodiment provides a polishing method for an optical component with a convex spherical surface, which is specifically as follows:
[0062] See also Figure 3This embodiment proposes a polishing method for an optical component with a convex spherical surface, which is used to polish at least one convex spherical surface 12 on a flat substrate 11. For example, a groove 13 is provided on the front of an optical component 10, and two convex spherical surfaces 12 are arranged on the bottom surface of the groove 13, and the diameters of the two convex spherical surfaces 12 are both less than 5mm, and a coating area 14 is arranged on the back of the optical component 10. It is required that the surfaces of the two convex spherical surfaces 12 need to be polished, the polishing surface roughness is Rq<80nm, the polishing surface shape requires PV<3.5λ@633nm, and the polishing grade is P2; the coating area 14 on the back has been coated and cannot be damaged during the polishing process.
[0063] See also Figure 1 In order to achieve the polishing requirements of the above optical component, a polishing method for an optical component with a convex spherical surface in this embodiment mainly includes the following steps:
[0064] Step S100: provide a protective member, and place the protective member on the back of the optical member.
[0065] For specific process, please refer to Figure 3 The protective member 20 is fixed to the back of the optical member 10 to support the thinner part of the optical member 10 to prevent damage to the optical member 10 due to excessive polishing pressure during polishing. In addition, an air avoidance groove 22 is provided on the surface of the protective member 20 connected to one side of the optical member 10 to prevent scratches on the coating area 14 on the back of the optical member 10.
[0066] See also Figure 1 , Figure 2 Therefore, step S100 specifically includes:
[0067] Step S110: The protective member includes a protective glass with a gas avoidance groove, and the protective glass is heated.
[0068] For specific process, please refer to Figure 3 The protective glass 21 has a certain thickness. The protective glass 21 can support the area where the groove 13 of the optical component 10 is located to prevent the bottom wall of the groove 13 from being too thin and deforming under force during the polishing process. An air avoidance groove 22 is provided on the front of the protective glass 21, and its shape corresponds to the shape of the coating area (or other areas that need to be protected or avoided) on the back of the optical component 10. Therefore, when the coating area is annular, the air avoidance groove 22 can be annular. When the protective glass 21 is connected to the back of the optical component 10, the coating area is located in the notch of the air avoidance groove 22, so that the coating area will not be damaged.
[0069] After wiping the prepared protective glass 21 clean with acetone or alcohol, place the protective glass 21 with the air-avoiding groove 22 facing upward on an electric stove and heat it to a predetermined temperature. The predetermined temperature can melt the hot-melt adhesive layer used to bond the protective glass 21 and the optical component 10. For example, the predetermined temperature can be 90°C.
[0070] Step S120, applying a hot melt adhesive layer on the side of the protective glass provided with the air avoidance groove.
[0071] In a specific process, the hot-melt adhesive layer 23 can be made of white wax, which is evenly applied on one side of the heated protective glass 21 having the air-avoiding groove 22 structure.
[0072] Step S130, bonding the side of the protective glass provided with the air avoidance groove to the back side of the optical component through a hot-melt adhesive layer, wherein the air avoidance groove is used to avoid the coating area on the back side of the optical component.
[0073] In the specific process, after the hot-melt adhesive layer 23 (white wax) melts and softens, the back of the optical component 10 is adhered to the white wax layer. After the optical component 10 and the protective glass 21 are completely cooled to room temperature, the optical component 10 and the protective glass 21 are fixed and prepared for the next step of polishing.
[0074] See also Figure 1 Step S200: Roughly polish the convex spherical surface on the front side of the optical component by using a first polishing tool and a second polishing tool respectively, wherein the convex spherical surface includes a local arcuate surface located in the middle and a local annular surface located on the outside, the first polishing tool is used for rough polishing the local arcuate surface, and the second polishing tool is used for rough polishing the local annular surface.
[0075] For specific process, please refer to Figure 4 , Figure 5 , Figure 6 , rough machining is performed on different areas of the convex spherical surface 12 on the front side of the optical component 10 by means of the first polishing tool 30 and the second polishing tool 40. The polishing surface range of the first polishing tool 30 is relatively large, and it can polish large areas that are easy to polish, such as large surfaces. The polishing surface range of the second polishing tool 40 is relatively small, and it can polish small areas that are not easy to polish, such as small gaps and small corners. Different polishing tools are used according to different areas on the convex spherical surface 12, specifically, the entire surface of the convex spherical surface 12 is divided into: a local arc surface located in the middle of the convex spherical surface 12 and a local annular surface surrounding the outside of the local arc surface. The range of the local arc surface is relatively large, and the polishing tool can be tilted to polish the area. The local annular surface is a surface area close to the outer edge of the convex spherical surface 12, so the space is small, and the polishing tool is not easy to extend into this position for surface polishing.
[0076] The surface area of the local arcuate surface of this embodiment accounts for three quarters of the surface area of the convex spherical surface at most, so the ratio of the surface area of the local arcuate surface to the surface area of the local annular surface is not greater than 3: 1. The first polishing abrasive tool is used to quickly polish the local arcuate surface that is easy to process, and the second polishing abrasive tool is used to quickly polish the local annular surface that is not easy to process, thereby achieving rough polishing of the entire surface of the convex spherical surface, with a large polishing amount and improved polishing efficiency.
[0077] See also Figure 1 , Figure 2 Therefore, step S200 specifically includes:
[0078] Step S210: drip a polishing auxiliary material mixture of a first concentration into the groove on the front surface of the optical component, so that the liquid level of the polishing auxiliary material mixture is above the top of the convex spherical surface.
[0079] In the specific process, a first concentration mixture of cerium oxide with a particle size of 0.7-0.8μ and pure water is used as a polishing auxiliary material mixture. The first concentration can be 0.15g / ml. The polishing auxiliary material mixture is dropped into the groove of the optical part with a rubber-tipped dropper so that the liquid level of the polishing auxiliary material mixture is above the top of the convex spherical surface.
[0080] Step S220: Roughly polishing the local arc surface of the convex spherical surface by using a first polishing tool, wherein the surface area of the local arc surface accounts for three quarters of the surface area of the convex spherical surface at most.
[0081] See also Figure 4 , Figure 5 In the specific process, the first polishing tool 30 can use a wool polishing head, which is relatively rough. The specific structure of the first polishing tool 30 includes: a cylindrical polishing end 31 and a connecting rod 32. The cylindrical polishing end 31 is installed and fixed to the engraving pen through the connecting rod 32. The connecting rod 32 has a certain length to ensure that the distance between the top of the cylindrical polishing end 31 and the top of the engraving pen clamp is greater than the depth H of the groove 13 of the optical part 10, and to ensure that the first polishing tool 30 is installed in place on the engraving pen, that is, to lock the clamp.
[0082] After turning on the power switch, the operator holds the electric engraving pen in his hand so that the first polishing abrasive on the electric engraving pen is in close contact with the local arc surface of the convex spherical surface, polishes the local arc surface area in the middle of the spherical surface, and rubs the cylindrical polishing end with the convex spherical surface of the optical part. During the polishing process, try to make the polishing auxiliary material mixture fully adhere to the convex spherical surface and the cylindrical polishing end.
[0083] During the polishing process, the first polishing tool can be tilted and contact the local arc surface of the convex spherical surface. In the specific process, if the selected first polishing tool is long enough, it can be tilted with the contact point as the center during the polishing process. The acute angle between the central axis of the first polishing tool and the horizontal plane is the tilt angle α. When the first polishing tool is tilted, it is necessary to ensure that the tilt angle α is greater than the anti-touch angle α. x , where the anti-touch angle α x is the angle between the line from the edge point of the convex spherical surface to the opening edge of the groove in the corresponding direction and the horizontal plane, where x represents different positions. x When the first polishing tool is used, it will not collide with the inner wall of the groove during the grinding process, thereby avoiding damage to other surfaces of the optical component and ensuring the quality of the optical component.
[0084] See also Figure 7 Figure (1) shows the anti-contact angle α between a convex spherical surface and the inner wall of a groove that is close to it when polishing a convex spherical surface. 1 , the groove depth is H, the line L1 from the edge point of the convex spherical surface to the opening edge of the groove in the corresponding direction, then Sinα 1 =H / L1; the anti-touch angle α between the convex spherical surface and the inner wall of the groove far away from it 2 , the groove depth is H, the line L2 from the edge point of the convex spherical surface to the opening edge of the groove in the corresponding direction, then Sinα 2 =H / L2.
[0085] See also Figure 7 Figure (2) shows the anti-contact angle α between the convex spherical surface and the inner wall of the groove far away from it when polishing another convex spherical surface. 3 , the depth of the groove is H, the line from the edge point of the convex spherical surface to the opening edge of the groove in the corresponding direction is L3, then Sinα3=H / L3; the anti-touch angle α between the convex spherical surface and the inner wall of the groove that is close to it 4 , the groove depth is H, the line L4 from the edge point of the convex spherical surface to the opening edge of the groove in the corresponding direction, then Sinα 4 =H / L4.
[0086] During the polishing process, the polishing speed of the first polishing tool is gradually increased, and finally the first rough polishing speed is reached. In the specific process, the engraving pen speed is first adjusted to within 300rad / min, and the initial polishing is performed to observe whether there are any problems, such as excessive polishing, etc. After confirming that the initial polishing is stable, the speed is adjusted to 600rad / min. This makes the rough polishing process more stable, while improving the polishing efficiency, taking into account quality control, and avoiding mistakes that lead to scrapping of optical parts.
[0087] During the polishing process using the first rough polishing speed, the inclination angle of the first polishing tool is adjusted within a predetermined range, and the adjustment range of the inclination angle is consistent with the anti-touch angle α. x Related, that is, in (90° to α x ). The angle is adjusted within the range, and the contact point of the first polishing tool within the range of the local arc surface is changed, and the optical part is rotated around the center point of the convex spherical surface at any angle from time to time. Thereby, full-surface polishing of the local arc surface is achieved, and the polishing amount is uniform and the polishing speed is fast. In the specific process, during the polishing process, the optical part needs to be rotated around the center point at any angle from time to time (at least once within 2 minutes), and the polishing head makes irregular movements relative to the spherical surface. By rotating at irregular angles from time to time and the irregular movement of the polishing head, the polishing trajectory is close to disorder. The disordered polishing process can make the surface polishing more uniform.
[0088] During the rough polishing process, the machine is stopped at a predetermined interval to observe the polishing auxiliary material mixture. When the liquid level of the polishing auxiliary material mixture is lower than the top of the convex spherical surface, the polishing auxiliary material mixture is added. In the specific process, the polishing auxiliary material mixture is stopped every 5 minutes to observe whether it is too little. If it is too little, it is necessary to add polishing auxiliary material mixture. In this way, the quality requirements of the polished surface are guaranteed.
[0089] During the rough polishing process, the rough-polished local curved surface is light-tested at intervals of the second predetermined time to ensure that the rough-polished local curved surface meets the rough polishing quality standard. In the specific process, the optical parts need to be cleaned and blown clean with compressed air every 10 minutes, and visually inspected under a special inspection light to prevent excessive local removal. And check whether the area where the local curved surface is located is polished and bright (without sand holes) to reach the polishing level of P2. If the local curved surface is not polished and bright, adjust the position of the first polishing abrasive tool to focus on polishing this position until it meets the requirements.
[0090] If there are multiple convex spherical surfaces on the planar substrate, the local arc-shaped surface of each convex spherical surface can be roughly polished in sequence in the above manner.
[0091] Step S230: Roughly polishing the partial annular surface of the convex spherical surface by using a second polishing tool, wherein the diameter of the top end of the second polishing tool is smaller than the diameter of the top end of the first polishing tool.
[0092] For specific process, please refer to Figure 4 , Figure 6, replace the polishing tool on the engraving pen with a second polishing tool 40. The second polishing tool 40 can use a cotton swab polishing head. The roughness of the cotton swab polishing head is smaller than that of the wool polishing head (first polishing tool 30). The specific structure of the second polishing tool 40 includes: a conical polishing end 41 and a connecting rod 32. The conical polishing end 41 is installed and fixed to the engraving pen through the connecting rod 32. The top of the conical polishing end 41 is a pointed cone structure. During the polishing process of the conical polishing end 41, the tip of the conical polishing end 41 can be abutted against the outer edge of the convex spherical surface 12 for grinding and polishing, so that the local annular surface of the convex sphere can be polished. The second polishing tool 40 can also use a streamlined conical end, which gradually becomes smaller in the direction toward the top and has a pointed cone structure at the top. The installation method, operation steps, precautions and polishing process of polishing the local annular surface area of the convex spherical surface with a cotton swab polishing head are the same as the rough polishing process of the first polishing abrasive tool. Refer to the rough polishing process of the above-mentioned first polishing abrasive tool to complete the rough polishing of the local annular surface through the second polishing abrasive tool.
[0093] If there are multiple convex spherical surfaces on the flat substrate, the partial annular surfaces of each convex spherical surface can be coarsely polished in sequence in the above manner. The polishing auxiliary material mixture on the surface of the optical component is rinsed clean with clean water, and the next step of fine polishing is prepared.
[0094] See also Figure 1 Step S300: fine-polish the convex spherical surface of the front surface of the optical component after rough polishing by using a third polishing tool and a fourth polishing tool, wherein the third polishing tool is used for fine-polishing a local arc surface, and the fourth polishing tool is used for fine-polishing a local annular surface.
[0095] For specific process, please refer to Figure 4 , Figure 5 , Figure 6 The convex spherical surface 12 on the front side of the roughly polished optical component 10 is finely polished by the third polishing tool 50 and the fourth polishing tool 60 respectively. The third polishing tool 50 finely polishes the local arc surface that is easy to process, and the fourth polishing tool 60 finely polishes the local annular surface that is not easy to process, thereby achieving fine polishing of the entire surface of the convex spherical surface 12 with a small amount of polishing, ensuring that the entire surface of the convex spherical surface 12 meets the high-precision requirements of roughness, surface shape, and polishing grade.
[0096] See also Figure 1 , Figure 2 Therefore, step S300 specifically includes:
[0097] Step S310, dripping a polishing auxiliary material mixture of a second concentration into the groove on the front side of the optical component so that the liquid level of the polishing auxiliary material mixture is above the top of the convex spherical surface, wherein the second concentration is higher than the first concentration.
[0098] In the specific process, a second concentration of a mixed solution prepared by mixing cerium oxide with a particle size of 0.7-0.8 μm and pure water is used as a polishing auxiliary material mixed solution, and the second concentration can be 0.34 g / ml, so that the concentration of the second concentration polishing auxiliary material mixed solution is higher than the first concentration polishing auxiliary material mixed solution in the rough polishing process. The higher the concentration of the polishing auxiliary material mixed solution, the higher the fine polishing efficiency, and the shorter the fine polishing process time, the polishing quality requirements can be achieved. The second concentration of the polishing auxiliary material mixed solution is dropped into the groove of the optical part with a rubber-tipped dropper so that the polishing auxiliary material mixed solution covers the top of the convex spherical surface.
[0099] Step S320, fine polishing the local arc-shaped surface after rough polishing is performed by a third polishing abrasive, wherein the roughness of the third polishing abrasive is less than that of the first polishing abrasive, and the polishing speed of the third polishing abrasive is gradually increased to reach a second fine polishing speed, which is less than the first rough polishing speed.
[0100] For specific process, please refer to Figure 4 , Figure 5 The third polishing tool 50 can be a sponge polishing head, the roughness of the sponge polishing head is lower than that of the wool polishing head. The structure of the third polishing tool 50 can be the same or similar to the shape of the first polishing tool 30. Similarly, the third polishing tool 50 is installed on the engraving pen and ensures that the top of the polishing head is greater than the depth H of the groove 13 of the optical part 10 from the top of the engraving pen clamp, and ensures that the polishing head is installed in place on the engraving pen, that is, the clamp is locked. After turning on the power switch, hold the electric engraving pen by hand so that the polishing head of the electric engraving pen is close to the local arc surface of the convex ball, and rub the cylindrical polishing end 31 of the third polishing tool 50 with the local arc surface. During the polishing process, try to make the polishing auxiliary material mixture fully adhere to the local arc surface and the polishing head.
[0101] During the polishing process, gradually increase the polishing speed of the third polishing tool to reach the second fine polishing speed, which is less than the first rough polishing speed. In the specific process, adjust the speed of the engraving pen within 300rad / min, perform initial polishing, and observe whether there are any problems. If there are no problems, adjust the speed to the second fine polishing speed, which can be 450rad / min. By gradually increasing the speed, the second fine polishing speed, which is smaller than the first rough polishing speed, is used for fine polishing. The operator can gradually adapt to the polishing process, making the fine polishing process more stable, and stably controlling the fine polishing quality to avoid mistakes that lead to scrapping of optical parts.
[0102] The third polishing tool can also adjust the inclination angle of the third polishing tool within a predetermined range by referring to the rough polishing process of the first polishing tool. During the polishing process, the optical part needs to be rotated around the center point at any angle at irregular intervals (at least once within 2 minutes), and the polishing head of the third polishing tool makes irregular movements relative to the spherical surface. By irregularly rotating the optical part at an uncertain angle and irregularly moving the polishing head, the polishing track is close to disorder, which can make the surface polishing more uniform.
[0103] During the fine polishing process, stop the machine at a predetermined interval to observe the polishing auxiliary material mixture. When the liquid level of the polishing auxiliary material mixture is lower than the top of the convex spherical surface, add polishing auxiliary material mixture. Stop every 5 minutes (the first predetermined time) to observe whether the polishing auxiliary material mixture is too little. If it is too little, add polishing auxiliary material mixture.
[0104] During the fine polishing process, the fine polished local curved surface is inspected at intervals of the second predetermined time to ensure that the fine polished local curved surface meets the fine polishing quality standard. In order to prevent excessive local processing, the fine polished local curved surface needs to be cleaned and blown clean with compressed air every 10 minutes (the second predetermined time), and the area within the local curved surface of the spherical surface is detected using a white light interferometer to see if the spherical surface reaches Rq < 80nm. If the local curved surface area does not meet the standard, the next polishing needs to focus on polishing. This process needs to be repeated 3 to 4 times, and the actual number depends on the actual situation, so as to complete the fine polishing of the local curved surface area of the spherical surface.
[0105] Step S330: fine-polishing the partial annular surface of the convex spherical surface by using a fourth polishing tool, wherein the top diameter of the fourth polishing tool is smaller than the top diameter of the third polishing tool.
[0106] For specific process, please refer to Figure 4 , Figure 6, replace the polishing tool on the engraving pen with the fourth polishing tool 60. The fourth polishing tool 60 can use a cotton swab polishing head. The roughness of the cotton swab polishing head is smaller than that of the wool polishing head (the first polishing tool 30), and the structure of the fourth polishing tool 60 is the same or similar to that of the second polishing tool 40, so that the top diameter of the fourth polishing tool 60 is smaller than the top diameter of the third polishing tool 50. In the specific structure, the fourth polishing tool 60 also has a conical polishing end 41, and the top of the conical polishing end 41 is a pointed cone structure, or the fourth polishing tool 60 has a streamlined conical end, which gradually becomes smaller in the direction toward the top and has a pointed cone structure at the top. In the process of polishing with the conical polishing end 41, the tip of the conical polishing end 41 can be abutted against the outer edge of the convex spherical surface 12 for grinding and polishing, so that the local annular surface of the convex sphere can be finely polished. The installation method, operation steps, precautions and polishing process of the local annular surface area of the convex spherical surface using a cotton swab polishing head are the same as the fine polishing process of the third polishing abrasive tool. The fourth polishing abrasive tool is used to complete the fine polishing of the local annular surface. The polishing surface roughness of the convex spherical surface after fine polishing reaches Rq<80nm, the surface shape requirement of the polishing surface is PV<3.5λ@633nm, and the polishing grade is the polishing requirement standard of P2.
[0107] If there are multiple convex spherical surfaces on the flat substrate, the partial annular surfaces of each convex spherical surface can be finely polished in sequence in the above manner. The polishing auxiliary material mixture on the surface of the optical component is rinsed clean with clean water to prepare for the next step of processing.
[0108] Step S350: The polished optical component with the protective component is ultrasonically cleaned in different cleaning tanks in sequence.
[0109] In the specific process, after the optical parts with protective parts are placed in the cleaning basket, they are placed in the ultrasonic chemical cleaning tank for cleaning through ultrasonic cleaning equipment. Specifically, they are cleaned in the strong alkali tank for 5 minutes, the weak alkali tank for 10 minutes, the A water washing tank for 10 minutes, and the B water washing tank for 5 minutes. Then, the optical parts with protective parts are taken out of the cleaning basket, wiped clean with a dust-free cloth, and placed on the storage tray, ready for the next step of unloading the tray.
[0110] See also Figure 1 , step S400, separating the finely processed optical component from the protective component.
[0111] In a specific process, the hot-melt adhesive layer between the protective component and the optical component is melted by heating, so that the optical component is separated from the protective component.
[0112] See also Figure 1 , Figure 2 Therefore, the specific process of step S400 includes:
[0113] Step S410: provide a cleaning tray, and place the polished optical component with the protective component into the cleaning tray containing cleaning liquid.
[0114] See also Figure 8 The cleaning tray 71 can be a small aluminum tray, which is light and has good heat conduction performance. First, the optical component 10 with the protective component 20 is placed in the small aluminum tray, and then a mixed cleaning liquid of alcohol and acetone is added to the small aluminum tray in a ratio of 1:1, and the liquid level must be above the optical component 10 with the protective component 20.
[0115] Step S420: heating the cleaning liquid in the cleaning tray to melt the hot-melt adhesive layer between the polished optical component and the protective component.
[0116] See also Figure 8 In this step, a heating plate 70 is provided, which may be a large aluminum plate, and hot water is placed in the heating plate 70, wherein the temperature of the hot water is higher than a preset temperature. A cleaning plate 71 containing cleaning liquid and the optical member 10 with the protective member 20 after polishing is placed in the heating plate 70 and left to stand for a predetermined time.
[0117] In the specific process, hot water is then placed in the large aluminum pan, and the liquid level is about half of the depth of the large aluminum pan, and the temperature should be higher than 70°C. Then the small aluminum pan containing the cleaning liquid and the optical parts with protective parts is placed in the large aluminum pan, and then left to stand for about 5 minutes. The wax layer is heated to melt and soften, so that the protective parts and the optical parts can be separated.
[0118] Step S430: remove the polished optical component from the protective component and clean it.
[0119] During the specific process, use special clips to take out the optical parts and protective parts, wipe them clean with a dust-free cloth, and place them on the storage tray in the same direction, ready for the next step of final inspection.
[0120] Step S500: After the separated optical components are left to stand at room temperature for a predetermined period of time, the optical components are finally inspected.
[0121] During the specific process, the cleaned product needs to be stabilized at room temperature for 1 hour and then sent to final inspection for final inspection of the optical parts.
[0122] In summary, the present application proposes a polishing method for an optical component with a convex spherical surface. By setting a protective member on the back of the optical component, the optical component is supported and protected on the back of the optical component. The convex spherical surface on the front of the optical component is roughly polished by the first polishing tool and the second polishing tool respectively. The first polishing tool quickly polishes the local arc surface that is easy to process on the surface, and the second polishing tool quickly polishes the local annular surface that is not easy to process, thereby achieving rough polishing of the entire surface of the convex spherical surface, with a large amount of polishing and improved polishing efficiency. The convex spherical surface on the front of the optical component after rough polishing is finely polished by the third polishing tool and the fourth polishing tool respectively. The third polishing tool finely polishes the local arc surface that is easy to process on the surface, and the fourth polishing tool finely polishes the local annular surface that is not easy to process, thereby achieving fine polishing of the entire surface of the convex spherical surface, with a small amount of polishing, ensuring that the entire surface of the convex spherical surface meets the high-precision requirements of roughness, surface shape, and polishing grade. After the finely processed optical component is separated from the protective member, the processed optical component is obtained. When the processing scheme is used to polish a spherical surface with a diameter less than 5 mm on a flat substrate, the local annular surface that is difficult to process can be polished by the second polishing abrasive and the fourth polishing abrasive, and the roughness, surface shape and polishing grade of the optical component can be stably controlled during the polishing process, so that this type of optical component product can meet the technical index requirements.
[0123] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A polishing method for an optical component with a convex spherical surface, It is characterized in that The method comprises the steps of: providing a protective member, and arranging the protective member on the back side of the optical member; Roughly polishing the convex spherical surface on the front surface of the optical component by using a first polishing tool and a second polishing tool, respectively, wherein the convex spherical surface includes a local arcuate surface located in the middle and a local annular surface located on the outside, the first polishing tool is used for rough polishing the local arcuate surface, and the second polishing tool is used for rough polishing the local annular surface; The convex spherical surface of the front surface of the optical component after rough polishing is finely polished by a third polishing tool and a fourth polishing tool, respectively, wherein the third polishing tool is used for fine polishing the local arc-shaped surface, and the fourth polishing tool is used for fine polishing the local annular surface; The optical component after finishing is separated from the protective component.
2. The polishing method for an optical component having a convex spherical surface according to claim 1, It is characterized in that In providing a protective member, the step of arranging the protective member on the back side of the optical member specifically includes: The protective member includes a protective glass with a gas avoidance groove, and the protective glass is heated; Applying a hot melt adhesive layer on the side of the protective glass provided with the air avoidance groove; The side of the protective glass provided with the air avoidance groove is bonded to the back side of the optical component through the hot-melt adhesive layer, wherein the air avoidance groove is used to avoid the coating area on the back side of the optical component.
3. The polishing method for an optical component with a convex spherical surface as claimed in claim 1, It is characterized in that The steps of roughly polishing the convex spherical surface of the front side of the optical component by using the first polishing tool and the second polishing tool respectively specifically include: Dropping a first concentration of a polishing auxiliary material mixed liquid into the groove on the front side of the optical component, so that the liquid level of the polishing auxiliary material mixed liquid is above the top of the convex spherical surface; Roughly polishing a local arc surface of the convex spherical surface by a first polishing abrasive tool, wherein the surface area of the local arc surface accounts for at most three quarters of the surface area of the convex spherical surface; The partial annular surface of the convex spherical surface is roughly polished by a second polishing abrasive tool, wherein the diameter of the top end of the second polishing abrasive tool is smaller than the diameter of the top end of the first polishing abrasive tool.
4. The polishing method for an optical component having a convex spherical surface as claimed in claim 3, It is characterized in that In the step of roughly polishing the local arc surface of the convex spherical surface by the first polishing abrasive tool: The first polishing tool is tilted and contacts the local arc surface of the convex spherical surface; gradually increasing the polishing speed of the first polishing tool to reach a first rough polishing speed; During polishing at the first rough polishing speed, the tilt angle of the first polishing tool is adjusted within a predetermined range, and the optical component is rotated around the center point of the convex spherical surface at an arbitrary angle from time to time.
5. The polishing method for an optical component having a convex spherical surface as claimed in claim 4, It is characterized in that In the step of roughly polishing the local arc surface of the convex spherical surface by the first polishing abrasive tool: Stopping the machine at a first predetermined interval to observe the polishing auxiliary material mixture, and adding the polishing auxiliary material mixture when the liquid level of the polishing auxiliary material mixture is lower than the top of the convex spherical surface; The roughly polished partial arc-shaped surface is subjected to lighting inspection at intervals of a second predetermined time to ensure that the roughly polished partial arc-shaped surface reaches the rough polishing quality standard.
6. The polishing method for an optical component having a convex spherical surface according to claim 4, It is characterized in that In the step of fine-polishing the convex spherical surface of the front surface of the optical component after rough polishing by the third polishing tool and the fourth polishing tool respectively: Dropping a polishing auxiliary material mixture of a second concentration into the groove on the front surface of the optical element so that the liquid level of the polishing auxiliary material mixture is above the top of the convex spherical surface, wherein the second concentration is higher than the first concentration; Performing fine polishing on the partially arc-shaped surface after rough polishing by a third polishing abrasive tool, wherein the roughness of the third polishing abrasive tool is less than that of the first polishing abrasive tool, and gradually increasing the polishing speed of the third polishing abrasive tool to reach a second fine polishing speed, wherein the second fine polishing speed is less than the first rough polishing speed; The partial annular surface of the convex spherical surface is finely polished by a fourth polishing tool, wherein the top diameter of the fourth polishing tool is smaller than the top diameter of the third polishing tool.
7. The polishing method for an optical component having a convex spherical surface according to claim 1, It is characterized in that The step of separating the finely processed optical component from the protective component specifically includes: Providing a cleaning tray, placing the polished optical component with the protective component into the cleaning tray containing the cleaning liquid; The cleaning liquid in the cleaning tray is heated to melt the hot-melt adhesive layer between the polished optical component and the protective component; Remove the polished optic from the protector and clean it.
8. The polishing method for an optical component having a convex spherical surface according to claim 7, It is characterized in that In the step of heating the cleaning liquid in the cleaning tray to melt the hot-melt adhesive layer between the polished optical component and the protective component: providing a heating pan, wherein hot water is contained in the heating pan, wherein the temperature of the hot water is higher than a preset temperature; The cleaning plate containing the cleaning liquid and the polished optical component with the protective component is placed in the heating plate and left to stand for a predetermined time.
9. The polishing method for an optical component having a convex spherical surface according to claim 1, It is characterized in that The step of applying the hot melt adhesive layer to the heated surface of the protective glass also includes: The polished optical parts with protective parts are ultrasonically cleaned in different cleaning tanks in sequence, wherein the different cleaning tanks include: a strong alkali tank, a weak alkali tank, a first water washing tank, and a second water washing tank.
10. The polishing method for an optical component having a convex spherical surface according to claim 1, It is characterized in that After the step of separating the finely processed optical component from the protective component, the method further comprises: After the separated optical components are left to stand at room temperature for a predetermined period of time, the optical components are finally inspected.
Citation Information
Patent Citations
Corner grinding device for high-pressure forming parts in automobile
CN111113188A
Double-sided polishing method for optical lens
CN113458909A
Preparation method of polishing grinding head for stone with complex curved surface and polishing method
CN115070629A
Polishing method for optical lens mold core
CN115139191A
Shear thickening and polishing device and method for optical lens
CN116394113A
Cited By
Surface polishing method for aluminum heating plate
CN119260479A